A pure-phase bimetallic selenide and its preparation method, a modified diaphragm and its preparation method and application
A pure-phase (Ni,Co)Se2 bimetallic selenide coating was prepared by inverted encapsulation vapor phase selenization, which solved the problem of not being able to meet the material performance requirements in lithium-sulfur battery separator modification technology. This achieved efficient suppression of polysulfide shuttle and improved the electrochemical performance and structural stability of the battery.
Patent Information
- Application Number
- CN202611176604.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-05
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2046-08-05
AI Technical Summary
Existing lithium-sulfur battery membrane modification technologies face the challenge of single-component materials simultaneously meeting multiple performance requirements, such as strong adsorption capacity, rapid catalytic conversion, high electronic conductivity, and long-term structural stability. The synthesis routes are complex, the preparation conditions are harsh, the costs are high, and there is a lack of coating materials that do not rely on external conductive frameworks such as graphene.
Using a co-precipitation method to synthesize a nickel-cobalt Prussian blue analogue (NiCo PBA) as a structural template, a pure-phase (Ni,Co)Se2 bimetallic selenide coating was prepared through inverted encapsulation vapor-phase selenization treatment. This coating was used to modify PP membranes, achieving multi-dimensional inhibition of polysulfide shuttle through physical blocking, chemical anchoring, and electrochemical catalysis.
Significantly improving the electrochemical performance of lithium-sulfur batteries, the modified separator assembled battery achieved a first-cycle discharge specific capacity of up to 1480 mAh g-1 at a 0.5 C rate, and retained 63.5% of its capacity after 100 cycles. Even at a high rate of 5.0 C, it still achieved a specific capacity of 584 mAh g-1. The charge transfer impedance and interface impedance were significantly reduced, improving the battery's rate performance and long-cycle stability.
Smart Images

Figure CN122685021B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a pure-phase bimetallic selenide and its preparation method, a modified separator and its preparation method and application, belonging to the field of lithium-sulfur battery technology. Background Technology
[0002] Lithium-sulfur batteries are known for their extremely high theoretical specific capacity (1675 mAh g). -1 ) and theoretical energy density (2600 Wh kg) -1 Furthermore, sulfur, as a cathode material, possesses advantages such as high resource abundance, low cost, and environmental friendliness, making it widely regarded as one of the most promising next-generation electrochemical energy storage systems for breaking through the current energy density bottleneck of lithium-ion batteries. However, its commercialization process has long been constrained by a series of intrinsic technical challenges, the most fundamental of which is the "polysulfide shuttle effect." During charge and discharge, soluble long-chain polysulfides (Li2S) generated at the cathode... x (4≤x≤8) will diffuse from the positive electrode region and migrate across the separator to the lithium anode interface. This process not only causes irreversible loss of active sulfur and rapid decline in the specific capacity of the positive electrode, but also exacerbates electrolyte decomposition, lithium anode corrosion and surface passivation, and leads to a significant decrease in coulombic efficiency. Ultimately, this severely restricts the battery's cycle stability, safety and reliability, and its actual usable energy density.
[0003] To address the shuttle effect of polysulfides in lithium-sulfur batteries, researchers have conducted extensive research in various areas, including cathode material design, electrolyte modification, and separator modification. Among these efforts, functional modification of commercial polypropylene (PP) separators to construct composite barriers that integrate multiple functions such as physical barrier, chemical anchoring, and electrochemical catalysis is considered a forward-looking strategy that combines practicality and high efficiency because it offers good process compatibility without altering the main processes of existing battery manufacturing and is easily integrated into large-scale production lines.
[0004] Currently, research on membrane modification mainly focuses on introducing various functional coating materials. For example, some existing technologies use carbon materials such as graphene (DOI:10.1016 / j.ensm.2016.12.004) and carbon nanotubes (DOI:10.1016 / S2095-4956(13)60042-X) for physical adsorption and to construct a conductive network. However, due to the weak chemical affinity of pure carbon materials for polysulfides, their anchoring effect is limited. To enhance chemical interactions, researchers have gradually turned to polar inorganic materials (such as metal oxides, sulfides, and nitrides) and organic polymers. For example, patent document CN120515472A discloses a method of using nitrogen and phosphorus doped graphene-coated hollow carbon spheres (HCS@NPrGO / CeNd) modified with cerium (Ce) and neodymium (Nd) dual rare earth metals as a membrane coating. This design leverages the unique electronic structure of rare earth metals to enhance catalytic activity, while combining the confinement effect of hollow carbon spheres with the conductive network of graphene to significantly improve electrochemical performance. However, this material system involves a wide variety of elements and has a complex structure, requiring multiple delicate processes such as hydrothermal treatment, high-temperature carbonization, and alkaline etching for preparation. This results in cumbersome processes, high costs, and stringent conditions, making it difficult to meet the needs of large-scale production.
[0005] In recent years, metal-organic framework (MOF) materials, especially Prussian blue analogues (PBA) and their thermal conversion derivatives (such as phosphides and selenides) with regular structures, easy synthesis, and rich active sites, have become a research hotspot in the field of lithium-sulfur battery separator modification due to their highly tunable composition and structure and significant chemisorption and catalytic effects on polysulfides. Currently, some studies have applied PBA or its derivatives to lithium-sulfur battery separators, demonstrating different material design strategies but also revealing several common challenges. For example, patent document CN113066964A uses NiCo PBA as a precursor, followed by polydopamine coating, high-temperature carbonization, and subsequent phosphating to prepare bimetallic phosphide-embedded carbon hollow nanocages for separator modification. While this design achieves functional integration of physical confinement and chemical catalysis, the process route is cumbersome, involving hazardous phosphorus sources and high-temperature processes, making large-scale production difficult. For example, patent document CN113422155A uses a nickel-iron selenide / graphene composite as a separator coating, leveraging the conductive network of graphene and the catalytic activity of nickel-iron selenide to improve battery performance. However, this approach is highly dependent on graphene and does not involve further regulation of the intrinsic structure of selenide.
