A bilayer self-assembled collagen fiber GBR membrane, its preparation method and application

A bilayer GBR membrane was prepared by a self-assembling collagen fiber process. The dense layer was irradiated and cross-linked to form a high-density fiber network, while the loose layer was a blend of uncross-linked and cross-linked collagen fibers. Rosmarinic acid was loaded, which achieved the sutureless self-adhesion, long-lasting antibacterial effect, and matching degradation rate of the collagen-based GBR membrane, solving the problems of mechanical properties, ease of operation, and antibacterial properties in the existing technology.

CN122745376BActive Publication Date: 2026-11-10TIANJIN UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611215198.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-12
Publication Date
2026-11-10
Estimated Expiration
2046-08-12

AI Technical Summary

Technical Problem

Existing collagen-based GBR membranes are difficult to optimize in a synergistic way in terms of mechanical properties, degradation rate and biocompatibility. Clinical operation relies on suture fixation, which is inconvenient and carries the risk of displacement. They also lack long-lasting antibacterial ability and are difficult to effectively inhibit biofilm formation.

Method used

A bilayer GBR membrane was prepared using a self-assembled collagen fiber process. The dense layer was cross-linked by irradiation to form a high-density fiber network, while the loose layer was made by blending uncross-linked and cross-linked self-assembled collagen fibers. Rosmarinic acid was loaded into both layers to achieve sutureless self-adhesion, long-lasting antibacterial effect, and regulated degradation.

Benefits of technology

It achieves sutureless self-adhesive fixation of GBR membrane, improves biocompatibility and antibacterial properties, and matches the degradation cycle with the drug release cycle to the bone regeneration cycle, thus synergistically optimizing anti-infection and barrier function.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122745376B_ABST
    Figure CN122745376B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of biomedical materials and relates to a bilayer self-assembled collagen fiber GBR membrane, its preparation method, and its applications. The GBR membrane has a bilayer structure consisting of a dense layer and a loose layer. The dense layer is a self-assembled collagen fiber membrane loaded with rosmarinic acid and cross-linked by irradiation. The loose layer is composed of a blend of uncross-linked self-assembled collagen fibers A and cross-linked self-assembled collagen fibers B. In this invention, component A gels upon contact with water, imparting self-adhesion to the membrane and enabling sutureless fixation; component A preferentially degrades to form microporous channels, synergistically providing a three-dimensional scaffold function to the loose layer along with the framework of component B; the irradiated cross-linked network enables 14-day sustained release of rosmarinic acid, inhibiting biofilm formation. This invention solves three major problems of existing GBR membranes: reliance on sutures, difficulty in simultaneously achieving barrier function and tissue integration, and lack of antibacterial ability. It can be used for guided bone regeneration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of biomedical materials and relates to a double-layer self-assembled collagen fiber GBR membrane, its preparation method and application. Background Technology

[0002] Guided bone tissue regeneration (GBR) originated in the field of periodontal disease treatment, and its core is the use of a guided bone regeneration membrane (GBR membrane) as a key medical device. This membrane provides a stable biological space for the bone defect area through its physical barrier function, thereby preventing fibrous tissue ingrowth; at the same time, its scaffold function can promote the adhesion and proliferation of osteogenic progenitor cells, accelerating the bone healing process.

[0003] Currently, collagen membranes are the most widely used membrane material in GBR procedures, with representative products including Bio-Gide® from Geistlich (Switzerland) and the domestically produced Hai'ao membrane. Bio-Gide®, composed of type I and type III porcine collagen, has gained widespread recognition due to its excellent biocompatibility and ease of clinical operation.

[0004] However, existing collagen-based GBR membranes still have the following shortcomings in clinical applications: I. Mechanical properties, degradation rate, and biocompatibility are difficult to optimize in a synergistic manner. Natural, uncrosslinked collagen membranes degrade too rapidly, typically lasting only 2-4 weeks in vivo, which is insufficient to match the physiological cycle of bone regeneration (approximately 8-12 weeks), making it difficult to maintain an effective barrier function throughout the bone healing process. To prolong degradation time and improve mechanical strength, researchers have attempted to employ various crosslinking techniques to slow down the degradation process in vivo, such as ultraviolet irradiation and chemical crosslinking (glutaraldehyde, formaldehyde, carbodiimide (EDC), genipin, diphenyl azidophosphate, diisocyanate, ribose, or glycogen), among which chemical crosslinking, represented by glutaraldehyde, is the most widely used.

[0005] However, a slower degradation rate for collagen membranes is not necessarily better. While cross-linking prolongs the degradation cycle, it also reduces the membrane's tissue integration capacity and vascularization. Furthermore, the soft tissue healing of the cross-linked membrane deteriorates, and early membrane exposure severely impacts bone regeneration. Therefore, chemical cross-linking has a double-edged sword effect. Maintaining or even improving the biocompatibility of collagen membranes while enhancing mechanical properties and regulating degradation rates remains a significant technical challenge for researchers in this field.

[0006] II. Clinical procedures rely on sutures, which are inconvenient for fixation. Existing collagen-based GBR membranes require suture fixation to the bone defect site during implantation. Suturing not only prolongs surgical time and demands high surgeon skill, but also causes additional trauma to the gingival tissue, increasing the risk of postoperative inflammation. In the moist and dynamic physiological environment of the oral cavity, the sutured membrane still carries the risk of displacement; once displaced, its barrier function fails, directly impacting bone regeneration outcomes. Therefore, developing a sutureless GBR membrane that can rapidly self-adhere to the bone defect surface is of great significance for simplifying surgical procedures, shortening surgical time, and reducing trauma.

[0007] Third, it lacks antibacterial activity, and its ability to inhibit biofilm formation needs to be improved. The oral cavity is a complex microenvironment where multiple bacterial flora coexist. Post-GBR surgery, wound dehiscence and infection are common. Bacteria proliferate on the membrane material, forming structured bacterial aggregates, known as "biofilms," which accelerate material degradation and ultimately lead to the failure of bone regeneration surgery. Therefore, endowing GBR membranes with antibacterial function and inhibiting biofilm formation has become a current research hotspot. Currently, antibacterial strategies for biomaterials mainly include sustained-release and controlled-release of antibacterial drugs, grafting modification of antibacterial agents, surface coating modification, and blending. Among these, the selection of antibacterial agents is crucial. Existing antibacterial agents can be divided into natural antibacterial agents (such as rosmarinic acid), inorganic antibacterial agents (such as nano-silver), and organic antibacterial agents (such as quaternary ammonium salts). However, antibiotics are prone to burst release, with short effective concentration maintenance time (usually less than 72 hours), and long-term use can easily induce bacterial resistance. While inorganic antibacterial agents such as nano-silver have broad-spectrum antibacterial properties, their potential toxicity to osteoblasts and the safety risks of long-term accumulation in vivo are not fully understood.

