A method for mix design of asphalt mixtures based on improved skid resistance and its application

By using a fine, closely spaced gradation design, the skeleton voids and microtexture of the asphalt mixture are precisely controlled, solving the problem of the decline in skid resistance of steel slag aggregate in asphalt mixtures, and realizing the stability of mixture performance and the resource utilization of steel slag.

CN122598889BActive Publication Date: 2026-11-17ANHUI TRANSPORT CONSULTING & DESIGN INST
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611072213.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-07-20
Publication Date
2026-11-17
Estimated Expiration
2046-07-20

AI Technical Summary

Technical Problem

Existing technologies cannot accurately control the skid resistance of asphalt mixtures, especially when using steel slag aggregates. This leads to a decline in the skid resistance of the mixtures over long-term use, and the changes in the porous structure and activity of steel slag cannot be effectively quantified, resulting in unstable pavement performance.

Method used

By adopting a fine, closely spaced gradation design, and by calculating the multi-level skeleton interlocking anti-skid coefficient, the critical threshold for steel slag fine aggregate filling, fiber content correction, and asphalt-aggregate ratio optimization, the skeleton voids and surface micro-texture of the mixture are precisely controlled. Combined with the effects of steel slag activity and traffic fatigue, the anti-skid performance of the mixture is improved.

Benefits of technology

It effectively inhibited the decline of skid resistance of asphalt pavement, extended the service life of pavement, realized the resource utilization of steel slag, and improved the road performance and construction accuracy of the mixture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_5
    Figure SMS_5
  • Figure SMS_6
    Figure SMS_6
  • Figure SMS_11
    Figure SMS_11
Patent Text Reader

Abstract

This invention belongs to the technical field of asphalt pavement surface materials for road engineering, specifically a method and application for asphalt mixture mix design based on improved skid resistance. This invention employs a fine, closely spaced gradation to optimize the aggregate structure, and combines it with coarse and fine steel slag composite aggregates. Through multi-level void verification, fine aggregate filling control, fiber content fatigue correction, and asphalt-aggregate ratio optimization, it achieves a synergistic improvement in both the macroscopic skeleton skid resistance and the microscopic texture skid resistance of the mixture. While meeting road service indicators, it extends the skid resistance service life of asphalt pavements and simultaneously achieves the efficient resource utilization of industrial solid waste, steel slag.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of asphalt pavement surface materials for road engineering, and particularly relates to a method for designing asphalt mixture mix proportions based on improved skid resistance and its application. Background Technology

[0002] SMA (Stone Mastic Asphalt) mixtures, relying on a coarse aggregate interlocking skeleton structure, possess excellent high-temperature stability and wear resistance, making them the preferred material for the surface layer of high-grade highways and municipal roads. Traditional SMA mixtures typically use a coarse gradation, with an excessive proportion of coarse aggregate and insufficient fine aggregate filling. While the macroscopic voids of the pavement are sufficient, the microscopic texture is lacking. After long-term vehicle load compaction, the aggregate edges wear down rapidly, and the pavement's anti-skid performance deteriorates significantly in a short period. Meanwhile, the extraction cost of natural basalt aggregates is high, and mineral resources are consumed in large quantities. Steel slag solid waste from steel smelting has the characteristics of high hardness, rough surface, strong alkaline adhesion, and excellent wear resistance, making it a high-quality raw material to replace natural aggregates in the preparation of anti-skid asphalt mixtures. However, the porous structure of steel slag itself results in a large asphalt adsorption capacity and a risk of slight volume expansion. Currently, the industry relies solely on experience to blend steel slag aggregates, lacking a quantitative design formula that considers the coupling of multiple variables such as multi-level voids, steel slag activity, and fatigue damage. This leads to poor mix proportion accuracy and difficulty in guaranteeing the stability of the mixture's road performance.

[0003] The current national standard Marshall mix design method only uses the volumetric and mechanical properties of the mixture as the core control basis, and the skid resistance index is only used as a post-construction testing item, which cannot control the skid resistance structure of the mixture in advance. At the same time, the skid resistance design of SMA mixture cannot match the coupling effect of multi-level void interaction, steel slag activity change and long-term fatigue load during the actual service of the road. There is no complete set of quantitative design methods for fine SMA + all steel slag fine aggregate system.