[0006] It is noteworthy that while existing research has applied Ni-Co bimetallic selenides to the modification of lithium-sulfur battery separators, these studies all rely on carbon frameworks or heterostructures of metal compounds to maintain structural stability or improve conductivity. Pure-phase transition metal selenides are prone to aggregation and structural collapse during high-temperature selenization. This reflects, to some extent, a long-standing technical bias in the field: the belief that stable pure-phase transition metal selenides are unattainable and that an external framework is necessary for physical support to obtain usable materials. This not only significantly restricts the simplification of material systems and cost control of preparation processes but also limits the in-depth exploration and effective utilization of the intrinsic catalytic activity of selenides.
[0007] Current membrane modification technology still faces several key bottlenecks, specifically: 1) Single-component materials struggle to simultaneously meet multiple performance requirements, including strong adsorption capacity, rapid catalytic conversion, high electronic conductivity, and long-term structural stability; 2) The synthesis routes and coating processes for most high-performance nanomaterials are complex, demanding in terms of preparation conditions and cost, hindering large-scale production; 3) Particularly noteworthy is the lack of a membrane coating material that does not rely on external conductive frameworks such as graphene. Such a material could achieve precise control over the morphology and phase of the product under mild conditions through a simple and controllable synthesis strategy, preserving the three-dimensional structural advantages of the precursor while fully exposing bimetallic active sites, thus balancing structural inheritance and catalytic activity. The design and controllable preparation of such materials remain a crucial technological gap in this field, requiring significant breakthroughs. Summary of the Invention
[0008] To address the shortcomings of existing technologies, especially the technical challenges of complex synthesis processes for existing high-performance composite materials, reliance on external conductive frameworks such as graphene, and difficulty in large-scale application, this invention provides a pure-phase bimetallic selenide and its preparation method, a modified diaphragm and its preparation method, and its application. Invention Overview:
[0010] This invention uses a nickel-cobalt Prussian blue analogue (NiCo PBA) synthesized by co-precipitation as a structural template and metal source. Through inverted encapsulation-type gas-phase selenization treatment, it is completely converted into a pure-phase (Ni,Co)Se2 bimetallic selenide, successfully preparing a pure-phase (Ni,Co)Se2 nanomaterial with a complete cubic morphology. This nanomaterial is then directly applied as a functional coating to modify PP separators, which can significantly accelerate the polysulfide conversion kinetics and suppress the shuttle effect. It simultaneously inhibits polysulfide shuttle from multiple dimensions such as physical barrier, chemical anchoring, and electrochemical catalysis, thus comprehensively improving the electrochemical performance of lithium-sulfur batteries.
[0011] This invention not only has a simple preparation process that does not rely on a carbon-based framework, but also achieves effective control over the phase and microstructure of the product by precisely regulating the selenization temperature. The resulting material has both a bimetallic synergistic catalytic effect and excellent structural stability.
[0012] Terminology Explanation:
[0013] Room temperature: refers to 20-25 °C.
[0014] PVDF: refers to polyvinylidene fluoride
[0015] KB refers to conductive carbon black (Ketjen black).
[0016] This invention is achieved through the following technical solution:
[0017] In a first aspect, the present invention provides a method for preparing a pure-phase bimetallic selenide, which employs an inverted encapsulation-type vapor-phase selenization process, comprising the following steps:
[0018] (1) Dissolve nickel nitrate hexahydrate and sodium citrate dihydrate in ultrapure water and stir until completely dissolved to form clear Ni 2+ Precursor solution, then slowly add potassium cobalt cyanide aqueous solution to Ni 2+ In the precursor solution, stir thoroughly, let stand at room temperature, wash, centrifuge, and dry to obtain NiCo PBA precursor powder;
[0019] (2) The NiCo PBA precursor powder is uniformly adhered to the ceramic boat a, the selenium powder is placed in the ceramic boat b, the ceramic boat a is precisely inverted and covered on the ceramic boat b, so that the openings of the ceramic boat a and the ceramic boat b are aligned, and then the two are encapsulated as a whole to form a closed selenium vapor reaction chamber. After encapsulation, the whole is placed under a protective atmosphere for calcination. Through the gas-solid reaction of selenium vapor and solid precursor, a complete cubic pure phase bimetallic selenide (Ni,Co)Se2 is obtained.
[0020] According to a preferred embodiment of the present invention, in step (1), the molar ratio of nickel nitrate hexahydrate to sodium citrate dihydrate is (1-4):(4-8).
[0021] According to a preferred embodiment of the present invention, in step (1), the molar ratio of nickel nitrate hexahydrate to the volume ratio of ultrapure water is (1-4):100, unit, mmol / mL.
[0022] According to a preferred embodiment of the present invention, in step (1), the concentration of the potassium cobalt cyanide aqueous solution is 0.01-0.05 mmol / mL.
[0023] According to a preferred embodiment of the present invention, in step (1), Ni 2+ The volume ratio of the precursor solution to the potassium cobalt cyanide aqueous solution is (1-2):(1-2).
