A method for preparing optical quartz materials

By optimizing the cooling rate and mold design in the hot forming process, the stress problem caused by the difference in the mold expansion coefficient during the hot forming of quartz material was solved, realizing the preparation of low-stress optical quartz material, simplifying the production process and improving material performance.

CN122725565BActive Publication Date: 2026-11-17CHANGFEI QUARTZ TECH (WUHAN) CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611207895.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-11
Publication Date
2026-11-17
Estimated Expiration
2046-08-11

AI Technical Summary

Technical Problem

Stress problems caused by the difference in thermal expansion coefficients of molds during the hot forming process of quartz materials affect the material properties and require additional annealing to eliminate thermal stress. Furthermore, rapid cooling causes temperature gradients that generate thermal stress.

Method used

The cooling rate and mold design of the hot forming process were optimized. By controlling the cooling rate in multiple stages and combining the annealing point and strain point temperature of the material, the quartz material was separated from the sidewall of the graphite mold, avoiding the generation of new stress. An isostatic graphite mold was also used to reduce stress.

Benefits of technology

It achieves complete elimination of thermal stress during the hot forming process, and low-stress optical quartz materials can be obtained without additional annealing, thus improving production efficiency and material properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122725565B_ABST
    Figure CN122725565B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing optical quartz materials. The quartz material is placed in a graphite mold and heated to 1700-1750℃ at a rate of 10℃ / h, then held at that temperature for 3-10h. The temperature is then lowered to 1250-1350℃ at a rate of 8-12℃ / h, followed by lowering the graphite base plate to detach the hardened quartz material from the graphite side plates. The temperature is then lowered to 1240-1280℃ at a rate of 4-6℃ / h and held for a period of time. Finally, the temperature is lowered to 9℃ / h. The material is held at 80-1020℃ for heat treatment; then cooled to 480-520℃ at a rate of 4-6℃ / h before being de-energized and cooled with the furnace. This invention optimizes the cooling rate after hot forming, combining the annealing point and strain point temperature of the material, and controls the cooling rate in multiple stages to completely eliminate the thermal stress of hot forming, achieving the required temperature without additional annealing. During the cooling process, the hardened quartz material is separated from the sidewall of the graphite mold, preventing the graphite mold from compressing the quartz material and generating new stress.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of inorganic non-metallic materials technology, specifically relating to a method for preparing optical quartz materials. Background Technology

[0002] In the field of quartz glass, quartz is an extremely viscous material. Even when heated above its softening point, its viscosity remains high. Furthermore, quartz requires high purity, is bubble-free, and exhibits low-stress birefringence, making it difficult to mold or form using defoaming agents. Therefore, hot forming of quartz typically involves heating the material above its softening point, allowing it to spread outwards under its own weight until it completely fills the mold. Due to the specific requirements of quartz, high-purity graphite is generally used as the forming mold. Throughout the hot forming process, to prevent leakage of quartz, the graphite mold must be fitted together tightly until it is completely cooled before demolding and removing the material.

[0003] Although graphite molds can effectively prevent quartz material leakage, during the cooling process, the coefficient of thermal expansion of graphite is much greater than that of quartz material. This results in the graphite mold shrinking more during cooling than the quartz material, causing the quartz material to be "pinched out" under great stress, and even causing chipping at the edges of the quartz material, which greatly affects the performance of the quartz material.

[0004] To improve production efficiency, quartz materials are cooled rapidly during the hot forming process. This results in a large temperature gradient in the hot-formed quartz material, generating thermal stress. This thermal stress can persist inside the quartz material for a long time and needs to be eliminated through subsequent precision annealing processes. Summary of the Invention

[0005] The purpose of this invention is to provide a method for preparing low-stress optical quartz materials. By optimizing the cooling rate after thermal shaping, the thermal stress of thermal shaping can be completely eliminated. At the same time, a new graphite mold is used to avoid the mold extruding the quartz material and generating new stress.