[0008] In summary, existing collagen-based GBR membranes present a contradiction in the synergistic optimization of mechanical properties, degradation rate, and biocompatibility. Clinical use relies on suture fixation, which is inconvenient and carries a risk of displacement. Furthermore, they lack long-lasting antibacterial capabilities, making it difficult to effectively inhibit biofilm formation. This is attributed to the failure of current technologies to systematically design from the perspective of material structure and functional integration. Therefore, developing a GBR collagen membrane that combines self-adhesion, sutureless construction, controllable degradation, long-lasting anti-infection effects, and good biocompatibility has significant clinical value and application prospects. Summary of the Invention

[0009] Rosmarinic acid (RA) is a widely distributed bioactive phenolic acid compound that has been used in the food, pharmaceutical, and cosmetic industries, and its safety has been confirmed. Multiple studies have shown that RA possesses various biological activities, including anti-inflammatory, antiviral, antibacterial, antioxidant, and antitumor effects, and can significantly reduce the release levels of inflammatory factors such as IL-1β, IL-6, and TNF-α in the body.

[0010] Self-assembly is an important behavioral characteristic of natural collagen molecules: collagen monomers with a complete triple helix structure can further form collagen fibers with periodic interlacing stripes through ordered intermolecular arrangement. Compared with free collagen monomers, collagen fibers formed through the self-assembly pathway show significant improvements in thermal stability, resistance to enzyme degradation, and biomechanical properties. Based on this, collagen fibers can be prepared using the self-assembly characteristics of collagen, and further processed into films. With the aid of cross-linking methods, collagen-based membrane materials with mechanical properties that meet the requirements of GBR applications can be obtained.

[0011] In view of this, the present invention provides a bilayer self-assembled collagen fiber GBR membrane, its preparation method and application. It achieves sutureless self-adhesion by the water-gelling of uncrosslinked self-assembled collagen fibers in the loose layer, comprehensively regulates the degradation rate and drug release behavior by the ratio of A / B dual components, and achieves long-term sustained release of rosmarinic acid by combining it with an irradiated crosslinking network, thus playing a synergistic role. This solves the three major technical problems of existing GBR membranes: inconvenient operation, degradation-mechanical contradiction and infection risk.

[0012] The technical solution of this invention is: The first aspect of this invention discloses a method for preparing a bilayer self-assembled collagen fiber GBR membrane, comprising the following steps: (1) Preparation of self-assembled hydrogel: Dissolve animal collagen in acetic acid solution, shake until completely dissolved to obtain collagen solution, then mix collagen solution and PBS solution to obtain collagen mixture, then add rosmarinic acid to collagen mixture, adjust the final concentration of rosmarinic acid to 0.1-3 mg / mL, and let stand to obtain collagen self-assembled hydrogel; (2) Preparation of dense layer: The collagen self-assembled hydrogel was air-dried, then rinsed with purified water, and cross-linked by irradiation to obtain the dense layer of the double-layer self-assembled collagen fiber GBR membrane.

[0013] (3) Preparation of self-assembled collagen fiber A and self-assembled collagen fiber B: The collagen self-assembled hydrogel obtained in step (1) is continuously stirred to precipitate white fibers. The fibers are collected through a stainless steel sieve and drained to obtain self-assembled collagen fiber A. Self-assembled collagen fiber A is irradiated and crosslinked. After the crosslinking is completed, self-assembled collagen fiber B is obtained.

[0014] (4) Preparation of a double-layer self-assembled collagen fiber GBR membrane: The dense layer from step (2) is pre-laid into a Buchner funnel, and then the self-assembled collagen fiber A and self-assembled collagen fiber B are mixed at a mass ratio of 1:5 to 5:1 and resuspended in purified water to prepare a mixed fiber suspension. Then, the mixture is filtered to make the mixed fibers uniformly deposited on the surface of the dense layer to form a loose layer. After sterilization, a double-layer self-assembled collagen fiber GBR membrane is obtained.

[0015] Preferably, the animal collagen is one of fish collagen, bovine collagen, or porcine collagen.

[0016] Preferably, the concentration of the acetic acid solution is 0.1-1 mol / L.

[0017] Preferably, the concentration of the collagen solution is 1-10 mg / mL.

[0018] Preferably, the temperature for standing in step (1) is 20-40℃ and the standing time is 0.5-2 h.

[0019] Preferably, the irradiation crosslinking is performed using cobalt-60 irradiation crosslinking with an irradiation dose of 2-10 kGy or electron beam irradiation crosslinking.

[0020] Preferably, the pH of the PBS solution is 6.5-10.

[0021] Preferably, the collagen solution and PBS solution are mixed at a volume ratio of 1:10-50.

[0022] A second aspect of the present invention provides a bilayer self-assembled collagen fiber GBR membrane obtained by the above preparation method, which has a bilayer structure containing a dense layer and a loose layer, wherein the dense layer is formed by irradiation crosslinking of a collagen self-assembled hydrogel loaded with rosmarinic acid; the loose layer comprises self-assembled collagen fiber A and self-assembled collagen fiber B in a mass ratio of 1:5 to 5:1, wherein self-assembled collagen fiber A is an uncrosslinked self-assembled collagen fiber loaded with rosmarinic acid, and self-assembled collagen fiber B is a self-assembled collagen fiber loaded with rosmarinic acid that has been crosslinked by irradiation.

[0023] A third aspect of the present invention provides the application of the above-mentioned double-layer self-assembled collagen fiber GBR membrane in the preparation of a medical device for guiding bone tissue regeneration.