[0024] According to a preferred embodiment of the present invention, in step (1), the stirring time is 20-60 min and the standing time at room temperature is 20-30 h.
[0025] According to a preferred embodiment of the present invention, in step (1), the washing is performed by washing with ultrapure water and anhydrous ethanol respectively, and the drying is performed by drying in a vacuum drying oven at 60 °C.
[0026] According to a preferred embodiment of the present invention, in step (2), the mass ratio of NiCo PBA precursor powder to selenium powder is 1:(1-5).
[0027] According to a preferred embodiment of the present invention, in step (2), the calcination under a protective atmosphere is carried out in the following manner:
[0028] The packaged ceramic boats a and b are placed into a tube furnace. The tube furnace is evacuated and filled with inert gas 2-4 times. Then, inert gas is continuously introduced for calcination at a temperature of 400-450 °C for 1-3 hours.
[0029] According to a preferred embodiment of the present invention, the inert gas is nitrogen or argon;
[0030] According to a preferred embodiment of the present invention, during the calcination process, inert gas is continuously introduced into the tubular furnace, and the outlet of the tubular furnace is connected to the tail gas absorption liquid through a pipe. By adjusting the gas flow rate, the time interval for the tail gas to generate bubbles in the absorption liquid is controlled to be 1-3 seconds.
[0031] According to a preferred embodiment of the present invention, the calcination temperature is 400 °C and the calcination time is 2 h.
[0032] In a second aspect, the present invention provides a pure-phase bimetallic selenide prepared by the above method.
[0033] According to a preferred embodiment of the present invention, the pure phase bimetallic selenide exhibits a three-dimensional nanocube structure derived from NiCo PBA, which is assembled from small particles with an average particle size of 39.63 nm and a side length of 300-400 nm; and the material has a pure cubic crystalline phase, and its XRD shows diffraction peaks at 30.28°, 33.96°, 37.31°, 43.34°, 51.28°, 56.11°, 58.45° and 73.40°, without other impurity phase peaks.
[0034] In a third aspect, the present invention provides a modified diaphragm, the modified diaphragm comprising a base membrane and a modified material coated on the surface of the base membrane, wherein the modified material comprises the above-mentioned pure phase bimetallic selenide.
[0035] Furthermore, the modified diaphragm is prepared by:
[0036] The above-mentioned pure phase bimetallic selenide was mixed and ground with KB and PVDF at a mass ratio of 8:1:1. Then, 1-methyl-2-pyrrolidone was added to form a slurry, which was stirred until uniformly mixed. The slurry was then coated onto the base film using a doctor blade coating rod and dried in a vacuum drying oven. Finally, it was cut into discs using a slicer to obtain (Ni,Co)Se2 bimetallic selenide modified membrane.
[0037] According to a preferred embodiment of the present invention, the stirring time is 20-50 h; more preferably, the stirring time is 24 h.
[0038] According to a preferred embodiment of the invention, drying is performed in a vacuum drying oven at 50 °C for 20-50 h.
[0039] According to the present invention, the diameter of the disc is preferably 16-18 mm, and more preferably 17 mm.
[0040] According to a preferred embodiment of the present invention, the loading of (Ni,Co)Se2 bimetallic selenide in the (Ni,Co)Se2 bimetallic selenide modified membrane is 0.352 mg cm⁻¹. -2 .
[0041] Application of the above-mentioned modified separator in the preparation of lithium-sulfur batteries.
[0042] This invention employs a one-step liquid co-precipitation method to prepare a NiCo PBA precursor, followed by a reverse-encapsulated vapor-phase selenization method to synthesize a bimetallic selenide. This allows the product to fully inherit the three-dimensional cubic morphology of the precursor and form a pure phase structure with a single phase, thereby obtaining a structurally stable and homogeneous transition metal selenide.
[0043] Technical features and beneficial effects of the present invention:
[0044] 1. This invention breaks through the technical prejudice in the field that "pure phase transition metal selenides must rely on carbon frameworks or metal compound heterostructures to maintain structural stability, and pure phase Ni-Co selenides are difficult to maintain regular morphology during high-temperature selenization." Through the precise synergy of the inverted encapsulation selenization process and the 400-450 °C temperature range, a structurally complete pure phase (Ni,Co)Se2 nanocube was unexpectedly obtained without relying on any external framework, and it has high rate performance (584 mAh / g at 5.0 C).
[0045] 2. This invention innovatively uses NiCo PBA nanocubes as templates and metal sources, and successfully transforms them completely into pure-phase (Ni,Co)Se2 bimetallic selenides through inverted encapsulation vapor-phase selenization. Unlike traditional processes that require the introduction of a carbon-based framework or post-processing composites, this invention can directly obtain coating materials with excellent intrinsic conductivity and complete structure without any added conductive agents. The process is simple, low-cost, and highly reproducible, possessing significant industrialization potential.
[0046] 3. This invention achieves effective control over the phase purity and nanocrystal size of the product through precise selenization temperature regulation (400-450 °C). Unlike the technical defects of easily generating orthorhombic impurities at lower temperatures (e.g., 350 °C) or causing excessive grain growth and cubic structure collapse at excessively high temperatures (e.g., 500 °C), this invention obtains a product with a single cubic phase and uniform particle size while ensuring the complete inheritance of the precursor morphology, thus fully releasing the active sites on the material surface.