[0006] To achieve the above objectives, the following technical solution is adopted: A method for preparing an optical quartz material includes the following steps: (1) The quartz material obtained by VAD deposition is placed in a graphite mold and heated to above the softening point for heat preservation treatment; the graphite mold consists of a graphite base plate and graphite side plates that match the shape of the graphite base plate and can be separated. (2) Cool down to 1250-1350℃ at a rate of 8-12℃ / h, then lower the graphite base plate, and the hardened quartz material separates from the graphite side plate; (3) Cool down to 1240-1280℃ at a rate of 4-6℃ / h and keep warm; then cool down to 980-1020℃ at a rate of 1-3℃ / h and keep warm for 30-150h; finally cool down to 480-520℃ at a rate of 4-6℃ / h and then turn off the power and cool with the furnace.

[0007] According to the above scheme, the hydroxyl content of the quartz material is less than 100 ppm.

[0008] According to the above scheme, the graphite mold material is isostatic graphite with an ash content of less than 50ppm; the graphite base plate is a circular graphite base plate or a square graphite base plate.

[0009] According to the above scheme, in step (1), the quartz material is heated to 1700-1750℃ at a heating rate of 10-20℃ / h and kept at that temperature for 3-10h, while being filled with 120000~200000Pa of inert gas.

[0010] In the optimized scheme, the temperature is reduced to 1280-1320℃ at a rate of 9-11℃ / h in step (2). In the even more optimized scheme, the temperature is reduced to 1300℃ at a rate of 10℃ / h in step (2).

[0011] In the optimized scheme, in step (3), the temperature is reduced to 1250-1270℃ at a rate of 4.5-5.5℃ / h and held for more than 100h; then the temperature is reduced to 990-1010℃ at a rate of 1.5-2.5℃ / h and held for more than 50h; finally, the temperature is reduced to 490-510℃ at a rate of 4.5-5.5℃ / h and then the power is cut off and the furnace is cooled. In a more optimized scheme, in step (3), the temperature is reduced to 1260℃ at a rate of 5℃ / h, then held for 100h, then reduced to 1000℃ at a rate of 2℃ / h, then held for 50h, and finally reduced to 500℃ at a rate of 5℃ / h and then the power is cut off and the furnace is cooled.

[0012] According to the above scheme, the graphite mold can also be replaced with a mold made of ceramic or gypsum material.

[0013] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention optimizes the cooling rate after hot forming, and controls the cooling rate in multiple stages by combining the annealing point and strain point temperature of the material, so that the thermal stress of hot forming can be completely eliminated, and the requirements can be met without additional annealing.

[0014] During the cooling process, at a temperature slightly above the annealing point, the mold design is optimized to separate the hardened quartz material from the sidewall of the graphite mold, thus preventing the graphite mold from compressing the quartz material and generating new stress. Attached Figure Description

[0015] Figure 1: Schematic diagram of the preparation method of the optical quartz material of the present invention.

[0016] Figure 2 Example 1: Stress condition of quartz material after thermal shaping.

[0017] Figure 3 Comparative Example 1: Stress condition of quartz material after thermal shaping.

[0018] Figure 4 Example 2: Stress condition of quartz material after thermal shaping.

[0019] Figure 5 Example 3: Stress condition of quartz material after thermal shaping.

[0020] Figure 6 Example 4: Stress condition of quartz material after thermal shaping.

[0021] Among them, 1-quartz material; 2-graphite base plate; 3-graphite side plate. Detailed Implementation

[0022] The following embodiments further illustrate the technical solution of the present invention, but are not intended to limit the scope of protection of the present invention.

