Primerless water-based color paint, and preparation method and application thereof
By using water-based paints made of polyether-type polyurethane resin and high glass transition temperature acrylic resin, the complexity and environmental issues of automotive bumper painting processes have been solved. This has resulted in simplified processes, reduced costs, and improved water resistance, making the paints suitable for automotive exterior coatings on a variety of substrates.
Patent Information
- Application Number
- CN202610957887.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-30
- Publication Date
- 2026-08-25
AI Technical Summary
Existing automotive bumper painting processes suffer from problems such as complex processes, high costs, poor environmental performance, poor resistance to high-pressure water jetting, and poor versatility, especially in terms of poor compatibility with PP substrates and PC+ABS substrates.
Using polyether-type polyurethane resin containing a polytetrahydrofuran ether diol structure and acrylic resin with a glass transition temperature higher than 60°C as film-forming resins, combined with an aqueous system, a primer-free waterborne color paint coating is prepared, which directly forms a two-coat system with PP or PC+ABS substrates, avoiding the need for additional PP primer spraying.
It simplifies the process, reduces costs, improves high-pressure water jet resistance, is environmentally friendly, and is suitable for a variety of substrates, meeting the aesthetic and functional requirements of automotive exteriors.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of coating technology, and particularly relates to a primer-free water-based colored paint coating, its preparation method and application. Background Technology
[0002] As one of the most critical components of a car's exterior, the bumper not only serves the safety function of absorbing collision energy but also directly affects the vehicle's visual aesthetics and brand image. Currently, the mainstream base material for car bumpers is polypropylene (PP) and its modified materials. As a non-polar semi-crystalline polymer, it has low surface energy, poor adhesion to polar paints, and is difficult to paint directly.
[0003] Traditional bumper painting processes typically employ a three-coat system of "primer + color paint + clear coat," which involves spraying a layer of solvent-based chlorinated polypropylene (CPP) primer (commonly known as PP water) onto a PP substrate. This utilizes the good affinity between CPP and the PP substrate, as well as its compatibility with polar resins in the color paint, to achieve interlayer adhesion.
[0004] The existing three-coat system has the following drawbacks and shortcomings:
[0005] (1) Complex process and high cost: The existing three-coat system requires additional PP primer spraying, which adds at least one spraying and one baking process, resulting in long cycle, high energy consumption and high cost.
[0006] (2) Poor environmental performance: The solvent-based CPP primer used in the existing three-coat system contains a large amount of volatile organic compounds (VOCs), which increases VOC emissions and causes serious environmental pollution.
[0007] (3) Poor resistance to high-pressure water jetting: The paint film peeled off when tested under the conditions of 90° spray angle, 10cm spacing, 60℃, 60s and 70bar.
[0008] (4) Poor versatility: The exterior includes non-PP substrate components such as spoilers. PP primer is not well matched with PC+ABS materials such as spoilers. It has poor water resistance and high-pressure water jet resistance. Separating a separate spraying line will also increase production costs. Summary of the Invention
[0009] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the background art above, and to provide a primer-free water-based paint coating for automotive exteriors, its preparation method and application.
[0010] To solve the above-mentioned technical problems, the technical solution proposed by this invention is as follows: A primer-free water-based paint coating includes a film-forming resin, wherein the film-forming resin includes a polyether-type polyurethane resin and an acrylic resin, wherein the polyether-type polyurethane resin contains a polytetrahydrofuran ether diol structure, and the glass transition temperature Tg of the acrylic resin is greater than 60°C, and the mass ratio of the polyether-type polyurethane resin to the acrylic resin is (40-60):(5-15).
[0011] As a further improvement, both the polyether-type polyurethane resin and the acrylic resin have a hydroxyl value of 0.
[0012] As a further improvement, the glass transition temperature (Tg) of the acrylic resin is 60-100℃.
[0013] As a further improvement, the primer-free water-based paint coating also includes color paste or pigment and additives, wherein the additives are selected from one or more of film-forming aids, wetting agents, pH adjusters, defoamers, and rheology modifiers.
