A high-temperature resistant composite plugging agent for drilling, its preparation method and application
By constructing a high heat-resistant molecular framework and introducing modified nano-silica into an organic-inorganic composite material, the problems of insufficient temperature resistance and poor aging performance of existing high-temperature resistant drilling plugging agents in deep and ultra-deep wells have been solved. This has achieved effective plugging and pressure-bearing capacity under high temperature and high pressure, ensuring the safety and efficiency of deep well drilling.
Patent Information
- Application Number
- CN202611281326.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-24
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-08-24
AI Technical Summary
Existing high-temperature resistant plugging agents for drilling have insufficient temperature resistance in deep and ultra-deep wells. Their performance deteriorates after aging, and their gel strength is low, making them unable to effectively resist re-leakage under high temperature and high pressure. This has become a key technical problem restricting the safety and efficiency of deep drilling.
A high-temperature-resistant composite plugging agent for drilling was prepared by copolymerizing selected heat-resistant monomers to construct a high-temperature-resistant molecular framework, introducing a specific crosslinking agent to achieve chemical crosslinking, and combining nano-silica modified with silane coupling agent as an inorganic reinforcing phase. The organic-inorganic composite synergistic effect was utilized to improve the heat resistance and physical strength of the material.
It maintains good sealing performance at a high temperature of 200℃, significantly reduces drilling fluid loss, and has a pressure bearing capacity of 3.5MPa, ensuring the safety of deep well drilling operations.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of drilling fluid additive technology, specifically relating to a high-temperature resistant composite plugging agent for drilling, its preparation method, and its application. Background Technology
[0002] Loss in wells is one of the most common downhole complications in drilling engineering. It refers to the phenomenon where drilling fluid leaks into formation pores, fractures, or caverns under positive pressure differential during drilling. When encountering formations with well-developed bedding and microfractures, drilling fluid filtrate easily seeps into deeper formations, leading to frequent losses. This not only affects normal drilling operations but also significantly increases drilling costs. Currently, the most efficient method for controlling losses is to use drilling-while-drilling (DWD) plugging technology. This involves adding a certain amount of DWD plugging material to the drilling fluid to form a dense sealing layer on the wellbore, thus achieving plugging while drilling and prevention of loss during drilling. Because DWD plugging requires a small amount of material, the method is simple, and drilling does not require a shutdown, this type of material has been widely used in drilling operations. As global oil and gas exploration and development continues to advance into deeper and ultra-deep formations, drilling depths continue to increase, and bottom hole temperatures rise significantly. Deep drilling generally faces harsh conditions such as high temperature (≥180℃) and high pressure. The temperature resistance of the plugging material during drilling has become a key technical bottleneck restricting the safety and efficiency of deep well drilling.
[0003] Existing high-temperature resistant plugging agents for drilling include bridging materials, polymer plugging agents, and ultra-low permeability plugging agents. Bridging plugging is inexpensive, easy to use, and safe to apply, and it is effective in dealing with various losses caused by porosity and fractures. However, bridging materials generally lack sufficient high-temperature resistance. To improve temperature resistance, high-temperature resistant bridging materials (such as mineral fibers and high-temperature resistant granular materials) are often added to develop high-temperature resistant plugging agents for drilling. For example, CN122234772A discloses the use of agricultural and forestry by-products as the main raw material for producing drilling fluid plugging agents for drilling, resulting in mud materials that meet the performance requirements of oil and gas field drilling. Intumescent polymer plugging agents have the characteristics of water absorption, swelling and deformability, and can be squeezed into formation fractures to form a strong and tough plugging layer. They mainly include water-absorbing resin, which is a cross-linked polymer gel that swells in water but does not dissolve. It is prepared by polymerization and cross-linking reaction of monomers such as acrylamide, acrylic acid, polysaccharides and quaternary ammonium cationic resins with cross-linking agents. However, it faces the problem of temperature resistance below 180℃ and insufficient compressive strength after expansion. For example, CN115785918A discloses a microsphere-type drilling plugging system suitable for fractured formations, which includes a microsphere-type drilling plugging agent, intumescent resin, plant fiber and elastic graphite. The intumescent resin is a combination of oil-absorbing and water-absorbing resins. Ultra-low permeability plugging agents are mixtures of polymers containing a large number of hydrophilic or lipophilic groups such as hydroxyl, amino, carbonyl, and carboxyl groups. These polymers with lipophilic and hydrophilic groups aggregate to form single-layer or multi-layer micelles of various shapes and sizes, such as spherical or rod-shaped ones. They can rapidly adsorb onto the pores of rock surfaces or mud cakes, and interact with bentonite and other solid particles in the drilling fluid to form a uniform and dense plugging layer. They exhibit significant leak-proofing and plugging effects when encountering pressure-depleted formations, fractured formations, and high-permeability formations. For example, Sun Dongshan et al. disclosed the experimental application of the novel ultra-low permeability treatment agent DLS-06 in the conglomerate and breccia fractured lost circulation formations of the Shu 3 well in the North China Oilfield at a depth of 1402-2300m, demonstrating that the ultra-low permeability drilling fluid formulated with it has good leak-proofing and plugging effects, ensuring normal drilling operations. However, the research and development cost of this type of plugging agent is currently high, and the mainstream research direction is mainly focused on polymer plugging agents.