[0023] A specific embodiment provides a method for preparing optical quartz materials, as shown in the appendix. Figure 1 As shown: (1) Quartz material 1 is placed in a graphite mold and heated to above its softening point for heat preservation treatment; the graphite mold consists of a graphite base plate 2 and graphite side plates 3 that match the shape of the graphite base plate and can be separated; the quartz material is synthetic quartz, natural quartz, or quartz sand particles; the hydroxyl content is less than 100 ppm, preferably less than 50 ppm, more preferably less than 30 ppm, and extremely preferably less than 15 ppm. The graphite mold material is isostatic graphite with an ash content of less than 50 ppm, preferably less than 20 ppm.

[0024] (2) Cool down to 1250-1350℃ at a rate of 8-12℃ / h, then lower the graphite base plate 2, and the hardened quartz material 1 separates from the graphite side plate 3.

[0025] (3) Cool down to 1240-1280℃ at a rate of 4-6℃ / h and keep warm; then cool down to 980-1020℃ at a rate of 1-3℃ / h and keep warm; finally cool down to 480-520℃ at a rate of 4-6℃ / h and then turn off the power to cool down with the furnace.

[0026] Example 1 A quartz blank (a section of a transparent glass rod obtained by VAD deposition, with a diameter of 250 mm and a height of 400 mm and a hydroxyl content of 15 ppm) with a diameter of 250 mm and a height of 400 mm was cleaned. The quartz blank to be heat-shaped was then placed in a square graphite mold (internal cavity size L500 mm). W500mm H200mm, material isostatic graphite, ash content less than 20ppm, mold is assembled from all graphite material, with an expansion margin of 10-20mm after assembly. The quartz material is heated to its softening point of 1700℃ (while being filled with 200000Pa high-purity argon gas), held for 3 hours, and then cooled to 1300℃ at a rate of 10℃ / h. The platform is then lowered to separate the graphite mold base plate and the hardened quartz material from the surrounding graphite mold side plates. The temperature is then lowered to 1260℃ at a rate of 5℃ / h, held for 100 hours, then lowered to 1000℃ at a rate of 2℃ / h, held for 50 hours, and finally cooled to 500℃ at a rate of 5℃ / h before power is cut off and the furnace is cooled. After being removed from the furnace, the surface is machined to achieve a surface quality suitable for testing stress birefringence.

[0027] The stress condition of the quartz material after heat shaping in this embodiment is shown in the appendix. Figure 2 As shown. The blank size after hot forming is L500mm. W500mm H75mm, test aperture L470mm W470mm, with... Figure 2 This is a stress birefringence distribution map for this aperture. The bluer the color, the closer the stress birefringence value is to 0 nm / cm. The closer it is to red, the closer the stress birefringence value is to ≥5 nm / cm. The map shows that most areas are blue, with a lighter blue tint on the left and right sides. L470mm The maximum stress birefringence within the W470mm region is 0.85nm / cm. Compared with the quartz workpieces prepared by the traditional structure, the present invention does not require additional annealing to eliminate thermal stress during the hot forming process, saving a lot of time and energy, and the edge impurity concentration is <20ppb.

[0028] Comparative Example 1 Repeat the operation of Example 1, but omit the operation of separating the graphite mold base plate and the hardened quartz material from the surrounding graphite mold side plates.

[0029] The stress condition of the quartz material in this comparative example after heat forming is shown in the appendix. Figure 3 As shown. The blank size after hot forming is L500mm. W500mm H75mm, test aperture L470mm W470mm, with... Figure 2This is a stress birefringence distribution map for this aperture. The bluer the color, the closer the stress birefringence value is to 0 nm / cm. The closer it is to red, the closer the stress birefringence value is to ≥5 nm / cm. The map shows a small area appearing blue, especially the left side which appears red, and the center which appears green. (L470mm) The maximum stress birefringence in the W470mm region is 5.68 nm / cm. This is due to the partial thermal stress generated by the temperature gradient during the cooling process and the excessive shrinkage of graphite relative to quartz during the cooling process, which causes the quartz workpiece to be clamped out of stress, and the edge impurity concentration is <50ppb.