[0047] 4. This invention ingeniously integrates the advantages of multi-level structures with the synergistic effect of bimetals: the three-dimensional nanocubic structure provides a physically confined space, the nickel-cobalt bimetallic active center endows it with strong chemical adsorption capacity, and the intrinsic high conductivity of selenides ensures rapid electron transport. The synergistic effect of these three elements makes this coating material a multifunctional barrier integrating physical barrier, chemical anchoring, and efficient catalysis, fundamentally suppressing the polysulfide shuttle effect.
[0048] 5. Performance tests show that the lithium-sulfur battery assembled with the modified separator of this invention has a first-cycle discharge specific capacity as high as 1480 mAh g⁻¹ at a 0.5 C rate. -1 After 100 cycles, the capacity retention rate was 63.5% (940 mAh g). -1 ); 584 mAh g can still be obtained at a high rate of 5.0 C. -1 The specific capacity. Electrochemical impedance spectroscopy (EIS) analysis showed that the modified separator significantly reduced the charge transfer impedance (Ro) of the battery. ct The modified layer significantly reduced the interfacial impedance and electrolyte contact angle from 38.4° to 10.1°. This is attributed to the optimization of the hydrophilicity of the membrane surface by the modified layer, which promoted lithium-ion transport kinetics, thereby endowing the battery with excellent rate performance and long-cycle stability. Attached Figure Description
[0049] Figure 1 The X-ray diffraction (XRD) pattern of the NiCo PBA precursor prepared in Example 1.
[0050] Figure 2The images are scanning electron microscope (SEM) images of the NiCo PBA precursor prepared in Example 1 at different magnifications: (a) low magnification morphology, (b) high magnification morphology.
[0051] Figure 3 The X-ray diffraction (XRD) pattern of the (Ni,Co)Se2 bimetallic selenide prepared in Example 1.
[0052] Figure 4 The images are scanning electron microscope (SEM) images of the (Ni,Co)Se2 bimetallic selenide prepared in Example 1 at different magnifications: (a) low magnification morphology, (b) high magnification morphology.
[0053] Figure 5 The X-ray diffraction (XRD) pattern of the (Ni,Co)Se2 bimetallic selenide prepared in Example 2.
[0054] Figure 6 The images are scanning electron microscope (SEM) images of the (Ni,Co)Se2 bimetallic selenide prepared in Example 2 at different magnifications: (a) low magnification morphology, (b) high magnification morphology.
[0055] Figure 7 The image shows a cross-sectional SEM image of the (Ni,Co)Se2 bimetallic selenide-modified PP diaphragm prepared in Example 3.
[0056] Figure 8 The X-ray diffraction (XRD) pattern of the (Ni,Co)Se2 bimetallic selenide prepared for Comparative Example 1.
[0057] Figure 9 Scanning electron microscope (SEM) images of the (Ni,Co)Se2 bimetallic selenide prepared in Comparative Example 1 at different magnifications: (a) low magnification morphology, (b) high magnification morphology.
[0058] Figure 10 The X-ray diffraction (XRD) pattern of the (Ni,Co)Se2 bimetallic selenide prepared for Comparative Example 2.
[0059] Figure 11 Scanning electron microscope (SEM) images of the (Ni,Co)Se2 bimetallic selenide prepared for Comparative Example 2 at different magnifications: (a) low magnification morphology, (b) high magnification morphology.
[0060] Figure 12 The X-ray diffraction (XRD) pattern of the (Ni,Co)Se2 bimetallic selenide prepared for Comparative Example 3.
[0061] Figure 13The following are comparative graphs showing the electrolyte contact angle tests of the membranes prepared in Example 3 and Comparative Example 4: (a) Contact angle of Comparative Example 4, (b) Contact angle of Example 3.
[0062] Figure 14 The images show a comparison of the mechanical bending properties of the diaphragms prepared in Example 3 and Comparative Example 4.
[0063] Wherein, (a)-(d) correspond to the initial state of the membrane prepared in Example 4, namely, the first fold, the second fold, and the springback state; (e)-(h) correspond to the initial state, the first fold, the second fold, and the springback state of the membrane prepared in Example 3, respectively.
[0064] Figure 15 Cycle curves of lithium-sulfur batteries assembled with separators prepared in Example 3 and Comparative Example 4.
[0065] Figure 16 The rate performance diagram of the lithium-sulfur battery assembled with the separator prepared in Example 3.
[0066] Figure 17 The charge-discharge curves of the lithium-sulfur battery assembled with the separator prepared in Example 3 at different rates are shown.
[0067] Figure 18 Cyclic voltammetry curves of lithium-sulfur batteries assembled with separators prepared in Example 3 and Comparative Example 4.
[0068] Figure 19 Electrochemical impedance spectroscopy (EIS) diagrams of lithium-sulfur batteries assembled with separators prepared in Example 3 and Comparative Example 4.
[0069] Figure 20 The conductivity properties of the membranes prepared in Example 3 and Comparative Example 4 are shown in the graph. Detailed Implementation
[0070] The present invention will be further described below with reference to specific embodiments, but is not limited thereto.
[0071] Furthermore, unless otherwise specified, the experimental methods described in the following embodiments are all conventional methods; and unless otherwise specified, the reagents, materials and apparatus are all commercially available.