[0004] Therefore, there is an urgent need for a mix design method and application for asphalt mixtures based on improved skid resistance to solve the above problems. Summary of the Invention

[0005] To overcome the shortcomings of the existing technology, this invention provides a method and application for designing asphalt mixture mix proportions based on improved skid resistance. This invention can precisely control the voids in the mixture skeleton and the micro-texture of the surface, effectively suppressing the decline in pavement skid resistance, while balancing the road performance of the mixture with the resource utilization benefits of solid waste.

[0006] To achieve one of the above objectives, the present invention adopts the following technical solution: A method for designing asphalt mixture mix proportions based on improved skid resistance, comprising the following steps: S1. Perform performance testing on raw materials and screen qualified raw materials according to preset admission thresholds; the raw material admission thresholds are as follows: The polishing value of the composite coarse aggregate is ≥44, and the crushing value is ≤22%; the water immersion expansion rate of steel slag is ≤1.5%, and the activity index of steel slag is ≥0.78; the sand equivalent of the steel slag fine aggregate is ≥70%, and the mud content is ≤1.0%. S2. Optimize and refine the aggregate gradation: Prepare several groups (generally three or more groups) of fine alternative gradations and test the basic parameters of multi-stage voids for each group of gradations; S3. Combine the aggregate porosity, steel slag activity and composite aggregate texture coefficient to calculate the multi-level skeleton interlocking anti-slip coefficient and screen the optimal target mineral gradation. S4. Calculate the critical threshold for steel slag fine aggregate filling, accurately control the amount of steel slag fine aggregate, and avoid microscopic pore blockage. S5. Based on the relationship between traffic fatigue damage and steel slag activity decay, the actual lignin fiber content is corrected. S6. Couple multiple volumetric parameters with anti-skid parameters to calculate the optimal anti-skid asphalt-aggregate ratio of the mixture.

[0007] Preferably, the key sieve passing rates of the candidate gradations in step S2 are: 34%~38% for 4.75mm, 18%~24% for 2.36mm, and 10%~13% for 0.075mm. The passing rate of the 4.75mm sieve falls between the requirements of AC-13 and SMA-13 ​​gradations in the "Technical Specification for Construction of Highway Asphalt Pavement" (JTGF40-2004), representing a completely new gradation. The basic porosity parameters of the asphalt mixture corresponding to this gradation are as follows: VCA DRC , VCA MIX VV VCA F VMA, etc.

[0008] Preferably, the multi-stage skeleton interlocking anti-skid coefficient is calculated using the following formula, and the gradation with the smallest K value is selected as the optimal target aggregate gradation: ; In the formula: K is the multi-stage skeleton interlocking anti-skid coefficient; VCA DRC The gap ratio of the dry-compacted coarse aggregate skeleton; VCA MIX This refers to the gap ratio of the coarse aggregate skeleton after compaction; VV is the porosity of the mixture; SA stands for the activity index of steel slag aggregate; VCA F This refers to the local packing gap ratio of fine aggregates; VMA stands for void ratio of mineral aggregate; GTI stands for Composite Aggregate Texture Coefficient.

[0009] Preferably, the critical threshold for steel slag fine aggregate filling is calculated using the following formula, which is used as the final steel slag fine aggregate dosage. The calculation formula is as follows: ; In the formula: T cr The critical threshold for filling steel slag fine aggregate; VCA MIX This refers to the gap ratio of the coarse aggregate skeleton after compaction; SE is the equivalent of fine aggregate sand in steel slag; VV is the porosity of the mixture; VMA stands for void ratio of mineral aggregate.

[0010] Preferably, the anti-slip structure attenuation correction coefficient is calculated using the following formula to correct the actual fiber content: ; F' = F × λ; Where: λ is the anti-skid structure attenuation correction coefficient; TD O The initial construction depth is in mm; TD N The remaining structural depth after fatigue, in mm; SA stands for the activity index of steel slag aggregate; SA max The limiting activity index of steel slag; N represents the number of fatigue wheel rolling cycles; e is the natural constant; F' represents the actual fiber content, % . F represents the standard fiber content.