[0024] The advantages and beneficial effects of this invention are: (1) This invention is based on a self-assembled collagen fiber process and designs a structurally complementary dense layer and a porous layer. The dense layer is cross-linked by irradiation to form a high-density fiber network, which effectively prevents soft tissue ingrowth during the bone repair cycle; the porous layer innovatively adopts a blending strategy of uncross-linked self-assembled collagen fiber A and cross-linked self-assembled collagen fiber B. The self-assembled collagen fiber A undergoes a gelation transformation upon contact with water, giving the membrane material wet tissue adhesion force, and for the first time realizing sutureless self-adhesion fixation of GBR membrane, fundamentally avoiding the additional trauma and postoperative displacement risks caused by traditional suturing operations. More importantly, the preferential degradation of self-assembled collagen fiber A forms in situ interconnected microporous channels in the three-dimensional skeleton maintained by self-assembled collagen fiber B, enabling the porous layer to have the function of a dynamic active scaffold of "degradation and pore formation with simultaneous cell ingrowth" (see Figure 7This technology completely changes the inherent defects of traditional cross-linked membranes, which are "more stable and denser, and more dense and harder to integrate," and achieves a synergistic unity between barrier function and tissue integration.

[0025] (2) In this invention, rosmarinic acid, a natural phenolic acid compound, is loaded into the dense and loose layers. The abundant phenolic hydroxyl groups in the rosmarinic acid molecule can interact strongly with collagen fibers and tissue interfaces through intermolecular forces such as hydrogen bonds. This achieves long-lasting antibacterial and anti-inflammatory effects while enhancing the wet adhesion strength of the membrane, thus possessing both chemical cross-linking enhancement and anti-infection effects. The dense layer is a cross-linked, self-assembled collagen fiber membrane that can slowly release rosmarinic acid, thereby inhibiting biofilm formation during wound healing. The rosmarinic acid in the loose layer can also enhance the adhesion strength of the membrane. Antibacterial experiments show that the GBR membrane of this invention has a significant inhibitory effect on the biofilm formation of common oral pathogens (such as Staphylococcus aureus and Escherichia coli) (see [link to GBR membrane]). Figure 3 Meanwhile, rosmarinic acid itself has anti-inflammatory activity and can promote wound healing.

[0026] (3) This invention utilizes an independent three-dimensional network constructed through irradiation crosslinking to control the release of rosmarinic acid, achieving a balance between drug release and membrane degradation. The GBR membrane of this invention has a degradation cycle of approximately 8-12 weeks in vivo, matching the physiological cycle of alveolar bone regeneration. The drug release cycle (14 days) and the membrane degradation cycle (8-12 weeks) are synergistically designed: rosmarinic acid is released during the inflammatory phase (0-14 days post-surgery) to exert anti-inflammatory and anti-infective effects; while the membrane itself degrades slowly, continuously providing barrier support throughout the bone healing process. This ensures the antibacterial requirements in the acute phase while avoiding the potential inhibition of bone healing by long-term drug exposure, achieving synergistic optimization of anti-infective and barrier functions. Attached Figure Description

[0027] Figure 1 The images show a schematic diagram and photograph of the GBR membrane prepared in Example 1 of this invention, where A is a schematic diagram of the bilayer membrane structure, B is a photograph of the dense layer, C is a photograph of the fiber suspension, D is a photograph of the dense layer membrane, and E is a photograph of the loose layer membrane.

[0028] Figure 2 The image shows a scanning electron microscope (SEM) image of the GBR membrane prepared in Example 1 of this invention, where A corresponds to the dense layer, B corresponds to the loose layer, C corresponds to the dense layer after trypsin degradation treatment, and D corresponds to the loose layer after trypsin degradation treatment.

[0029] Figure 3 The images are scanning electron microscope (SEM) images of the GBR membranes prepared in Example 1 and Comparative Example 1 of this invention after being co-cultured with Escherichia coli and Staphylococcus aureus for 48 hours, respectively. The bacterial test images of Staphylococcus aureus and Escherichia coli in Comparative Example 1 correspond to A and C, respectively, while the bacterial test images of Staphylococcus aureus and Escherichia coli in Example 1 correspond to B and D, respectively.

[0030] Figure 4 The in vitro release curves of rosmarinic acid from the GBR membranes prepared in Example 1 and Comparative Example 2 of this invention are shown.

[0031] Figure 5 Micro-CT images of the defect area after 8 weeks of critical bone defect experiments on the skulls of SD rats using the GBR membranes prepared in Example 1 and Comparative Example 4.

[0032] Figure 6 H&E staining images of tissue in the defect area of ​​SD rats 8 weeks after the critical bone defect experiment.

[0033] Figure 7 This is a three-dimensional image of the cell ingrowth experiment results. Detailed Implementation

[0034] The present invention will be further described in detail below through specific embodiments. The following embodiments are merely descriptive and not limiting, and should not be used to limit the scope of protection of the present invention.

[0035] Unless otherwise specified, the experimental methods described in the following examples are conventional methods in the art; the materials and reagents used are commercially available unless otherwise specified. Unless otherwise specified, the concentrations of liquid solutions are expressed as volume ratios (v / v), and the concentrations of solid solutions are expressed as mass-volume ratios (w / v).

[0036] Example 1 A method for preparing a bilayer self-assembled collagen fiber GBR membrane includes the following steps: (1) Preparation of self-assembled hydrogel: Dissolve fish collagen in 0.5 mol / L acetic acid solution and shake at 8℃ until completely dissolved to obtain a 5 mg / mL fish collagen solution. Then mix the fish collagen solution and pH 7.4 PBS solution (0.1M phosphate buffer, manufacturer: Zhongke Ruitai, catalog number: PB7450) at a volume ratio of 1:20 to obtain a fish collagen mixture. Then add rosmarinic acid to the fish collagen mixture and adjust the final concentration of rosmarinic acid to 1.0 mg / mL. Let stand at 30℃ for 1 h to obtain the fish collagen self-assembled hydrogel for later use. (2) Preparation of the dense layer: The fish collagen self-assembled hydrogel from step (1) was air-dried in an oven at 30°C, then rinsed with purified water, and then subjected to cross-linking modification by cobalt-60 irradiation at a dose of 5 kGy to obtain the dense layer of the bilayer self-assembled collagen fiber GBR membrane (e.g. Figure 1 (As shown in B).