[0014] As a further improvement, the film-forming aid is one or both of ethylene glycol butyl ether and N-methylpyrrolidone; And / or, the wetting agent component is a polyether-modified siloxane; And / or, the pH adjuster is an organic amine; And / or, the defoamer component is tetramethyldecynyl diol; And / or, the rheology modifier is an alkali-swellable non-associated acrylic thickener.
[0015] The present invention also provides a method for preparing the primer-free water-based colored paint coating, comprising: Polyether-type polyurethane resin and acrylic resin are dispersed, and then additives and water are added for further dispersion to obtain the base material; The base material is mixed with color paste or pigment to obtain a primer-free water-based paint coating.
[0016] The present invention also provides a primer-free coating, comprising: A paint layer is formed by coating a substrate with the primer-free water-based paint coating or the primer-free water-based paint coating obtained by the preparation method. The varnish layer is formed by applying varnish onto the colored varnish layer.
[0017] As a further improvement, the substrate includes a PP substrate or a PC+ABS substrate.
[0018] The present invention also provides an application of the primer-free water-based paint coating or the primer-free water-based paint coating or the primer-free coating obtained by the preparation method, characterized in that it is used for automotive exterior trim.
[0019] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) The water-based paint coating of the present invention uses polyether polyurethane resin containing polytetrahydrofuran ether diol structure as the main body and a small amount of acrylic resin with Tg>60℃. It has good affinity and good adhesion to the flame-treated PP substrate, realizing a two-layer coating system of "paint + clear coat". There is no need to add an additional PP primer spraying process, achieving the effect of "no primer". The process is short and the cost is low.
[0020] (2) The water-based paint coating of the present invention improves the high pressure water flushing resistance and meets the requirements of testing under the test conditions of 90° spray angle, 10cm spacing, 60℃, 60s and 70bar.
[0021] (3) The water-based paint coating of the present invention adopts a water-based system, avoiding the use of organic solvents, which is more environmentally friendly.
[0022] (4) The water-based paint coating of the present invention meets the universality of automotive exterior parts and can be matched with PP, PC+ABS materials at the same time. Detailed Implementation
[0023] To facilitate understanding of the present invention, the present invention will be described more fully and in detail below with reference to preferred embodiments, but the scope of protection of the present invention is not limited to the following specific embodiments.
[0024] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of the invention.
[0025] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this invention can be purchased from the market or prepared by existing methods.
[0026] In some specific embodiments, the primerless water-based paint coating for automotive exteriors of the present invention includes a film-forming resin, wherein the film-forming resin includes a polyether-type polyurethane resin and an acrylic resin, and the mass ratio of the polyether-type polyurethane resin to the acrylic resin is (40-60):(5-15).
[0027] The polyether-type polyurethane resin of the present invention is required to contain a polytetrahydrofuran ether diol (PTMG) structure, that is, the polyether-type polyurethane resin contains PTMG segments (the soft segments of the polyether-type polyurethane resin are prepared from diols containing PTMG), which provides the resin with excellent mechanical properties and elasticity.
[0028] The polyether-type polyurethane resin of this invention is required to be free of hydroxyl and carboxyl groups (the hydroxyl value of the polyether-type polyurethane resin is 0). This ensures that the coating film is less prone to water molecule penetration, which could lead to bubbling and decreased adhesion to the substrate under high temperature and humidity conditions. Hydroxyl and carboxyl groups are hydrophilic groups, and their presence can affect performance in subsequent water resistance tests.
[0029] The ether bonds (COC) in the polyether segments of polyether-type polyurethane resins are chemically stable and not easily hydrolyzed, ensuring their water resistance as paints. The low rotational barrier within the ether bonds and low glass transition temperature result in good elasticity at low temperatures, making it less prone to stress after clear coat application, which could lead to decreased adhesion to the substrate.
[0030] The excellent elasticity of the polyether-type polyurethane resin of the present invention allows the paint film to stretch and bend along with the PP substrate, and its volume change and internal stress are small during curing, thus avoiding the decrease in adhesion caused by the shrinkage stress of the paint film.
[0031] In some embodiments, the polyether polyurethane resin is one or both of RHERITM U114 (Guangdong Runchang Nanxing New Materials Co., Ltd.) and Covestro NeoRez E-123. Both of the above polyether polyurethane resins contain a PTMG structure and have a hydroxyl value of 0.