[0030] Example 2 A quartz blank (a section of a transparent glass rod obtained by VAD deposition, with a diameter of 250mm and a height of 400mm, and a hydroxyl content of 80ppm) with a diameter of 250mm and a height of 400mm was cleaned. The quartz blank to be heat-shaped was then placed in a square graphite mold (internal cavity size L500mm). W500mm The blank is made of H200mm isostatically pressed graphite with an ash content of less than 20ppm. The mold is assembled entirely of graphite material, with an expansion allowance of 10-20mm after assembly. The mold is moved into a heating furnace and heated to 1720℃ at a rate of 10℃ / h (while simultaneously filling with 200,000Pa high-purity argon gas), and held for 3 hours. It is then cooled to 1250℃ at a rate of 8℃ / h (after the quartz has hardened). The platform (graphite base plate) is lowered to completely detach the quartz blank from the surrounding side plates. The temperature is further reduced to 1240℃ at a rate of 4℃ / h and held for 60 hours. Then, it is cooled to 980℃ at a rate of 1℃ / h and held for 30 hours. Finally, it is cooled to 480℃ at a rate of 4℃ / h, and the furnace is cooled with the power off. After removal from the furnace, the surface is machined to achieve a surface quality suitable for testing stress birefringence.

[0031] The stress condition of the quartz material after heat shaping in this embodiment is shown in the appendix. Figure 4 As shown. The blank size after hot forming is L500mm. W500mm H75mm, test aperture L470mm With a diameter of 470mm, the maximum stress birefringence within this region is 0.95nm / cm, and the distribution is uniform. The edge impurity concentration is <15 ppb. This method also eliminates the need for additional annealing, directly yielding low-stress optical quartz plates, thus verifying the stability of the process with smaller blank sizes.

[0032] Example 3 A quartz blank (a section of a transparent glass rod obtained by VAD deposition, with a diameter of 250 mm and a height of 400 mm and a hydroxyl content of 100 ppm) with a diameter of 250 mm and a height of 400 mm was cleaned. The quartz blank to be heat-shaped was then placed in a square graphite mold (internal cavity size L500 mm). W500mm The quartz blank (H200mm, isostatically pressed graphite, ash content less than 20ppm, mold assembled entirely of graphite material, with an expansion allowance of 10-20mm after assembly) is placed in a heating furnace and heated to 1750℃ at an appropriate rate (while simultaneously charging with 200,000Pa high-purity argon gas), and held for 5 hours. It is then cooled to 1350℃ at a rate of 12℃ / h until fully hardened. The platform is lowered to detach the quartz blank from the side plates. The blank is then cooled to 1280℃ at a rate of 6℃ / h and held for 120 hours. It is then cooled to 1020℃ at a rate of 3℃ / h and held for 80 hours. Finally, it is cooled to 520℃ at a rate of 6℃ / h, and cooled with the furnace after power is cut off. The blank is then removed from the furnace and the surface is machined to meet testing requirements.

[0033] The stress condition of the quartz material after heat shaping in this embodiment is shown in the appendix. Figure 5 As shown. The blank size after hot forming is L500mm. W500mm H75mm, test aperture L470mm With a diameter of 470mm, the maximum stress birefringence in this region is 0.75nm / cm. The light blue area dominates, and no red high-stress area is observed. The edge impurity concentration is <18 ppb. This example demonstrates that, under large-size blank conditions, by extending the holding time and controlling the cooling rate, low-stress quartz material meeting optical requirements can still be obtained without secondary annealing.