[0037] (3) Preparation of self-assembled collagen fiber A and self-assembled collagen fiber B: The fish collagen self-assembled hydrogel from step (1) is continuously stirred to precipitate white fibers. The fibers are collected through a stainless steel sieve and drained to obtain self-assembled collagen fiber A. Self-assembled collagen fiber A is further cross-linked by cobalt-60 irradiation with an irradiation dose of 5 kGy. After the cross-linking is completed, self-assembled collagen fiber B is obtained.

[0038] (4) Preparation of a bilayer self-assembled collagen fiber GBR membrane: The dense layer from step (2) is pre-laid into a Buchner funnel, and then self-assembled collagen fiber A and self-assembled collagen fiber B are mixed at a mass ratio of 1:1 and resuspended in purified water to prepare a mixed fiber suspension. Figure 1 (C), and then the mixed fiber suspension is poured into the Buchner funnel while stirring for filtration, so that the mixed fibers are uniformly deposited on the surface of the dense layer to form a loose layer. Then, after freeze drying and ethylene oxide sterilization, a double-layer self-assembled collagen fiber GBR membrane is obtained.

[0039] A schematic diagram of the bilayer membrane structure of a bilayer self-assembled collagen fiber GBR membrane is shown below. Figure 1 As shown in Figure A, the membrane has a dense layer and a loose layer. Figure B is a photograph of the dense layer, Figure C is a photograph of the fiber suspension, Figure D is a photograph of the dense layer membrane, and Figure E is a photograph of the loose layer membrane.

[0040] The prepared bilayer self-assembled collagen fiber GBR membrane was sputter-coated with gold, and its microstructure was observed using a scanning electron microscope. Figure 2 As shown, A corresponds to the dense layer and B corresponds to the loose layer. The results show that both the dense and loose layers have obvious collagen fiber morphology.

[0041] In addition, a bilayer self-assembled collagen fiber GBR membrane was immersed in 0.25% trypsin solution and incubated at 37°C for 3 h to simulate the degradation state of the GBR membrane sample after implantation in vivo. The sample was then lyophilized and sputter-coated with gold, and the microstructure of its dense and porous layers was observed using scanning electron microscopy. Figure 2 (C corresponds to the dense layer, and D corresponds to the loose layer). Experimental results show that the loose layer develops more pores after being soaked in trypsin for 3 hours, and this structure is more conducive to cell ingrowth, while the dense layer remains a dense structure after treatment.

[0042] Example 2 A method for preparing a bilayer collagen self-assembled fiber GBR membrane includes the following steps: (1) Preparation of self-assembled hydrogel: Dissolve porcine collagen in 0.1 mol / L acetic acid solution and shake at 4℃ until completely dissolved to obtain a 1 mg / mL porcine collagen solution. Then mix the porcine collagen solution and pH 6.6 PBS solution (0.1M phosphate buffer, manufacturer: Zhongke Ruitai, catalog number: PB6650) at a volume ratio of 1:10 to obtain a porcine collagen mixture. Then add rosmarinic acid to the porcine collagen mixture to adjust the final concentration of rosmarinic acid to 0.1 mg / mL. Let stand at 20℃ for 0.5 h to obtain porcine collagen self-assembled hydrogel for later use.

[0043] (2) Preparation of dense layer: The porcine collagen self-assembled hydrogel from step (1) was air-dried in an oven at 20°C, then rinsed with purified water, and then irradiated with cobalt-60 for cross-linking modification. The irradiation dose was 2 kGy, thus obtaining the dense layer of the double-layer self-assembled collagen fiber GBR membrane.

[0044] (3) Preparation of self-assembled collagen fiber A and self-assembled collagen fiber B: The porcine collagen self-assembled hydrogel from step (1) is continuously stirred to precipitate white fibers. The fibers are collected through a stainless steel sieve and drained to obtain self-assembled collagen fiber A. Self-assembled collagen fiber A is further cross-linked by cobalt-60 irradiation with an irradiation dose of 2 kGy. After the cross-linking is completed, self-assembled collagen fiber B is obtained.

[0045] (4) Preparation of bilayer self-assembled collagen fiber GBR membrane: The dense layer from step (2) is pre-laid into the Buchner funnel. Then, self-assembled collagen fiber A and self-assembled collagen fiber B are mixed at a mass ratio of 1:5 and resuspended in purified water to prepare a mixed fiber suspension. The mixed fiber suspension is then poured into the Buchner funnel while stirring and filtered to make the mixed fibers uniformly deposited on the surface of the dense layer to form a loose layer. After freeze-drying and irradiation sterilization, a bilayer self-assembled collagen fiber GBR membrane is obtained.

[0046] Example 3 A method for preparing a bilayer self-assembled collagen fiber GBR membrane includes the following steps: (1) Preparation of self-assembled hydrogel: Bovine collagen was dissolved in 1 mol / L acetic acid solution and shaken at 15℃ until completely dissolved to obtain a 10 mg / mL bovine collagen solution. Then, the bovine collagen solution and pH 8.0 PBS solution (0.1M phosphate buffer, manufactured by Zhongke Ruitai, catalog number PB8050) were mixed at a volume ratio of 1:50 to obtain a bovine collagen mixture. Rosmarinic acid was then added to the bovine collagen mixture to adjust the final concentration of rosmarinic acid to 3 mg / mL. The mixture was allowed to stand at 37℃ for 0.5 h to obtain a bovine collagen self-assembled hydrogel for later use. (2) Preparation of dense layer: Bovine collagen self-assembled hydrogel was air-dried in an oven at 37°C, then rinsed with purified water, and then irradiated with cobalt-60 for cross-linking modification. The irradiation dose was 10 kGy, thus obtaining the dense layer of the double-layer self-assembled collagen fiber GBR membrane.

[0047] (3) Preparation of self-assembled collagen fiber A and self-assembled collagen fiber B: The bovine collagen self-assembled hydrogel from step (1) is continuously stirred to precipitate white fibers. The fibers are collected through a stainless steel sieve and drained to obtain self-assembled collagen fiber A. Self-assembled collagen fiber A is further cross-linked by electron beam irradiation with an irradiation dose of 10 kGy. After the cross-linking is completed, self-assembled collagen fiber B is obtained.