[0004] However, the aforementioned high-temperature resistant plugging agents still exhibit numerous bottlenecks in practical applications in deep and ultra-deep wells. Firstly, most materials have limited long-term temperature resistance, making it difficult to meet the continuous operation requirements when bottom-hole temperatures exceed 180°C. Secondly, during high-temperature aging, the molecular structure of the plugging agent is prone to degradation or cross-linking network destruction, leading to a significant deterioration in sealing performance and a sharp decline in permeability recovery after aging. Furthermore, the strength of the formed gel or sealing layer is generally low, with insufficient pressure-bearing capacity, failing to effectively resist re-leakage under high pressure differentials. Therefore, the inherent defects of existing plugging agents in terms of temperature resistance, aging stability, and gel strength have become key technical challenges restricting their safe and efficient application in deep and ultra-deep wells. Summary of the Invention
[0005] This invention addresses the technical challenges of drilling fluid plugging under high-temperature conditions in deep and ultra-deep well drilling, aiming to provide a temperature-resistant composite plugging agent and its preparation method. By copolymerizing selected temperature-resistant monomers to construct a highly heat-resistant molecular framework, introducing specific crosslinking agents to achieve appropriate chemical crosslinking and improve molecular chain rigidity, and simultaneously introducing silane coupling agent-modified nano-silica as an inorganic reinforcing phase, a temperature-resistant composite plugging agent that maintains good plugging performance at 200℃, has a simple preparation process, and excellent compatibility with drilling fluids is prepared. This overcomes the key technical problems of existing plugging agents in deep and ultra-deep well drilling, such as insufficient temperature resistance, performance deterioration after aging, and low gel strength, ensuring the safety of deep well drilling operations.
[0006] On the one hand, the present invention provides a high-temperature resistant composite plugging agent for drilling, the raw materials for which are prepared include: The mixture contains 10-15 parts of acrylamide monomers, 5-10 parts of sulfonic acid monomers, 5-10 parts of 4-[(3-methacrylamidopropyl)dimethylammonium]butane-1-sulfonate, 0.5-1 parts of N,N'-(1,2-dihydroxyethylene)bisacrylamide, 2-5 parts of silane coupling agent modified nano-silica, 0.2-0.5 parts of initiator, and 60-80 parts of water. In some embodiments, the acrylamide monomer is N,N-dimethylacrylamide, acrylamide, N,N-diethylacrylamide, or methacrylamide.
[0007] In some embodiments, the sulfonic acid monomer is 2-acrylamide-2-methylpropanesulfonic acid, sodium methpropylene sulfonate, sodium vinyl sulfonate, or sodium p-styrene sulfonate.
[0008] In some embodiments, the silane coupling agent modified nano-silica is one or more of aminosilane modified nano-silica, epoxysilane modified nano-silica, or methacryloyloxysilane modified nano-silica, preferably one or more of 3-aminopropyltriethoxysilane modified nano-silica, γ-(2,3-epoxypropoxy)propyltrimethoxysilane modified nano-silica, or γ-methacryloyloxypropyltrimethoxysilane modified nano-silica.
[0009] In some embodiments, the preparation method of silane coupling agent modified nano-silica includes: dispersing nano-silica in an alcohol-water mixed solvent to obtain a dispersion; adjusting the dispersion to acidity to obtain an acidified dispersion; adding a silane coupling agent to the acidified dispersion, stirring and heating, and maintaining the temperature for reaction; separating the reaction product into solid and liquid components, collecting the solid components after solid-liquid separation, washing and drying them to obtain silane coupling agent modified nano-silica. Preferably, the weight ratio of nano-silica to silane coupling agent is 9-11:2-3. The particle size of the nano-silica needs to match the size of the fractures and pores in the lost formation, preferably 500-10000 nm, more preferably 5000-10000 nm. Preferably, the reaction temperature is 50-80℃, more preferably 70℃, and the reaction time is 3-5 h, more preferably 4 h. Preferably, the volume ratio of alcohol to water in the alcohol-water mixed solvent is 1:1, the alcohol is ethanol, and the water includes, but is not limited to, distilled water and deionized water. Preferably, the pH is adjusted to 3-5.