[0011] Preferably, the optimal anti-lubricating stone ratio is calculated using the following formula: ; In the formula: OAC opt For the optimal anti-lubricating stone ratio, % OAC mar Marshall reference oil-stone ratio, % National Land Agency act These are the measured values ​​of the pendulum. National Land Agency req The minimum required value; VMA is the void fraction of the mineral aggregate, %; VV is the porosity of the mixture.

[0012] To achieve the second objective mentioned above, this invention provides an application of an asphalt mixture mix design method based on improved skid resistance, comprising the following steps: (1) Based on the proportions of each grade of materials in the asphalt mixture designed by the mix proportion, the mixing plant prepares the pavement surface material; (2) Transport the road surface material to the site for paving and compaction; (3) After compaction is completed, quality inspection shall be carried out in accordance with the requirements of the Technical Specification for Construction of Asphalt Pavement of Highway (JTG F40-2004).

[0013] Preferably, in step (2), a 60°C immersion fatigue test is carried out using a Hamburger roller tester, with a fixed number of roller cycles of 50,000.

[0014] Preferably, the volumetric properties of the asphalt mixture are controlled as follows: void ratio of 3.5%~5.0%, aggregate void ratio ≥18.0%, and asphalt saturation of 70%~80%; The acceptance criteria for asphalt mixtures are: initial pendulum value ≥ 68; initial texture depth ≥ 0.72 mm; and texture depth after 50,000 wheel rolling cycles accounting for ≥ 85% of the initial value.

[0015] The advantages of this invention are: (1) In view of the long-term skid resistance degradation of traditional SMA asphalt mixtures, the lack of quantitative proportioning standards for steel slag solid waste aggregates, and the inability of conventional mix design to couple the multiple variables of void structure, aggregate activity and driving fatigue, this invention adopts a new type of fine-textured closely spaced mineral aggregate gradation (between SMA-13 ​​and AC-13), which partially replaces natural basalt aggregates with steel slag aggregates. Based on the step-by-step calculation formula, the gradation, fine aggregate content, fiber content and asphalt-aggregate ratio are quantitatively controlled. The voids of the mixture skeleton and the micro-texture of the surface can be precisely controlled, effectively suppressing the degradation of pavement skid resistance performance, taking into account the road performance of the mixture and the resource utilization benefits of solid waste. No changes are required to the existing construction process. It is suitable for the design of surface asphalt mixtures for highways, urban roads, municipal interchanges, high-grade highways and other road sections.

[0016] (2) The present invention adopts fine-grained gradation to optimize the mineral structure and compound steel slag coarse and fine composite aggregates. Through multi-level void verification, fine aggregate filling control, fiber content fatigue correction and asphalt-aggregate ratio optimization, the macroscopic skeleton skid resistance and micro-texture skid resistance of the mixture are synergistically improved. On the basis of meeting the road use index, the skid resistance service life of asphalt pavement is extended, and the resource utilization of industrial solid waste steel slag is realized.

[0017] (3) This invention uses fine-grained SMA gradation combined with steel slag composite aggregate, while taking into account the stability of the coarse aggregate interlocking skeleton and the micro-rough texture of the fine aggregate. It accurately quantifies the synergistic effects of multiple variables such as multi-level void structure, chemical activity of steel slag, traffic fatigue load, and cleanliness of fine aggregate on anti-skid performance. Compared with traditional empirical design methods, the accuracy of mix design is significantly improved, effectively solving the problems of easy clogging of voids in fine SMA mixtures, abnormal asphalt adsorption of steel slag aggregates, and rapid passivation of anti-skid structure under long-term load. The initial anti-skid pendulum value, texture depth, and long-term anti-skid retention rate of the finished mixture are all greatly improved. The entire design process can be completed using conventional testing equipment in road laboratories without the need for additional special testing devices. During construction, there is no need to modify the existing mixing, paving, and compaction processes. It is suitable for most road construction sites and laboratory conditions in China. At the same time, it can dispose of steel slag industrial solid waste on a large scale, reduce the cost of natural stone mining, and take into account road traffic safety, engineering economy, and environmental benefits of solid waste resource utilization. Detailed Implementation