[0048] (4) Preparation of bilayer self-assembled collagen fiber GBR membrane: The dense layer from step (2) is pre-laid into the Buchner funnel. Then, self-assembled collagen fiber A and self-assembled collagen fiber B are mixed at a mass ratio of 5:1 and resuspended in purified water to prepare a mixed fiber suspension. The mixed fiber suspension is then poured into the Buchner funnel while stirring and filtered to make the mixed fibers uniformly deposited on the surface of the dense layer to form a loose layer. After freeze-drying and irradiation sterilization, a bilayer self-assembled collagen fiber GBR membrane is obtained.

[0049] Comparative Example 1 The only difference from Example 1 is that rosmarinic acid with a final concentration of 1 mg / mL was not added when preparing the self-assembled hydrogel in step (1) to investigate the effect of adding rosmarinic acid on the performance of GBR.

[0050] Comparative Example 2 The only difference from Example 1 is that the irradiation crosslinking step is omitted in steps (2), (3) and (4) to compare and examine the effect of irradiation crosslinking on GBR performance.

[0051] The specific steps are as follows: (2) Preparation of dense layer: The fish collagen self-assembled hydrogel from step (1) was air-dried in an oven at 30°C and then rinsed with purified water to obtain the dense layer of the double-layer self-assembled collagen fiber GBR membrane.

[0052] (3) Preparation of self-assembled collagen fibers: The fish collagen self-assembled hydrogel from step (1) is continuously stirred to precipitate white fibers. The fibers are collected through a stainless steel sieve and drained to obtain self-assembled collagen fibers.

[0053] (4) Preparation of a double-layer self-assembled collagen fiber GBR membrane: The dense layer from step (2) is pre-laid into a Buchner funnel, and then the self-assembled collagen fibers are resuspended in purified water to prepare a mixed fiber suspension. The mixed fiber suspension is then poured into the Buchner funnel while stirring and filtered to make the mixed fibers uniformly deposited on the surface of the dense layer to form a loose layer. After freeze-drying and ethylene oxide sterilization, a double-layer self-assembled collagen fiber GBR membrane is obtained.

[0054] Comparative Example 3 A method for preparing a chemically cross-linked bilayer self-assembled collagen fiber GBR membrane differs from that in Example 1 only in that, in steps (2) and (3), irradiation cross-linking is replaced with carbodiimide cross-linking to compare and examine the effect of irradiation cross-linking on GBR performance.

[0055] The specific steps are as follows: (2) Preparation of dense layer: The fish collagen self-assembled hydrogel from step (1) was air-dried in an oven at 30°C, then rinsed with purified water, and then placed in a 50 mmol / L MES (2-(N-morpholino)ethanesulfonic acid) solution (pH 5.5), with 80 mmol / L EDC (1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride) and 40 mmol / L NHS (N-hydroxysuccinimide). The mixture was shaken and reacted at 20°C for 3 h, and then rinsed thoroughly with purified water to remove the crosslinking agent, thus obtaining the dense layer of the bilayer self-assembled collagen fiber GBR membrane.

[0056] (3) Preparation of self-assembled collagen fiber A and self-assembled collagen fiber B: The fish collagen self-assembled hydrogel from step (1) was continuously stirred to precipitate white fibers. The fibers were collected through a stainless steel sieve and drained to obtain self-assembled collagen fiber A. Self-assembled collagen fiber A was further placed in 50 mmol / L MES solution (pH 5.5), 80 mmol / L EDC and 40 mmol / L NHS were added, and the reaction was shaken at 20°C for 3 h. Then, it was thoroughly rinsed with purified water to remove the crosslinking agent to obtain self-assembled collagen fiber B.

[0057] Comparative Example 4 The only difference from Example 1 is that, in step (4) when preparing the loose layer of the bilayer self-assembled collagen fiber GBR membrane, only self-assembled collagen fiber B is used, and self-assembled collagen fiber A is not used.

[0058] Comparative Example 5 The only difference from Example 1 is that the mass ratio of self-assembled collagen fiber A to self-assembled collagen fiber B in step (4) is 6:1.

[0059] Comparative Example 6 The only difference from Example 1 is that the mass ratio of self-assembled collagen fiber A to self-assembled collagen fiber B in step (4) is 1:6.

[0060] Performance testing and analysis (1) Anti-biofilm performance test Using the GBR membrane prepared in Example 1 as the test sample and the GBR membrane of Comparative Example 1 as the control sample, the anti-biofilm performance was tested. The specific method is as follows: Escherichia coli and Staphylococcus aureus bacterial suspensions were prepared separately, with a bacterial concentration of 1.5 × 10⁻⁶. 6 CFU / mL. The membrane samples to be tested were cut into 10 mm × 10 mm square sheets and laid flat on the surface of solid agar medium. 50 μL of the above-mentioned *E. coli* bacterial suspension and *Staphylococcus aureus* bacterial suspension were respectively added evenly to the surface of each membrane sheet and incubated at 37℃ for 48 hours. After incubation, the membrane sheets were washed with PBS buffer to remove unattached free bacteria. Then, 2.5% glutaraldehyde solution was added, and the fixation time was no less than 4 hours. After fixation, the membrane sheets were rinsed three times with PBS, and then dehydrated sequentially with graded ethanol solutions of 30%, 50%, 70%, 80%, 90%, and 100% (v / v), each dehydration lasting 15 minutes. The dehydrated samples were then subjected to critical point carbon dioxide drying and ion sputtering gold sputtering. Finally, the samples were observed under a scanning electron microscope to record bacterial morphology and biofilm formation. The experimental results are as follows: Figure 3 As shown, the membrane sample in Comparative Example 1 was covered with bacteria and formed a distinct biofilm (the test images of Staphylococcus aureus and Escherichia coli in Comparative Example 1 are shown in Figure 1). Figure 3 As shown in Figures A and C), the membrane sample of Example 1 had very few bacteria (the test results for Staphylococcus aureus and Escherichia coli in Example 1 are shown in Figures A and C, respectively). Figure 3 As shown in Figures B and D, the pure collagen GBR membrane without added rosmarinic acid has extremely poor antibacterial and anti-biofilm capabilities, making it highly susceptible to bacterial adhesion and biofilm growth. However, the introduction of rosmarinic acid into the collagen membrane system can significantly inhibit the adhesion and proliferation of Escherichia coli and Staphylococcus aureus, effectively preventing the formation of bacterial biofilms and greatly improving the anti-biofilm performance of the double-layer collagen self-assembled GBR membrane, thus endowing the material with excellent antibacterial protection capabilities.