[0010] In some embodiments, the preparation method of silane coupling agent modified nano-silica is as follows: 40-50 parts of ethanol, 40-50 parts of water, and 9-11 parts of nano-silica with a particle size of 500-10000 nm are mixed evenly. The pH of the mixed solution is adjusted to 3-5 using an acidic pH adjuster. Then, 2-3 parts of silane coupling agent are added, and the mixture is heated to 50-80°C under stirring and kept at this temperature for 3-5 hours. The reaction product is then subjected to solid-liquid separation. The precipitate obtained from the solid-liquid separation is collected, washed, and dried to obtain silane coupling agent modified nano-silica. Preferably, the acidic pH adjuster is a hydrochloric acid or acetic acid solution with a concentration of 1-2 mol / L, more preferably acetic acid.
[0011] In some embodiments, the initiator is a persulfate, preferably potassium persulfate and / or sodium persulfate.
[0012] On the other hand, the present invention provides a method for preparing the aforementioned high-temperature resistant composite plugging agent while drilling, comprising: dispersing silane coupling agent modified nano-silica in water, and then adding acrylamide monomers, sulfonic acid monomers, 4-[(3-methacrylamidopropyl)dimethylammonium]butane-1-sulfonate and N,N'-(1,2-dihydroxyethylene)bisacrylamide to obtain a mixed solution; The pH of the mixed solution is adjusted to 6-8. An inert gas is then introduced into the pH-adjusted mixed solution, followed by the addition of an initiator to initiate the polymerization reaction. After the polymerization reaction is complete, the product is dried and pulverized to obtain a high-temperature resistant composite plugging agent for drilling. Preferably, the polymerization temperature is 50-70℃, more preferably 60℃, and the polymerization time is 6-8 hours, more preferably 7 hours. Preferably, the pH of the mixed solution is adjusted to 6-8 using an alkaline solution, which is a sodium hydroxide or potassium hydroxide solution with a concentration of 1-2 mol / L. Preferably, the inert gas is nitrogen, argon, or helium. Preferably, the pulverized product is finely ground and passed through an 80-500 mesh sieve, more preferably through an 80-200 mesh sieve.
[0013] On the other hand, the present invention provides an application of the aforementioned high-temperature resistant composite drilling plugging agent in drilling fluid. Preferably, the amount of the high-temperature resistant composite drilling plugging agent added to the drilling fluid is 3-5%.
[0014] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) Excellent temperature resistance: The monomers selected in this invention are mainly acrylamide monomers and sulfonic acid monomers with strong temperature resistance. At the same time, the monomer 4-[(3-methacrylamidopropyl)dimethylammonium]butane-1-sulfonate contains long side groups and quaternary ammonium salt structure, which has large steric hindrance and can further improve the thermal stability of the molecular chain. The temperature resistance of the prepared drilling plugging agent can reach 200℃.
[0015] (2) High physical strength and structural stability: By introducing N,N'-(1,2-dihydroxyethylene) bisacrylamide to achieve chemical cross-linking between molecular chains, the rigidity and strength of the polymer network structure are significantly improved; at the same time, the introduction of modified nano silica to prepare organic-inorganic composite materials further enhances the physical strength and temperature resistance of the materials, ensuring that they can still maintain an effective blocking morphology under high temperature and high pressure; the N,N'-(1,2-dihydroxyethylene) bisacrylamide used has hydroxyl side groups compared with commonly used bisacrylamide cross-linking agents, which can form a certain hydrogen bond with the hydroxyl groups on the surface of modified silica, further improving the compatibility between organic and inorganic materials and avoiding agglomeration or phase separation.
[0016] (3) Good plugging effect: After aging at 200℃ for 16 hours, the plugging agent can still significantly reduce the API filtration loss and HTHP filtration loss of drilling fluid. The pressure bearing capacity for plugging while drilling reaches 3.5MPa. It has good plugging performance while drilling in high-temperature environments of deep and ultra-deep wells, which can effectively ensure the safety of drilling operations. Detailed Implementation
[0017] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0018] Example 1 (1) Mix 40 parts of ethanol, 40 parts of water and 9 parts of silica (particle size 500~5000 nm), adjust the pH to 3 with 1 mol / L acetic acid, add 2 parts of 3-aminopropyltriethoxysilane, and heat to 50℃ for 3 hours under stirring. After centrifugation, washing and drying, 3-aminopropyltriethoxysilane modified nano silica is obtained.