[0018] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0019] Example 1 The specific steps for designing the mix proportions of fine-grained SMA-13 ​​steel slag composite asphalt mixture are as follows: Step S1: Conduct a full set of physical, mechanical, and activity tests on the raw materials according to the preset access threshold indicators. The tests use conventional road testing equipment such as Marshall stability tester, crushing value tester, expansion rate test device, and pendulum friction tester to obtain the measured parameters of the raw materials in sequence: polished value PSV of composite coarse aggregate = 46, crushing value = 20.3%, water immersion expansion rate of steel slag = 1.21%, activity index of steel slag SA = 0.85, sand equivalent SE of steel slag fine aggregate = 73%, mud content = 0.72%, texture coefficient of composite aggregate GTI = 1.41. All test indicators meet the access threshold, the raw materials are deemed qualified, and can proceed to the next step of gradation design.

[0020] Step S2: Following the requirements for fine SMA gradation, design three sets of gradient mineral aggregate gradations. The content of steel slag coarse aggregate in the three sets of gradations is uniformly set at 45%, and all fine aggregates are made of steel slag fine aggregate. Grade 1 (coarse skeleton): 45% steel slag coarse aggregate, 42.3% basalt coarse aggregate, 6.7% steel slag fine aggregate, and 6% mineral powder; Grade 2 (median skeleton): 45% steel slag coarse aggregate, 38.6% basalt coarse aggregate, 10.4% steel slag fine aggregate, and 6% mineral powder; Grade 3 (slightly fine and dense): 45% steel slag coarse aggregate, 33.1% basalt coarse aggregate, 15.9% steel slag fine aggregate, and 6% mineral powder; The combined passing rates of the three gradations with different sieve apertures are shown in Table 1 below: Table 1. Synthetic passing rate of different gradations and sieve apertures

[0021] The measured uniform foundation void parameters are shown in Table 2 below: Table 2. Porosity parameters of foundations with different gradations

[0022] Step S3: Substitute all the measured parameters from steps S1 and S2 into the following formula, and calculate the anti-skid coefficients of the three sets of gradation multi-stage skeleton interlocking one by one: ; The calculated K value for gradation 1 is 16.9, for gradation 2 it is 18.5, and for gradation 3 it is 21.0. The gradation 1 with the smallest value is selected as the final target mineral gradation in this embodiment, and all subsequent designs are based on this set of fine-to-coarse skeleton gradations.

[0023] Step S4: Extract the void parameters corresponding to the optimal gradation in Step S3: VCA=27.6%, VV=4.3%, VMA=18.7%. Combined with the measured sand equivalent SE=73% in Step S1, substitute them into the following formula to calculate the critical threshold for steel slag fine aggregate filling: ; The calculated critical threshold for filling is: T cr =6.11%, as the final steel slag fine aggregate dosage, to prevent excessive filling and clogging of the microscopic anti-slip voids in the mixture.

[0024] Step S5: Preset the equivalent fatigue wheel rolling cycles N=50000 times, and measure the initial texture depth of the mixture. TD O =0.83mm, remaining structural depth after 50,000 wheel rolling cycles TD N =0.71mm, given the limiting activity index of steel slag. SA max =0.92, substitute all parameters into the following formula: ; F' = F × λ; The calculated anti-slip structure attenuation correction coefficient λ = 0.93; the standard fiber content F = 0.3%, and the actual fiber content F' in construction is 0.279%, which meets the requirements of the reasonable fiber content range.

[0025] Adjust the steel slag coarse aggregate according to the determined final fine aggregate dosage (filling critical threshold) so that the total material usage ratio remains at 100%.

[0026] Specifically: steel slag coarse aggregate accounts for 45.59%, basalt coarse aggregate accounts for 42.3%, steel slag fine aggregate accounts for 6.11%, and mineral powder accounts for 6%. Fiber content is 0.279%.

[0027] Step S6: Measure the reference oil-stone ratio using a standard Marshall test. OAC mar =6.2%, measured initial pendulum value of the mixture National Land Agency act =70, minimum required pendulum value National Land Agency req =68, combining the VMA, VV, and SA parameters, and substituting them into the following formula to calculate the oil-stone ratio: ; The optimal anti-lubricating asphalt aggregate ratio (OAC) was finally obtained, which was 5.94%, and the final asphalt dosage was determined.