[0032] The acrylic resin used in this invention requires a glass transition temperature (Tg) > 60℃, for example, 60-100℃. The glass transition temperature is used to address the softening and wrinkling issues of the paint film under high temperature and humidity conditions. Acrylic resin has a high glass transition temperature, making it less prone to bubbling and softening in high temperature and humidity environments. Adding a small amount of acrylic resin can effectively improve the softening problem of the paint film during water resistance tests. This avoids appearance problems such as decreased gloss and brightness caused by paint film softening during damp heat tests on exterior parts.
[0033] The acrylic resin used in this invention is required to be free of hydroxyl and carboxyl groups (the hydroxyl value of acrylic resin is 0). The coating film is less prone to water molecule penetration, which can lead to bubbling and reduced adhesion to the substrate under high temperature and high humidity conditions.
[0034] In some embodiments, the acrylic resin is DB3428 (Wuhan Double Bond New Material Co., Ltd.). This acrylic resin has a Tg > 60°C and a hydroxyl value of 0.
[0035] The present invention is a water-based paint coating, and the solvent used is water, preferably deionized water. The mass ratio of water added to polyether polyurethane resin is (5-10):(40-60).
[0036] In addition to the film-forming resin, additives can be added as needed, such as film-forming aids, wetting agents, pH adjusters, defoamers, and rheology modifiers.
[0037] In some preferred embodiments, the raw materials for preparing the primerless water-based paint coating for automotive exteriors include the following components (base materials) by weight: 40-60 parts of polyether polyurethane resin, 5-15 parts of acrylic resin, 3-6 parts of film-forming aid, 5-10 parts of deionized water, 0-1 part of wetting agent, 0.1-0.3 parts of pH adjuster, 0-1 part of defoamer, and 1-3 parts of rheology modifier.
[0038] In some preferred embodiments, the film-forming aid is one or both of BCS (ethylene glycol butyl ether) and NMP (N-methylpyrrolidone). Preferably, BCS and NMP are used in a mass ratio of 1:(0.8-1.2), more preferably 1:1 (50% BCS, 50% NMP), with boiling points of 171°C and 202°C respectively, to temporarily lower the resin's glass transition temperature and ensure uniform film formation.
[0039] In some preferred embodiments, the substrate wetting agent is a polyether-modified siloxane, which, upon addition to the liquid, accumulates on the liquid surface, significantly reducing the liquid surface tension; its amphiphilic structure allows it to oriented at the liquid-solid interface, reducing the interfacial energy difference and achieving efficient wetting. In some preferred embodiments, the substrate wetting agent is one or more of Evonik Chemical's EVONIK WET KL 245, TEGO 4100, TEGO Wet KL 245, and BYK-346 from BYK Chemical, and its composition is a polyether-modified siloxane.
[0040] In some preferred embodiments, the pH adjuster is an organic amine, preferably DMEA (dimethylethanolamine), which can react with the carboxyl groups in polyurethane to control the pH of the system at 8.0-9.0, prevent resin flocculation under acidic conditions, and avoid damage to the spraying equipment; it is also used in conjunction with an alkali swelling thickener to adjust the rheological properties of the coating.
[0041] In some preferred embodiments, the defoamer is tetramethyldecynediol, which can significantly reduce the dynamic surface tension of the system and has defoaming and wetting effects. For example, it can be EVONIK 104E, whose active ingredient is tetramethyldecynediol.
[0042] In some preferred embodiments, the rheology modifier is an alkali-swellable (ASE) non-associated acrylic thickener, a highly efficient low-shear thickener that thins under high shear, improving the coating's anti-sagging and anti-settling properties. In some preferred embodiments, one or more of BASF Rheovis AS 1130 and Rheovis® AS 1188, whose components are alkali-swellable (ASE) non-associated acrylic thickeners, may be used.