[0061] (2) Rosmarinic acid drug release test The GBR membrane samples prepared in Example 1 and Comparative Example 2 were placed in a PBS solution containing 0.1% Tween 80 and incubated at 37°C to simulate the in vivo release environment. Samples were taken at different time points to detect the content of rosmarinic acid released into the PBS solution. The detection method was the same as that described by Lin Shuangshuang in "Simultaneous Determination of the Content of Sargenin, Sargenin and Rosmarinic Acid by HPLC".

[0062] Rosmarinic acid in vitro release curve as follows Figure 4 As shown, in Comparative Example 2, the rosmarinic acid released into the solution reached more than 80% of its maximum concentration after 2 hours, which is a clear case of drug burst release. After that, the release curve entered a plateau phase, indicating that the drug was rapidly released and exhausted in a short period of time. In contrast, the GBR membrane sample of Example 1 showed a slow release of rosmarinic acid, with the concentration of rosmarinic acid showing a gradual increasing trend. Even after 336 hours (14 days) of continuous release, no obvious plateau was observed, indicating that the irradiated crosslinking network can effectively delay the release of rosmarinic acid and achieve a long-term and stable drug supply.

[0063] (3) Adhesion strength Using the GBR membrane prepared in Example 1 as the test sample, and the GBR membranes of Comparative Examples 1 and 4 as controls, the adhesion strength was tested. The adhesion strength of the hydrogel was determined by the overlap shear test. Fresh pigskin was taken, the fat layer was removed before use, and it was cut into uniform 1 cm × 3 cm strips. After washing with physiological saline, it was soaked in PBS buffer overnight for later use. To simulate the microenvironment of the GBR surgical wound, rabbit venous blood was dripped onto one side of the pigskin, and then the GBR membrane to be tested was covered on this area to form an overlap structure. It was left to stand for 1 hour to allow it to fully adhere. Tensile tests were performed using a universal testing machine according to GB / T 1040.4—2006 standard. The adhered pigskin strips were fixed in the testing machine fixture, equipped with a 500 N force sensor, and the tensile rate was set to 1 mm / min. The maximum load value was read. The adhesion strength was calculated according to the following formula: Adhesion strength = Maximum load / Contact area.

[0064] Experimental results showed that the adhesion strengths of the three groups of samples—Example 1, Comparative Example 1, and Comparative Example 4—were 15.17±0.31 kPa, 7.36±1.04 kPa, and 9.92±2.65 kPa, respectively. The adhesion strength of Example 1 was significantly better than the other two groups, with statistical significance (p<0.05). This experiment indicates that, compared to Comparative Example 4, which contained only component B in its loose layer, the combination of components A and B in the loose layer of Example 1 significantly improved the adhesion performance. This is because the hydrophilicity of component B weakens after cross-linking. Furthermore, compared to Comparative Example 1 without added rosmarinic acid, the adhesion strength of Example 1 was significantly increased. This indicates that the addition of rosmarinic acid has the effect of enhancing adhesion strength. This may be because rosmarinic acid is rich in phenolic hydroxyl structures. Phenolic hydroxyl groups have good hydrophilicity and chemical reactivity. These groups can interact with different material surfaces through various mechanisms such as hydrogen bonding and coordination, thereby effectively enhancing interfacial adhesion performance.

[0065] (4) Cell ingrowth experiment Mouse embryonic osteoblasts MC3T3-E1 were cultured using GBR membranes prepared in Example 1 and Comparative Example 4 to verify the effectiveness of the loose layer of the GBR membrane as a three-dimensional scaffold for guiding cell ingrowth. Specifically, the sample to be tested was cut into circular membrane pieces with a diameter of 15 mm and placed in a 24-well culture plate with the loose layer of the membrane facing upwards. 0.5 mL of α-MEM culture medium was added to each well to soak the membrane pieces, and pre-incubated at 37°C and 5% CO2 for 12 hours. After pre-incubation, the supernatant from each well was discarded, and 2.5 × 10⁻⁶ mL of medium was added to each well. 4 200 μL of MC3T3-E1 cell suspension was seeded onto the membrane surface at a density of 1 / 2 cells, followed by 300 μL of preheated DMEM complete culture medium at 37°C to each well. The culture medium was changed every 2 days. After 14 days of culture, the culture plate was removed, and the cell-membrane complex in each well was carefully separated and washed three times with PBS buffer. The complex was completely embedded with OCT embedding agent and frozen at -80°C for 12 hours. After freezing, sections with a thickness of 8 μm were cut using a cryostat. The sections were treated with PBS solution containing 0.1% Triton X-100 to increase cell membrane permeability, washed three times with PBS, and then stained with Hoechst 33342 staining solution for cell nuclei. The stained sections were observed using a laser confocal microscope, and the images were reconstructed and analyzed using 3D imaging software to obtain a direct image of cell migration into the membrane. The experimental results are as follows: Figure 7 As shown, the cells clearly grow into the interior of the GBR membrane in Example 1, and the cell distribution has a certain thickness ( Figure 7 (A); while in Comparative Example 4, the GBR membrane had only a thin layer of cells distributed ( Figure 7 In Example B), the cell ingrowth effect was significantly less than in Example 1, verifying that the loose layer prepared by blending self-assembled collagen fibers A and B in a specific mass ratio in Example 1 can impart three-dimensional scaffold properties to the loose layer, promoting cell ingrowth. Specifically, the uncrosslinked self-assembled collagen fiber A is more easily degraded, preferentially degrading and forming interconnected microporous channels in situ, providing three-dimensional space for cell ingrowth. Meanwhile, the self-assembled collagen fiber B maintains a relatively stable fibrous skeleton structure due to radiation crosslinking, continuously providing mechanical support during the degradation of component A and preventing premature scaffold collapse. The synergistic effect of pore formation by component A degradation and skeleton maintenance by component B enables a dynamic matching between degradation, pore formation, and cell ingrowth in the loose layer.