[0028] The final mix proportions are: 45.59% steel slag coarse aggregate, 42.3% basalt coarse aggregate, 6.11% steel slag fine aggregate, and 6% mineral powder. Fiber content is 0.279%. The oil-aggregate ratio is 5.94%.

[0029] Step S7: In accordance with the test requirements, a 60℃ immersion fatigue test was carried out using a Hamburg roller mill. The number of roller mill cycles was fixed at 50,000. The volumetric parameters of the mixture were tested simultaneously: void ratio VV=4.3%, aggregate void ratio VMA=18.7%, and asphalt saturation VFA=77%. All volumetric parameters met the limits of the volumetric parameters of asphalt mixtures, and the test conditions and parameters met the standards.

[0030] Step S8: Conduct comprehensive performance testing on the formed asphalt mixture according to the acceptance criteria. Measured results: Measured pendulum value National Land Agency act =70, initial construction depth TD O =0.76mm, and the texture depth after 50,000 wheel rolling cycles accounts for 87.2% of the initial value; at the same time, the Marshall stability was measured to be 13.12kN, the dynamic stability was 8896 cycles / mm, and the low-temperature bending failure strain was 3215με. These mechanical properties all meet the requirements of the "Technical Specification for Construction of Highway Asphalt Pavement" (JTG F40—2004), and all acceptance indicators are qualified. The mix design is now complete.

[0031] Comparative Example 1 Traditional Marshall design for SMA-13 ​​aggregate (without steel slag aggregate, traditional design method): The design method for this comparative proportion adopts the mix proportion determination method in Appendix B and Appendix C of the current standard "Technical Specification for Construction of Highway Asphalt Pavement" (JTG F40-2004). It uses conventional SMA gradation, a 4.75mm pass rate of 28%, and all aggregates are natural basalt. The standard fiber content is 0.3%, the Marshall reference asphalt-aggregate ratio is 6.1%, and there is no pre-design for skid resistance indicators. The measured core skid resistance indicator is the initial measured pendulum value. National Land Agency act =62, initial construction depth TD O =0.71mm.

[0032] Comparative Example 2 Fine SMA + steel slag aggregate (traditional design method): The gradation and steel slag aggregate ratio of this comparative example are consistent with those of Example 1. The determination of the asphalt-aggregate ratio and fiber ratio adopts the methods in Appendix B and Appendix C of the current standard "Technical Specification for Construction of Asphalt Pavement of Highway" (JTG F40-2004).

[0033] The asphalt mixtures designed in Example 1 and Comparative Examples 1-2 were subjected to 50,000 wheel rolling cycles. The results of comparing the proportion of texture depth to the initial value are shown in Table 3 below: Table 3 Comparison results between Example 1 and Comparative Examples 1-2

[0034] As shown in Table 3 above, the asphalt mixture designed in Comparative Example 1 has a texture depth of 75.1% of the initial value after 50,000 wheel rolling cycles, while the asphalt mixture designed in Comparative Example 2 has a texture depth of 80.3% of the initial value after 50,000 wheel rolling cycles. The asphalt mixture designed in this invention has a texture depth of 87.2% of the initial value after 50,000 wheel rolling cycles, which is much higher than that of Comparative Example 1 and Comparative Example 2. Furthermore, its overall skid resistance and durability are also much higher than those of Comparative Example 1 and Comparative Example 2. Compared with the design scheme of this invention, Comparative Example 1 and Comparative Example 2 show a significant gap in long-term skid resistance and durability, demonstrating the technical superiority of the formula system of this invention.