[0043] In some specific embodiments, the preparation method of the primerless water-based paint coating for automotive exterior trim of the present invention includes: dispersing polyether-type polyurethane resin and acrylic resin, then adding additives and water for further dispersion to obtain a base material. The base material is then mixed with a colorant to obtain the water-based paint coating. In some preferred embodiments, the mass ratio of base material to colorant is 100:(35-45), and the colorant mass concentration is 60-80%.
[0044] In some preferred embodiments, the specific preparation method is as follows: (1) Disperse the polyether-type polyurethane resin at 400-600 rpm for 4-10 min; (2) Slowly add acrylic resin to the material obtained in step (1) at a dispersion rate of 400-600 rpm and disperse for 4-10 min; (3) After premixing the film-forming aid and water, add it to the material obtained in step (2) at a dispersion rate of 400-600 rpm and disperse for 8-15 min; (4) Add the wetting agent, pH adjuster and defoamer to the material obtained in step (3) in sequence at a dispersion rate of 400-600 rpm and disperse for 8-15 min; (5) Increase the dispersion rate to 600-800 rpm, add rheology modifier to the material obtained in step (4), disperse for 8-15 min, and obtain the base material.
[0045] The obtained base material and color paste are mixed to obtain a primer-free water-based paint coating for automotive exteriors.
[0046] In use, the water-based paint is sprayed onto a PP or PC+ABS substrate, preferably with a film thickness of 15-25 μm. In some embodiments, the curing method is as follows: baking at 70-90°C for 15-30 minutes to form a paint layer. After the paint layer is formed, a clear varnish is sprayed onto it, and then cured to obtain a primer-free coating layer.
[0047] The water-based paint coating of this invention exhibits good color stability. In contrast, if polyolefin resin is used, on the one hand, polyolefin resin has a wide molecular weight distribution, and the low molecular weight components easily carry pigments and additives, resulting in color inconsistency with the high molecular weight components; on the other hand, polyolefins have extremely low Hansen solubility parameters, and pigments easily aggregate, causing color fading.
[0048] Example 1 The base composition of the primerless water-based paint for automotive exterior trim in this embodiment is as follows:
[0049] Preparation method: 1. Disperse the above-mentioned polyether polyurethane at 500 rpm for 5 min; 2. Slowly add the acrylic resin to step 1 at a dispersion rate of 500 rpm and disperse for 5 min; 3. After premixing the film-forming aid and water, add it to step 2 at a dispersion rate of 500 rpm and disperse for 10 min; 4. Add the wetting agent, pH adjuster, and defoamer sequentially to step 3 at a dispersion rate of 500 rpm and disperse for 10 min. 5. Increase the dispersion rate to 700 rpm, add the rheology modifier to step 4, disperse for 10 min, and obtain the base material.
[0050] Example 2 The base composition of the primerless water-based paint for automotive exterior trim in this embodiment is as follows:
[0051] Preparation method: 1. Disperse the above-mentioned polyether polyurethane at 500 rpm for 5 min; 2. Slowly add the acrylic resin to step 1 at a dispersion rate of 500 rpm and disperse for 5 min; 3. After premixing the film-forming aid and water, add it to step 2 at a dispersion rate of 500 rpm and disperse for 10 min; 4. Add the wetting agent, pH adjuster, and defoamer sequentially to step 3 at a dispersion rate of 500 rpm and disperse for 10 min. 5. Increase the dispersion rate to 700 rpm, add the rheology modifier to step 4, disperse for 10 min, and obtain the base material.
[0052] Example 3 The base composition of the primerless water-based paint for automotive exterior trim in this embodiment is as follows:
[0053] Preparation method: 1. Disperse the above-mentioned polyether polyurethane at 500 rpm for 5 min; 2. Slowly add the acrylic resin to step 1 at a dispersion rate of 500 rpm and disperse for 5 min; 3. After premixing the film-forming aid and water, add it to step 2 at a dispersion rate of 500 rpm and disperse for 10 min; 4. Add the wetting agent, pH adjuster, and defoamer sequentially to step 3 at a dispersion rate of 500 rpm and disperse for 10 min. 5. Increase the dispersion rate to 700 rpm, add the rheology modifier to step 4, disperse for 10 min, and obtain the base material.