[0072] Example 1
[0073] A method for preparing (Ni,Co)Se2 bimetallic selenide, comprising the following steps:
[0074] (1) Take 3 mmol of nickel nitrate hexahydrate and 5 mmol of sodium citrate dihydrate and add them to 100 mL of ultrapure water. Stir for 30 min and after complete dissolution, obtain clear Ni. 2+Precursor solution: Add 2 mmol of potassium cobalt cyanide to 100 mL of ultrapure water, stir for 30 min until completely dissolved to obtain an aqueous solution of potassium cobalt cyanide; slowly pour the potassium cobalt cyanide aqueous solution into Ni 2+ After stirring the precursor solution for 30 min, let it stand at room temperature (25 °C) for 24 h. The resulting light blue precipitate was washed with ultrapure water and anhydrous ethanol, centrifuged, and then dried in a vacuum drying oven at 60 °C to finally obtain light blue NiCo PBA precursor powder.
[0075] The morphology and structure of the obtained light blue NiCo PBA precursor powder were characterized, and the X-ray diffraction (XRD) pattern is shown in the figure. Figure 1 The results show that the diffraction peaks of the precursor powder completely correspond to the standard card (JCPDS: 89-3738) of Ni3[Co(CN)6]2·12H2O, and no impurity peaks were observed, indicating that the pure-phase NiCo PBA precursor has been successfully prepared. Scanning electron microscope (SEM) images are shown below. Figure 2 The results show that the precursor is a uniformly sized three-dimensional nanocube with a side length of approximately 400 nm and a smooth surface.
[0076] (2) Take 70 mg of the NiCo PBA precursor powder prepared in step (1) and adhere it to a ceramic boat a; separately weigh 140 mg of selenium powder and put it into a ceramic boat b; precisely invert the ceramic boat a and cover the ceramic boat b, aligning the openings of the ceramic boat a and ceramic boat b, and then use tin foil to seal and fix the ceramic boat a and ceramic boat b as a whole to form a sealed selenium vapor reaction chamber, and then transfer it to the constant temperature zone of the tube furnace, and perform three vacuuming-nitrogen circulation cycles on the tube furnace to completely remove the internal air; then continuously introduce nitrogen as a protective gas, connect the exhaust gas absorbent to the exhaust gas outlet of the tube furnace, and adjust the nitrogen flow rate to control the bubble generation rate in the exhaust gas absorbent to 1-3 per second. Set the tube furnace to 2 °C min -1 The temperature was increased to 400 °C at a rising rate and held at that temperature for 2 h. After the reaction was completed, the furnace was cooled to room temperature, and the porcelain boat was removed to obtain a black powder, which is (Ni,Co)Se2 bimetallic selenide.
[0077] Phase and morphology analysis of (Ni,Co)Se2 bimetallic selenide was performed. Its X-ray diffraction (XRD) pattern is shown below. Figure 3As shown, the diffraction peaks appearing at 30.28°, 33.96°, 37.31°, 43.34°, 51.28°, 56.11°, 58.45° and 73.40° are located between the (200), (210), (211), (220), (311), (023), (321) and (421) crystal planes of the standard card of cubic NiSe2 (JCPDS: 88-1711) and the standard card of cubic CoSe2 (JCPDS: 89-2002), and no impurity phase peaks were detected, indicating that the obtained sample is a (Ni,Co)Se2 bimetallic selenide, indicating that the present invention successfully prepared a pure phase (Ni,Co)Se2 bimetallic selenide.
[0078] Figure 4 This is a scanning electron microscope (SEM) image of the (Ni,Co)Se2 bimetallic selenide sample prepared in Example 1. It can be seen that the selenized product inherits the three-dimensional cubic morphology of the precursor well, without structural collapse. However, the overall structure is transformed into nanocubes composed of small particles with an average particle size of 39.63 nm. The nanocubes are uniform in size, with a side length still approximately 400 nm.
[0079] Example 2
[0080] The preparation method of (Ni,Co)Se2 bimetallic selenide described in Example 1 differs from that in that:
[0081] In step (1), 4 mmol of nickel nitrate hexahydrate and 6 mmol of sodium citrate dihydrate were added to 200 mL of ultrapure water and completely dissolved to obtain clear Ni. 2+ Precursor solution; add 10 mmol of potassium cobalt cyanide to 200 mL of ultrapure water, and after complete dissolution, obtain an aqueous solution of potassium cobalt cyanide; slowly pour the potassium cobalt cyanide aqueous solution into Ni 2+ After stirring thoroughly in the precursor solution for 40 min, let it stand at room temperature (25 °C) for 30 h.
[0082] In step (2), 150 mg of the NiCo PBA precursor powder prepared in step (1) is taken and adhered to a ceramic boat a; 450 mg of selenium powder is weighed and loaded into a ceramic boat b; a tube furnace is set up and heated to 2 °C for min. -1 The temperature was increased to 450 °C at a certain rate and held at that temperature for 3 h.
[0083] Other steps and conditions are performed as in Example 1.
[0084] The X-ray diffraction (XRD) pattern of the (Ni,Co)Se2 bimetallic selenide prepared in this embodiment is shown in [reference needed]. Figure 5 . Figure 5The peak positions are similar to those in Example 1. The diffraction peaks of the sample are all located between the (200), (210), (211), (220), (311), (023), (321) and (421) crystal planes in the standard card of cubic NiSe2 (JCPDS: 88-1711) and the standard card of cubic CoSe2 (JCPDS: 89-2002), and no impurity phase peaks were detected.
[0085] The scanning electron microscope (SEM) image of the (Ni,Co)Se2 bimetallic selenide prepared in this embodiment is shown below. Figure 6 , Figure 6 The results show that the selenized product as a whole inherits the three-dimensional nanocubic morphology of the precursor.