[0035] The above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for designing the mix proportions of asphalt mixtures based on improved skid resistance, characterized in that, The specific steps are as follows: S1. Conduct performance testing on raw materials and screen qualified raw materials according to preset admission thresholds; the raw material admission thresholds are as follows: The polishing value of the composite coarse aggregate is ≥44, and the crushing value is ≤22%; the water immersion expansion rate of steel slag is ≤1.5%, and the activity index of steel slag is ≥0.78; the sand equivalent of the steel slag fine aggregate is ≥70%, and the mud content is ≤1.0%. S2. Prepare several sets of alternative gradations and test the basic parameters of multi-stage voids for each set of gradations. S3. Combine the aggregate porosity, steel slag activity and composite aggregate texture coefficient to calculate the multi-level skeleton interlocking anti-slip coefficient and screen the optimal target mineral gradation. S4. Calculate the critical threshold for steel slag fine aggregate filling and control the amount of steel slag fine aggregate added. S5. Based on the relationship between traffic fatigue damage and steel slag activity decay, the actual lignin fiber content is corrected. S6. Couple volumetric parameters with anti-skid parameters to calculate the optimal anti-skid asphalt-aggregate ratio of the mixture; The multi-stage skeleton interlocking anti-skid coefficient is calculated using the following formula, and the gradation with the smallest K value is selected as the optimal target aggregate gradation: ; In the formula: K is the multi-stage skeleton interlocking anti-skid coefficient; VCA DRC The gap ratio of the dry-compacted coarse aggregate skeleton; VCA MIX This refers to the gap ratio of the coarse aggregate skeleton after compaction; VV is the porosity of the mixture; SA stands for the activity index of steel slag aggregate; VCA F This refers to the local packing gap ratio of fine aggregates; VMA stands for void ratio of mineral aggregate; GTI is the texture coefficient of composite aggregates; The critical threshold for steel slag fine aggregate filling is calculated using the following formula, which is used as the final steel slag fine aggregate dosage. The calculation formula is as follows: ; In the formula: T cr The critical threshold for filling steel slag fine aggregate; VCA MIX This refers to the gap ratio of the coarse aggregate skeleton after compaction; SE is the equivalent of fine aggregate sand in steel slag; VV is the porosity of the mixture; VMA stands for void ratio of mineral aggregate; The anti-slip structure attenuation correction factor is calculated using the following formula to correct the actual fiber content: ; F' = F × λ; Where: λ is the anti-skid structure attenuation correction coefficient; TD O The initial construction depth is in mm; TD N The remaining structural depth after fatigue, in mm; SA stands for the activity index of steel slag aggregate; SA max The limiting activity index of steel slag; N represents the number of fatigue wheel rolling cycles; e is the natural constant; F' represents the actual fiber content, % . F represents the standard fiber content, % . The optimal anti-lubricating stone ratio is calculated using the following formula: ; In the formula: OAC opt For the optimal anti-lubricating stone ratio, % OAC mar Marshall reference oil-stone ratio, % BPN act These are the measured values ​​of the pendulum. BPN req The minimum required value; VMA is the void fraction of the mineral aggregate, %; VV is the porosity of the mixture, %; SA stands for Steel Slag Aggregate Activity Index.

2. The asphalt mixture mix design method based on improved skid resistance according to claim 1, characterized in that, The sieve passing rates of the alternative gradations in step S2 are: 34%~38% for 4.75mm, 18%~24% for 2.36mm, and 10%~13% for 0.075mm.

3. An application of the asphalt mixture mix design method based on improved skid resistance as described in any one of claims 1-2, characterized in that, Includes the following steps: (1) Based on the proportions of each grade of materials in the asphalt mixture designed by the mix proportion, the mixing plant prepares the pavement surface material; (2) Transport the road surface material to the site for paving and compaction; (3) After compaction is completed, quality inspection shall be carried out in accordance with the requirements of the Technical Specification for Construction of Asphalt Pavement on Highways.

4. The application of the asphalt mixture mix design method based on improved skid resistance as described in claim 3, characterized in that: In step (2), a 60°C immersion fatigue test was carried out using a Hamburg roller tester, with a fixed number of roller cycles of 50,000.

5. The application of the asphalt mixture mix design method based on improved skid resistance as described in claim 3, characterized in that the asphalt... The volumetric properties of the mixture are controlled as follows: void ratio of 3.5%~5.0%, aggregate void ratio ≥18.0%, and asphalt saturation of 70%~80%.

6. The application of the asphalt mixture mix design method based on improved skid resistance as described in claim 3, characterized in that the asphalt... The acceptance criteria for the mixture are: initial pendulum value ≥ 68; initial texture depth ≥ 0.72 mm, and texture depth after 50,000 wheel rolling cycles accounting for ≥ 85% of the initial value.

Citation Information

Patent Citations

  • Steel slag and rubber asphalt concrete and preparation method thereof

    CN101967047A

  • Design method of double-framework-high-viscosity cement paste asphalt mixture for anti-skid surface layer of road surface

    CN122201551A