[0054] Comparative Example 1 The composition of the water-based paint base in this comparative example is as follows:
[0055] Preparation method: 1. Disperse the above-mentioned polyether polyurethane at 500 rpm for 5 min; 2. After premixing the film-forming aid and water, add it to step 1 at a dispersion rate of 500 rpm and disperse for 10 min; 3. Add the wetting agent, pH adjuster, and defoamer sequentially to step 2 at a dispersion rate of 500 rpm and disperse for 10 min; 4. Increase the dispersion rate to 700 rpm, add the rheology modifier to step 3, disperse for 10 min, and obtain the base material.
[0056] Comparative Example 2 The composition of the water-based paint base in this comparative example is as follows:
[0057] Preparation method: 1. Disperse the above-mentioned polycarbonate polyurethane at 500 rpm for 5 min; 2. After premixing the film-forming aid and water, add it to step 1 at a dispersion rate of 500 rpm and disperse for 10 min; 3. Add the wetting agent, pH adjuster, and defoamer sequentially to step 2 at a dispersion rate of 500 rpm and disperse for 10 min; 4. Increase the dispersion rate to 700 rpm, add the rheology modifier to step 3, disperse for 10 min, and obtain the base material.
[0058] Comparative Example 3 The composition of the water-based paint base in this comparative example is as follows:
[0059] Preparation method: 1. Disperse the above chlorinated polyolefin acrylic emulsion at 500 rpm for 5 min; 2. After premixing the film-forming aid and water, add it to step 1 at a dispersion rate of 500 rpm and disperse for 10 min; 3. Add the wetting agent, pH adjuster, and defoamer sequentially to step 2 at a dispersion rate of 500 rpm and disperse for 10 min; 4. Increase the dispersion rate to 700 rpm, add the rheology modifier to step 3, disperse for 10 min, and obtain the base material.
[0060] Comparative Example 4 The composition of the water-based paint base in this comparative example is as follows:
[0061] Preparation method: 1. Disperse the above acrylic resin at 500 rpm for 5 min; 2. After premixing the film-forming aid and water, add it to step 1 at a dispersion rate of 500 rpm and disperse for 10 min; 2. Add the wetting agent, pH adjuster, and defoamer sequentially to step 2 at a dispersion rate of 500 rpm and disperse for 10 min; 4. Increase the dispersion rate to 700 rpm, add the rheology modifier to step 3, disperse for 10 min, and obtain the base material.
[0062] Comparative Example 5 The composition of the water-based paint base in this comparative example is as follows:
[0063] Preparation method: 1. Disperse the above-mentioned polyether polyurethane at 500 rpm for 5 min; 2. Slowly add the acrylic resin to step 1 at a dispersion rate of 500 rpm and disperse for 5 min; 3. After premixing the film-forming aid and water, add it to step 2 at a dispersion rate of 500 rpm and disperse for 10 min; 4. Add the wetting agent, pH adjuster, and defoamer sequentially to step 3 at a dispersion rate of 500 rpm and disperse for 10 min. 5. Increase the dispersion rate to 700 rpm, add the rheology modifier to step 4, disperse for 10 min, and obtain the base material.
[0064] Comparative Example 6 The composition of the water-based paint base in this comparative example is as follows:
[0065] Preparation method: 1. Disperse the above-mentioned polyether polyurethane at 500 rpm for 5 min; 2. Slowly add the acrylic resin to step 1 at a dispersion rate of 500 rpm and disperse for 5 min; 3. After premixing the film-forming aid and water, add it to step 2 at a dispersion rate of 500 rpm and disperse for 10 min; 4. Add the wetting agent, pH adjuster, and defoamer sequentially to step 3 at a dispersion rate of 500 rpm and disperse for 10 min. 5. Increase the dispersion rate to 700 rpm, add the rheology modifier to step 4, disperse for 10 min, and obtain the base material.
[0066] Construction methods and performance testing: 1. Wipe the PP substrate with alcohol and then flame treat it until the Dyne value is >38; wipe the PC+ABS substrate with alcohol.