[0086] Example 3
[0087] A method for modifying PP separators with (Ni,Co)Se2 bimetallic selenide, comprising the following steps:
[0088] The nickel cobalt selenide Prussian blue derivative, KB, and PVDF prepared in Example 1 were weighed in a mass ratio of 8:1:1. The three components were ground in an agate mortar until no obvious particles remained. Then, 1-methyl-2-pyrrolidone was added and mixed to form a slurry, which was stirred until uniformly mixed. The slurry was then coated onto a PP membrane using a 250 μm thick doctor blade and dried in a vacuum oven at 50 °C for 24 h. The membrane was then sliced into 17 mm discs using a slicer, ultimately obtaining the (Ni,Co)Se2 bimetallic selenide modified PP membrane.
[0089] The modified PP membrane prepared in this embodiment has a (Ni,Co)Se2 bimetallic selenide loading of 0.352 mg / cm³. -2 .
[0090] SEM images of the modified PP diaphragm cross section are shown below. Figure 7 ,from Figure 7 It can be found that the coating thickness of the modified PP diaphragm is approximately 5.8 μm.
[0091] Comparative Example 1
[0092] The preparation method of (Ni,Co)Se2 bimetallic selenide described in Example 1 differs from that in that:
[0093] In step (2), the tube furnace is set to 2 °C min. -1 The temperature was increased to 350 °C at a certain rate and held at that temperature for 3 h.
[0094] Other steps and conditions are performed as in Example 1.
[0095] The X-ray diffraction (XRD) pattern of the (Ni,Co)Se2 bimetallic selenide prepared in this comparative example is shown below. Figure 8 . Figure 8 The results show that the overall peak positions of the selenized sample obtained at 350 °C are located between the standard card of cubic NiSe2 (JCPDS: 88-1711) and the standard card of cubic CoSe2 (JCPDS: 89-2002). However, impurity peaks appeared at 28.8°, 35.4°, and 47.4°, with peak positions located between the (011), (120), and (211) crystal planes of the standard card of orthorhombic NiSe2 (JCPDS: 18-0886) and the standard card of orthorhombic CoSe2 (JCPDS: 53-0449). This indicates that at this relatively low selenization temperature, a certain proportion of orthorhombic diselenide was generated in the product, forming a mixture of cubic and orthorhombic phases. At the same time, the particle size of the selenized nanocubes obtained at this calcination temperature is smaller than that of Examples 1 and 2 ( Figure 9 The particle size is 20.14 nm.
[0096] Comparative Example 2
[0097] The preparation method of (Ni,Co)Se2 bimetallic selenide described in Example 1 differs from that in that:
[0098] In step (2), the tube furnace is set to 2 °C min. -1 The temperature was increased to 500 °C at a certain rate and held at that temperature for 3 hours.
[0099] Other steps and conditions are performed as in Example 1.
[0100] The X-ray diffraction (XRD) pattern of the (Ni,Co)Se2 bimetallic selenide prepared in this comparative example is shown below. Figure 10 . Figure 10 The peak positions were similar to those in Example 1, with the diffraction peaks of the sample all located between the standard cards for cubic NiSe2 (JCPDS: 88-1711) and cubic CoSe2 (JCPDS: 89-2002), and no impurity peaks were detected. However, the corresponding scanning electron microscope (SEM) images ( Figure 11 The study revealed significant morphological differences. At this temperature, selenization resulted in nanocube particles with significantly larger sizes than those in Examples 1 and 2, with an average particle size of 120.10 nm. This excessive particle growth prevented the product from maintaining the regular cubic framework of the precursor, leading to significant deformation of the overall morphology.
[0101] Comparative Example 3
[0102] The preparation method of (Ni,Co)Se2 bimetallic selenide is the same as that described in Example 1, except that this method does not use inverted encapsulation-type vapor-phase selenization. Specifically:
[0103] In step (2), 70 mg of the NiCo PBA precursor powder prepared in step (1) is taken and spread evenly in ceramic boat a; 350 mg of selenium powder is separately weighed and spread evenly in ceramic boat b. Ceramic boat a is placed downstream of the tube furnace, and ceramic boat b is placed upstream of the tube furnace; the tube furnace is set to 2°C min. -1 The temperature was increased to 400 °C at a heating rate and held at that temperature for 2 hours.
[0104] Other steps and conditions are performed as in Example 1.
[0105] The X-ray diffraction (XRD) pattern of the (Ni,Co)Se2 bimetallic selenide prepared in this comparative example is shown below. Figure 12 . Figure 12 The results show that the positions of the main diffraction peaks are basically consistent with those of Example 1, with most diffraction peaks falling between the standard peak positions of cubic NiSe2 (JCPDS: 88-1711) and cubic CoSe2 (JCPDS: 89-2002). However, characteristic peaks of the (200), (220), and (400) crystal planes belonging to the precursor Ni3[Co(CN)6]2·12H2O (JCPDS: 89-3738) were also detected at 17.47°, 24.81°, and 35.37°, indicating that the reverse-encapsulated vapor-phase selenization was not used, the precursor was not completely converted into the target selenide, and there is a certain degree of residue.
[0106] Comparative Example 4
[0107] Commercial PP membranes were cut into 17 mm diameter discs using a slicer to serve as blank control membranes. These membranes were uncoated and free of (Ni,Co)Se2 bimetallic selenide.