[0034] Example 4 A quartz blank (a section of a transparent glass rod obtained by VAD deposition, with a diameter of 250 mm and a height of 400 mm and a hydroxyl content of 30 ppm) with a diameter of 250 mm and a height of 400 mm was cleaned. The quartz blank to be heat-shaped was then placed in a square graphite mold (internal cavity size L500 mm). W500mm H200mm, material isostatically pressed graphite, ash content less than 20ppm, mold assembled entirely of graphite material (with 10~20mm expansion margin after assembly). High-purity argon gas at 120000Pa is introduced while heating to 1710℃, held for 3.5 h. Cooling is then carried out at a rate of 10℃ / h to 1280℃ for quartz hardening. The platform is lowered to separate the base plate, billet, and side plates. Cooling is then carried out at a rate of 5℃ / h to 1250℃, held for 80 h. Cooling is then carried out at a rate of 2℃ / h to 990℃, held for 40 h. Finally, cooling is carried out at a rate of 5℃ / h to 490℃, and the furnace is cooled with the power off.

[0035] The stress condition of the quartz material after heat shaping in this embodiment is shown in the appendix. Figure 6 As shown. The blank size after hot forming is L500mm. W500mm H75mm, test aperture L470mm Within a W470mm region, the maximum stress birefringence is 0.88 nm / cm, exhibiting extremely uniform distribution. Edge impurity concentration is <12 ppb. This example demonstrates the feasibility of using low-hydroxyl raw materials in a slightly positive-pressure argon atmosphere, broadening the applicability to various gas environments and raw material specifications while maintaining excellent optical uniformity.

Claims

1. A method for preparing an optical quartz material, characterized in that... Includes the following steps: (1) The quartz material obtained by VAD deposition is placed in a graphite mold and heated to 1700-1750℃ at a heating rate of 10-20℃ / h, and held at that temperature for 3-10h, while being filled with 120000~200000Pa of inert gas; the graphite mold consists of a graphite base plate and graphite side plates that match the shape of the graphite base plate and can be separated; the hydroxyl content of the quartz material is less than 100ppm; (2) Cool down to 1250-1350℃ at a rate of 8-12℃ / h, then lower the graphite base plate, and the hardened quartz material separates from the graphite side plate; (3) Cool down to 1240-1280℃ at a rate of 4-6℃ / h and keep warm; then cool down to 980-1020℃ at a rate of 1-3℃ / h and keep warm for 30-150h; finally cool down to 480-520℃ at a rate of 4-6℃ / h and then turn off the power and cool with the furnace.

2. The method for preparing the optical quartz material as described in claim 1, characterized in that... The graphite mold is made of isostatically pressed graphite with an ash content of less than 50 ppm.

3. The method for preparing the optical quartz material as described in claim 1, characterized in that... The graphite base plate can be a circular graphite base plate or a square graphite base plate.

4. The method for preparing the optical quartz material as described in claim 1, characterized in that... In step (2), the temperature is reduced to 1280-1320℃ at a rate of 9-11℃ / h.

5. The method for preparing the optical quartz material as described in claim 1, characterized in that... In step (2), the temperature is reduced to 1300℃ at a rate of 10℃ / h.

6. The method for preparing the optical quartz material as described in claim 1, characterized in that... In step (3), the temperature is lowered to 1250-1270℃ at a rate of 4.5-5.5℃ / h and held for more than 100 hours; then the temperature is lowered to 990-1010℃ at a rate of 1.5-2.5℃ / h and held for more than 50 hours; finally, the temperature is lowered to 490-510℃ at a rate of 4.5-5.5℃ / h and then the power is cut off and the furnace is cooled.

7. The method for preparing the optical quartz material as described in claim 1, characterized in that... In step (3), the temperature is reduced to 1260℃ at a rate of 5℃ / h, then held for 100h, then reduced to 1000℃ at a rate of 2℃ / h, then held for 50h, and finally reduced to 500℃ at a rate of 5℃ / h before the power is cut off and the furnace is cooled.

8. The method for preparing the optical quartz material as described in claim 1, characterized in that... Replace the graphite mold with a mold made of ceramic or gypsum material.

Citation Information

Patent Citations

  • Method of press-forming

    JP2002104831A