[0066] (5) Experiment on repair of critical bone defects in rat skull The GBR membrane prepared in Example 1 was used as the test sample, and the membranes prepared in Comparative Examples 1, 2, 3, and 4 were used as control samples to examine the repair effect of each group of samples on critical bone defects in the rat skull. The specific method was as follows: SD rats were anesthetized, their heads were shaved, and routine disinfection was performed. Sterile drapes and perforated drapes were then laid. A longitudinal incision of approximately 2 cm was made along the midline of the head, sequentially cutting through the skin, subcutaneous tissue, and periosteum to expose the midline suture of the skull. The periosteum was separated laterally to fully expose the bilateral parietal bones. Full-thickness skull defects with a diameter of 5 mm were prepared on both sides in the lower outer quadrant at the intersection of the midline suture and the lambdoid suture using a hollow drill. The defect areas were rinsed with saline to remove bone debris. GBR membrane samples from each group were placed in the bone defect area and sutured in layers; a blank control group was also included, where the bone defect area was directly sutured without any GBR membrane sample covering it. Postoperatively, animals were routinely administered penicillin intramuscularly for 3 days. Eight weeks postoperatively, the animals were sacrificed, dissected, and the membrane material was grossly observed for displacement. Specimens from the defect area were collected for micro-CT three-dimensional reconstruction and tomographic scanning to qualitatively assess the size of the bone defect area. After being embedded in paraffin, sections were prepared and stained with hematoxylin and eosin (H&E) to evaluate the degree of local inflammatory response.

[0067] The results showed that the GBR membrane sample prepared in Example 1 of this invention could effectively prevent material displacement. Eight weeks after implantation, the membrane remained firmly adhered to the bone defect area, while the GBR membranes in Comparative Examples 1 and 4 showed significant displacement and did not completely cover the bone defect area. Micro-CT detection results are as follows... Figure 5 As shown, Figure 5 A shows the blank control on the left and Example 1 on the right; Figure 5 B is Comparative Example 1 on the left and Comparative Example 2 on the right; Figure 5 The left side of C represents Comparative Example 3, and the right side represents Comparative Example 4. It can be seen that the bone repair effect of Example 1 is significantly better than that of the other groups.

[0068] H&E staining results are as follows Figure 6 As shown, Figure 6 A represents the blank control group. Figure 6 In the first example, B corresponds to the first instance. Figure 6 The ratio of C to C is 1. Figure 6 The ratio of D to 2 is 2. Figure 6 China's response ratio to E is 3. Figure 6 The ratio of F to the control group was 4. Compared with the control group and each control group, the degree of inflammatory cell infiltration in the bone defect area of ​​Example 1 was the mildest, and the inflammatory response in the bone defect area of ​​Example 1 was the mildest. Figure 6 In Comparative Example 1 (B), the local inflammatory response is controllable, and the biocompatibility is good. Furthermore, the membrane material from Example 1 can still be observed in the newly formed bone area, indicating that the membrane prepared by the method of this invention has a slow degradation rate and can maintain a stable scaffold structure during the bone regeneration cycle. Comparative Example 1 shows inflammation in the bone defect area (…). Figure 6 In comparison, the GBR membrane in Example 2 was almost completely degraded (C). Figure 6In Comparative Example D, residual membrane material was difficult to see, and it could not provide long-term barrier support during the bone repair cycle. The membrane material in Comparative Example 3 degraded very slowly, with few new blood vessels visible inside, and showed obvious fibrosis encapsulation. Figure 6 The E indicates that the compatibility of the membrane prepared by carbodiimide crosslinking is not as good as that of the radiation crosslinking used in this invention; in Comparative Example 4, the GBR membrane was not completely degraded, and residual membrane material was visible, indicating that radiation crosslinking plays a role in delaying material degradation. Figure 6 (Middle F).

[0069] In summary, this invention utilizes a membrane material with a cobalt-60 irradiation cross-linking and a double-layer self-assembly structure, which can precisely match the degradation rate of the material during the bone regeneration cycle and maintain a stable scaffold barrier structure throughout the bone repair process. At the same time, relying on the long-acting sustained-release effect of rosmarinic acid and its ability to enhance adhesion strength, it effectively avoids many defects of traditional collagen membranes, such as easy displacement, inflammation caused by sudden drug release, and fibrosis caused by excessively rapid or delayed degradation. It exhibits excellent in vivo application effects and bone defect repair capabilities.

[0070] (6) Barrier function test (subcutaneous implantation experiment in rats) Subcutaneous implantation experiments were conducted in rats in accordance with international standard ISO 10993-6:2016 and national standard GB / T 16886.6-2022. Samples were selected and implanted into the subcutaneous tissue of the rat's back, and the in vivo degradation of the implant was observed periodically.

[0071] A sufficient number of female SD rats were selected and housed individually in a standard temperature and humidity environment with free access to water and food, and subjected to 12-hour light-dark cycles. Preoperatively, the membrane samples from the examples and comparative examples were cut into 1 cm × 1 cm squares in a clean bench. Rats were anesthetized with an intraperitoneal injection of sodium pentobarbital at a dose of 45 mg / kg. Hair was removed from the back, and 1.5 cm transverse incisions were made on both sides of the back. The connective tissue was bluntly dissected to form subcutaneous sacs. Samples were randomly implanted into the sacs, ensuring the sample was at least 1 cm from the incision edge. The deep fascia and skin were closed sequentially using poly(lactic-co-glycolic acid) copolymer sutures and silk sutures, and the area was disinfected with povidone-iodine. Postoperatively, penicillin (40,000 U / time, twice daily) was administered intramuscularly for 3 consecutive days. After implantation, the overall condition of the rats was observed regularly. Rats were sacrificed at 4, 8, 12, 16, and 20 weeks post-surgery, and the condition of the membrane material during the implantation cycle was carefully recorded. If the membrane material could maintain a basic membrane structure without premature disintegration or barrier failure, it could be determined as an effective barrier with a stable and controllable cycle. The test results are shown in Table 1.

[0072] The performance test results of the GBR films in the examples and comparative examples are shown in Table 1.

[0073] Table 1 Summary of performance test results for each group of GBR membranes

[0074] The adhesion strength and drug release results were tested using the same test method as in Example 1.