[0108] The electrolyte for the membranes prepared in Example 3 and Comparative Example 4 (electrolyte was 1.0 mol L) -1 Contact angle test results for a LiTFSI DOL / DME mixed solution (volume ratio 1:1, with 1 wt% LiNO3 added as an additive) are shown below. Figure 13 The wetting performance of the modified layer on the electrolyte was investigated by contact angle testing. The results showed that the membrane with (Ni,Co)Se2 as the coating material had a contact angle of 10.1°, which was significantly lower than the 38.4° of the blank PP membrane, indicating that the modified membrane had significantly improved interfacial wettability. Figure 14The figures show the mechanical bending properties of the diaphragms prepared in Example 3 and Comparative Example 4. As shown, after undergoing continuous bending and other mechanical deformations, the modified diaphragm of Example 3 maintained its coating structure intact, without cracking or delamination, fully demonstrating its excellent deformation resistance and stable interfacial bonding strength.
[0109] Experimental Example 1
[0110] To verify the effectiveness of the present invention, a series of performance tests were conducted on the separators prepared in Example 3 and Comparative Example 4 and the lithium-sulfur batteries assembled therefrom.
[0111] The preparation process of the positive electrode for lithium-sulfur batteries is as follows:
[0112] (1) Weigh sublimed sulfur and carbon nanotubes at a mass ratio of 7:3, and then grind and mix them thoroughly in an agate mortar.
[0113] (2) Transfer the above mixture into a glass bottle and perform three vacuum-argon filling cycles in an argon glove box to completely remove the internal air.
[0114] (3) The sealed glass bottle was placed in a drying oven and heat-treated at 155 °C for 12 h to obtain sulfur / carbon nanotube composite (CNT / S).
[0115] (4) Weigh CNT / S, KB and PVDF in a mass ratio of 8:1:1, grind them evenly in an agate mortar, add an appropriate amount of 1-methyl-2-pyrrolidone to make a slurry, and stir continuously for 24 hours to make it evenly mixed.
[0116] (5) Use a scraper to coat the slurry evenly onto the carbon-coated aluminum foil. After drying in a vacuum drying oven at 60 °C for 24 hours, use a slicer to cut it into round pieces with a diameter of 12 mm to obtain the positive electrode sheet. Weigh and record its mass.
[0117] Lithium-sulfur battery assembly process:
[0118] In an argon-filled glove box, a CR2032 button battery casing was used, with lithium foil as the negative electrode, and the modified separator of Example 3 or the blank PP separator of Comparative Example 4 was used as the separator. The electrolyte was 1.0 mol / L. -1 A mixed solution of LiTFSI and DOL / DME (volume ratio 1:1) was prepared, with 1 wt% LiNO3 added as an additive. After assembly, the batteries were stamped and sealed using a battery packaging machine. After static activation for 6 hours, electrochemical performance tests were performed.
[0119] Electrochemical performance testing of lithium-sulfur batteries:
[0120] The cycle performance and rate performance of the batteries were tested at different rates using the LAND battery testing system (electrochemical window of 1.7-2.8 V).
[0121] The CV curves were obtained using a CHI760E electrochemical workstation within a voltage range of 1.7–2.8 V.
[0122] EIS testing was conducted on the CHI760E at frequencies ranging from 0.01 Hz to 100 kHz.
[0123] Figure 15 The lithium-sulfur batteries assembled with the separators prepared for Example 3 and Comparative Example 4 exhibit cycle charge-discharge performance at a 0.5 C rate. Figure 15 It can be seen that the highest discharge specific capacity of the comparative battery using the blank PP separator is only 820 mAh g. -1 After 100 cycles, it rapidly decreased to 440 mAh g. -1 The synergistic catalytic effect of pure-phase nickel-cobalt bimetals and the high intrinsic conductivity of selenides greatly accelerated the reaction kinetics, effectively suppressing the shuttle effect. The lithium-sulfur battery assembled with a (Ni,Co)Se2 bimetallic selenide-modified PP separator achieved a maximum discharge specific capacity of 1480 mAh g⁻¹ at a rate of 0.5 C. -1 After 100 cycles, the discharge specific capacity remained at 940 mAh g. -1 .
[0124] Figure 16 The graph shows the rate performance of the lithium-sulfur battery assembled with the separator prepared in Example 3. The average specific capacities of this battery at 0.05 C, 0.1 C, 0.2 C, 0.5 C, 1.0 C, 2.0 C, and 5.0 C are 1620, 1359, 1270, 1108, 1011, 824, and 584 mAh g, respectively. -1 When the current returns to 0.1 C, the battery capacity recovers to 1205 mAh g. -1 This is equivalent to 88.7% of the original value, indicating that the battery has excellent cycle stability.
[0125] Figure 17 The charge-discharge curves of the lithium-sulfur battery assembled with the separator prepared in Example 3 at different rates, and the current density and Figure 16 Correspondingly, it exhibits a corresponding charge-discharge plateau at different rates.
[0126] Figure 18The CV test curves are for lithium-sulfur batteries assembled with the separators prepared in Example 3 and Comparative Example 4. Compared to the control battery using a blank PP separator, the lithium-sulfur battery assembled with the (Ni,Co)Se2 bimetallic selenide modified PP separator exhibits a stronger redox peak current, a larger peak area, and a smaller peak spacing. This indicates that the lithium-sulfur battery assembled with the (Ni,Co)Se2 bimetallic selenide modified PP separator shows significantly enhanced polysulfide conversion kinetics and significantly reduced battery polarization.