[0067] 2. Mix the base material prepared in the above examples and comparative examples with the color paste (70% titanium dioxide paste) at a ratio of 100:40, and then spray it onto the PP substrate or PC+ABS substrate. The film thickness is between 15-25μm. Bake at 80℃ for 20 minutes and then cool at room temperature. 3. Spray the oil-based varnish (Matsui QF311-10059:QFH-109:QFG-208=100:33:5) onto the color paint layer and bake at 80℃ for 60 minutes.
[0068] The test results are shown in Table 1-2 below: Table 1
[0069] Table 2
[0070] As can be seen from the table above: Compared with Comparative Example 1, Examples 1-3 did not contain acrylic resin, resulting in a lower glass transition temperature for the paint layer, making it more prone to softening and wrinkling in a 40°C water immersion environment.
[0071] Comparing Comparative Example 1 and Comparative Example 2, it is shown that the polyether-type polyurethane resin used in this invention is superior to the polycarbonate-type polyurethane resin in terms of high-pressure water flushing performance.
[0072] Compared with Comparative Examples 2-4, Examples 1-3 used polycarbonate polyurethane and modified polyolefin, while Comparative Example 4 did not add polyether polyurethane resin. The paint film had poor elasticity, high internal stress and poor adhesion after topcoat, and the primer peeled off during the high-pressure water jet test.
[0073] Compared with Comparative Example 5, Examples 1-3 show that after applying a topcoat of polyether polyurethane resin without PTMG structure to a PP substrate, the adhesion of the blister coating decreases and the primer peels off under high pressure water rinsing.
[0074] Compared with Comparative Example 6, Examples 1-3 introduced an acrylic resin containing a glass transition temperature of <60°C and hydroxyl groups (-OH: 1.1%). After being soaked in water, the paint film not only wrinkled but also bubbled.
[0075] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention in any way. Therefore, any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention should fall within the protection scope of the present invention.
Claims
1. A primer-free water-based paint coating, comprising a film-forming resin, characterized in that, The film-forming resin includes a polyether-type polyurethane resin and an acrylic resin. The polyether-type polyurethane resin contains a polytetrahydrofuran ether diol structure. The glass transition temperature (Tg) of the acrylic resin is greater than 60°C. The mass ratio of the polyether-type polyurethane resin to the acrylic resin is (40-60):(5-15).
2. The primer-free water-based paint coating according to claim 1, characterized in that, Both the polyether-type polyurethane resin and the acrylic resin have a hydroxyl value of 0.
3. The primer-free water-based colored paint coating according to claim 1 or 2, characterized in that, The glass transition temperature (Tg) of the acrylic resin is 60-100℃.
4. The primer-free water-based colored paint coating according to claim 1 or 2, characterized in that, The primer-free water-based paint coating also includes color paste or pigment and additives, wherein the additives are selected from one or more of film-forming aids, wetting agents, pH adjusters, defoamers, and rheology modifiers.
5. The primer-free water-based paint coating according to claim 4, characterized in that, The film-forming aid is one or two of ethylene glycol butyl ether and N-methylpyrrolidone; And / or, the wetting agent component is a polyether-modified siloxane; And / or, the pH adjuster is an organic amine; And / or, the defoamer component is tetramethyldecynyl diol; And / or, the rheology modifier is an alkali-swellable non-associated acrylic thickener.
6. A method for preparing a primer-free water-based colored paint coating according to any one of claims 1 to 5, characterized in that, include: Polyether-type polyurethane resin and acrylic resin are dispersed, and then additives and water are added for further dispersion to obtain the base material; The base material is mixed with color paste or pigment to obtain a primer-free water-based paint coating.
7. A primer-free coating, characterized in that, include: A paint layer is formed by coating a substrate with a primer-free water-based paint coating as described in any one of claims 1 to 5 or a primer-free water-based paint coating obtained by the preparation method described in claim 7; The varnish layer is formed by applying varnish onto the colored varnish layer.
8. The primer-free coating according to claim 7, characterized in that, The substrate includes PP substrate or PC+ABS substrate.
9. The application of a primerless water-based paint coating according to any one of claims 1 to 5, or a primerless water-based paint coating obtained by the preparation method according to claim 7, or a primerless coating according to any one of claims 7 to 8, characterized in that, It is used for car exterior trim.