[0075] Results analysis: As shown in Table 1, the barrier function period of Examples 1-3 can all reach 12 weeks, which matches the physiological cycle of alveolar bone regeneration (8-12 weeks). This indicates that by using different collagen sources (fish, pig, cattle) and different ratios of self-assembled collagen fibers A and B, the preparation method of the present invention can effectively control the degradation rate and has good universality. Among them, Example 3 has the highest adhesion strength (24.14 kPa), which is related to the fact that the 5:1 mass ratio of self-assembled collagen fibers A and B provides more water-reactive gelation sites and has a higher content of rosmarinic acid. The better barrier function period of Examples 1-3 is related to the radiation crosslinking and the content of self-assembled collagen fibers A and B. When the self-assembled collagen fiber component is higher, there are fewer micropores generated by degradation, which may delay the complete degradation of the membrane.

[0076] Comparative Example 1, without the addition of rosmarinic acid, showed a significant decrease in adhesion strength and a loss of anti-biofilm ability. Figure 3 This indicates that rosmarinic acid is indispensable for enhancing adhesion strength and imparting antibacterial function. In Comparative Example 2, omitting irradiation crosslinking shortened the barrier function period from 12 weeks to 4 weeks, and rosmarinic acid was released burst-released within 2 hours, indicating that irradiation crosslinking is a key process for regulating degradation rate and achieving sustained drug release. Comparative Example 3, using EDC / NHS chemical crosslinking instead of irradiation crosslinking, extended the barrier function period to 16 weeks, far exceeding the 8-12 weeks required for bone regeneration, and histological examination showed obvious fibrosis encapsulation within the material. Figure 6 The results (E) indicate that chemical crosslinking is overly stable and has poor biocompatibility, while irradiation crosslinking has significant advantages.

[0077] Comparative Example 4, which used only self-assembled collagen fiber B, showed that the adhesion strength decreased from 15.17 kPa to 9.92 kPa, indicating that the hydrogelation property of self-assembled collagen fiber A is key to endowing the membrane with self-adhesion and forming cell-infiltrating micropore channels.

[0078] Comparative Example 5, a mixture of self-assembled collagen fibers A and B at a mass ratio of 6:1, showed the highest adhesion strength (24.56 kPa), but the barrier function period was significantly shortened to 8 weeks, failing to meet the requirements of the bone regeneration cycle. Comparative Example 6, a mixture of self-assembled collagen fibers A and B at a mass ratio of 1:6, extended the barrier function period to 16 weeks, but the adhesion strength decreased significantly. This demonstrates that the optimal balance between self-adhesion performance and barrier function maintenance can be achieved when the ratio of self-assembled collagen fibers A to B is controlled within the range of 1:5 to 5:1; an imbalance in this ratio leads to the deterioration of key performance characteristics.

[0079] The above description is merely a specific embodiment of the present invention. However, those skilled in the art should understand that various changes and substitutions can be made to the specific embodiments without departing from the spirit and scope of the present invention. All such changes and substitutions fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing a bilayer self-assembled collagen fiber GBR membrane, characterized in that, The steps are as follows: (1) Preparation of self-assembled hydrogel: Dissolve animal collagen in acetic acid solution, shake until completely dissolved to obtain collagen solution, then mix collagen solution and PBS solution to obtain collagen mixture, then add rosmarinic acid to collagen mixture, adjust the final concentration of rosmarinic acid to 0.1-3 mg / mL, and let stand to obtain collagen self-assembled hydrogel; (2) Preparation of dense layer: The collagen self-assembled hydrogel was air-dried, then rinsed with purified water, and cross-linked by irradiation to obtain dense layer; (3) Preparation of self-assembled collagen fiber A and self-assembled collagen fiber B: The collagen self-assembled hydrogel obtained in step (1) is continuously stirred to precipitate white fibers. The fibers are collected through a stainless steel sieve and drained to obtain self-assembled collagen fiber A. Self-assembled collagen fiber A is irradiated and cross-linked. After the cross-linking is completed, self-assembled collagen fiber B is obtained. (4) Preparation of a double-layer self-assembled collagen fiber GBR membrane: The dense layer from step (2) is pre-laid into a Buchner funnel, and then the self-assembled collagen fiber A and self-assembled collagen fiber B are mixed at a mass ratio of 1:5 to 5:1 and resuspended in purified water to prepare a mixed fiber suspension. Then, the mixture is filtered to make the mixed fibers uniformly deposited on the surface of the dense layer to form a loose layer. After sterilization, a double-layer self-assembled collagen fiber GBR membrane is obtained.

2. The preparation method according to claim 1, characterized in that, The animal collagen is one of fish collagen, bovine collagen, or porcine collagen.

3. The preparation method according to claim 1, characterized in that, The concentration of the acetic acid solution is 0.1-1 mol / L.

4. The preparation method according to claim 1, characterized in that, The concentration of the collagen solution is 1-10 mg / mL.

5. The preparation method according to claim 1, characterized in that, The temperature for standing in step (1) is 20-40℃, and the standing time is 0.5-2 h.

6. The preparation method according to claim 1, characterized in that, The irradiation crosslinking is performed using cobalt-60 irradiation crosslinking with an irradiation dose of 2-10 kGy or electron beam irradiation crosslinking.

7. The preparation method according to claim 1, characterized in that, The pH of the PBS solution is 6.5-10.

8. The preparation method according to claim 1, characterized in that, The collagen solution and PBS solution are mixed at a volume ratio of 1:10-50.

9. A double-layer self-assembled collagen fiber GBR membrane, characterized in that, The product is prepared by any one of claims 1-8 and has a bilayer structure containing a dense layer and a loose layer. The dense layer is formed by irradiation crosslinking of a collagen self-assembled hydrogel loaded with rosmarinic acid. The loose layer contains self-assembled collagen fibers A and B in a mass ratio of 1:5 to 5:

1. Self-assembled collagen fiber A is an uncrosslinked self-assembled collagen fiber loaded with rosmarinic acid, and self-assembled collagen fiber B is a self-assembled collagen fiber loaded with rosmarinic acid that has been crosslinked by irradiation.

10. The application of the double-layer self-assembled collagen fiber GBR membrane as described in claim 9 in the preparation of a medical device for guiding bone tissue regeneration.

Citation Information

Patent Citations

  • Bone tissue regeneration guiding membrane and preparation method thereof

    CN102225219A

  • Collagen-based bilayer membrane material for directional release of loaded growth factors and manufacturing method of collagen-based bilayer membrane material

    CN107412869A