[0127] Figure 19 Impedance plots of lithium-sulfur batteries assembled with the separators prepared in Example 3 and Comparative Example 4 are shown. It can be observed that the semicircle diameter of the lithium-sulfur battery assembled with the (Ni,Co)Se2 bimetallic selenide-modified PP separator is significantly smaller in the high-frequency region than that of the comparative example. This indicates that under the action of the modified separator of this invention, the charge transport resistance at the battery interface is greatly reduced, and the conduction of ions and electrons is smoother. Furthermore, the smaller charge transfer impedance implies a lower energy barrier in the polysulfide redox reaction process, resulting in a significant improvement in electrode reaction kinetics. This is entirely consistent with the results observed in CV testing: a higher peak current and a smaller peak spacing.
[0128] Figure 20 This is a comparison chart of the ionic conductivity of the membranes prepared in Example 3 and Comparative Example 4. The conductivity values are based on... Figure 19 The AC impedance spectrum is used to read the charge transfer resistance (R). ct After that, the result is calculated according to the following formula:
[0129]
[0130] Where L is the diaphragm thickness (cm), R ct S is the charge transfer resistance (Ω), and S is the effective area of the diaphragm (cm²). 2 It is evident that the modified PP membrane exhibits significantly higher conductivity than the blank PP membrane, indicating that its interfacial ion transport capability is superior to that of the blank PP membrane.
[0131] The above data corroborate each other, collectively and powerfully demonstrating that the (Ni,Co)Se2 bimetallic selenide-modified PP separator not only inhibits polysulfide shuttle but also improves the electrochemical performance of lithium-sulfur batteries by enhancing reaction kinetics and reducing interfacial impedance, thus verifying the practical value of this invention.
Claims
1. A modified diaphragm, characterized in that, The modified membrane includes a base membrane and a modifying material coated on the surface of the base membrane. The modifying material contains a pure-phase bimetallic selenide, which exhibits a three-dimensional nanocubic structure derived from NiCo PBA. This cubic structure is assembled from particles with an average particle size of 39.63 nm and a side length of 300-400 nm. The material has a pure cubic crystalline phase, and its XRD shows diffraction peaks at 30.28°, 33.96°, 37.31°, 43.34°, 51.28°, 56.11°, 58.45°, and 73.40°, with no other impurity phase peaks. The preparation method employs an inverted encapsulation-type vapor phase selenization process, comprising the following steps: (1) Dissolve nickel nitrate hexahydrate and sodium citrate dihydrate in ultrapure water and stir until completely dissolved to form clear Ni 2+ Precursor solution, then slowly add potassium cobalt cyanide aqueous solution to Ni 2+ In the precursor solution, stir thoroughly, let stand at room temperature, wash, centrifuge, and dry to obtain NiCo PBA precursor powder; (2) The NiCo PBA precursor powder is uniformly adhered to a ceramic boat a, and the selenium powder is placed in a ceramic boat b. The mass ratio of NiCo PBA precursor powder to selenium powder is 1:1-5. The ceramic boat a is precisely inverted and placed on top of the ceramic boat b, so that the openings of the ceramic boat a and ceramic boat b are aligned. Then, the two are sealed together to form a closed selenium vapor reaction chamber. The sealed ceramic boat a and ceramic boat b are placed into a tube furnace. The tube furnace is evacuated and filled with inert gas 2-4 times. Then, inert gas is continuously introduced for calcination. The calcination temperature is 400-450 °C and the calcination time is 1-3 hours. h, through the gas-solid reaction of selenium vapor with the solid precursor, a pure phase bimetallic selenide (Ni,Co)Se2 with a complete cubic morphology is obtained; the inert gas is nitrogen or argon, and during the calcination process, the inert gas is continuously introduced into the tube furnace, and the outlet of the tube furnace is connected to the tail gas absorption liquid through a pipe. By adjusting the gas flow rate, the time interval for the tail gas to generate bubbles in the absorption liquid is controlled to be 1-3 s.
2. The modified diaphragm according to claim 1, characterized in that, In step (1), the molar ratio of nickel nitrate hexahydrate to sodium citrate dihydrate is (1-4):(4-8), the molar amount of nickel nitrate hexahydrate to the volume ratio of ultrapure water is (1-4):100, the unit is mmol / mL, and the concentration of potassium cobalt cyanide aqueous solution is 0.01-0.05 mmol / mL.
3. The modified diaphragm according to claim 1, characterized in that, In step (1), Ni 2+ The volume ratio of the precursor solution to the potassium cobalt cyanide aqueous solution is (1-2): (1-2). The stirring time is 20-60 min, and the standing time at room temperature is 20-30 h. The washing is done with ultrapure water and anhydrous ethanol respectively, and the drying is done in a vacuum drying oven at 60 °C.
4. The method for preparing the modified diaphragm according to claim 1, characterized in that, Pure phase bimetallic selenide was mixed and ground with KB and PVDF at a mass ratio of 8:1:
1. Then, 1-methyl-2-pyrrolidone was added to form a slurry, which was stirred until uniformly mixed. The slurry was then coated onto the base film using a doctor blade coating rod and dried in a vacuum drying oven. Finally, it was cut into discs using a slicer to obtain (Ni,Co)Se2 bimetallic selenide modified membrane.
5. The application of the modified separator according to claim 1 in the preparation of lithium-sulfur batteries.
Citation Information
Patent Citations
Bimetal phosphide inlaid carbon hollow nanocage as well as preparation method and application thereof
CN113066964A
Preparation method of multifunctional diaphragm coating for lithium-sulfur battery
CN113422155A
Dual-rare earth metal catalytic nano material, diaphragm and preparation method and application of dual-rare earth metal catalytic nano material
CN120515472A
Functional coating modified diaphragm as well as preparation method and application thereof
CN120261916A