[0019] (2) Take 2 parts of 3-aminopropyltriethoxysilane modified nano-silica and disperse it in 60 parts of deionized water. Then add 10 parts of N,N-dimethylacrylamide, 5 parts of 2-acrylamido-2-methylpropanesulfonic acid, 5 parts of 4-[(3-methacrylamidopropyl)dimethylammonium]butane-1-sulfonate, and 0.5 parts of N,N'-(1,2-dihydroxyethylene)bisacrylamide. Adjust the pH of the solution to 6 with sodium hydroxide. Transfer the aqueous solution to a three-necked flask, purge with nitrogen and heat to 50°C. Add 0.2 parts of potassium persulfate and react at 50°C for 6 hours. Dry the reaction mixture thoroughly, pulverize, grind, and sieve (80 mesh) to obtain a high-temperature resistant composite drilling plugging agent.
[0020] Example 2 (1) Mix 45 parts of ethanol, 45 parts of water and 10 parts of silica (particle size 5000~10000 nm), adjust the pH to 4 with 1.5 mol / L acetic acid, add 3 parts of γ-methacryloxypropyltrimethoxysilane, heat to 65℃ for 4 h under stirring, and obtain γ-methacryloxypropyltrimethoxysilane modified nano silica by centrifugation, washing and drying.
[0021] (2) Disperse 3.5 parts of γ-methacryloxypropyltrimethoxysilane modified nano-silica in 70 parts of deionized water, then add 12.5 parts of N,N-dimethylacrylamide, 7.5 parts of 2-acrylamido-2-methylpropanesulfonic acid, 7.5 parts of 4-[(3-methacrylamidopropyl)dimethylammonium]butane-1-sulfonate, and 0.75 parts of N,N'-(1,2-dihydroxyethylene)bisacrylamide. Adjust the pH of the solution to 7 with sodium hydroxide. Transfer the aqueous solution to a three-necked flask, purge with nitrogen and heat to 60°C. Add 0.35 parts of potassium persulfate and react at 60°C for 7 hours. Dry the reaction mixture thoroughly, pulverize, grind, and sieve (200 mesh) to obtain a high-temperature resistant composite drilling plugging agent.
[0022] Example 3 (1) Mix 50 parts of ethanol, 50 parts of water and 11 parts of silica (particle size 500~10000 nm), adjust the pH to 5 with 2 mol / L hydrochloric acid, add 3 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane (KH560), heat to 80℃ for 5 h under stirring, and obtain γ-(2,3-epoxypropoxy)propyltrimethoxysilane modified nano silica by centrifugation, washing and drying.
[0023] (2) Take 5 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane modified nano-silica and disperse it in 80 parts of deionized water. Then add 15 parts of N,N-diethylacrylamide, 10 parts of sodium p-styrenesulfonate, 10 parts of 4-[(3-methacrylamidopropyl)dimethylammonium]butane-1-sulfonate, and 1 part of N,N'-(1,2-dihydroxyethylene)bisacrylamide. Adjust the pH of the solution to 8 with sodium hydroxide. Transfer the aqueous solution to a three-necked flask, purge with nitrogen and heat to 70°C. Add 0.5 parts of sodium persulfate and react at 70°C for 8 hours. Dry the reaction mixture thoroughly, pulverize, grind, and sieve (500 mesh) to obtain a high-temperature resistant composite drilling plugging agent.
[0024] Example 4 (1) Mix 50 parts of ethanol, 50 parts of water and 10 parts of silica (particle size 500~8000 nm), adjust the pH to 4 with 1 mol / L acetic acid, add 2 parts of 3-aminopropyltriethoxysilane, and heat to 70℃ for 4 hours under stirring. After centrifugation, washing and drying, 3-aminopropyltriethoxysilane modified nano silica is obtained.
[0025] (2) Take 5 parts of 3-aminopropyltriethoxysilane modified nano-silica and disperse it in 70 parts of deionized water. Then add 15 parts of acrylamide, 10 parts of sodium vinyl sulfonate, 5 parts of 4-[(3-methacrylamidopropyl)dimethylammonium]butane-1-sulfonate, and 1 part of N,N'-(1,2-dihydroxyethylene)bisacrylamide. Adjust the pH of the solution to 7 with sodium hydroxide. Transfer the aqueous solution to a three-necked flask, purge with nitrogen and heat to 60°C. Add 0.5 parts of potassium persulfate and react at 60°C for 6 hours. Dry the reaction mixture thoroughly, pulverize, grind, and sieve (400 mesh) to obtain a high-temperature resistant composite drilling plugging agent.
[0026] Example 5 (1) Mix 50 parts of ethanol, 50 parts of water and 10 parts of silica (particle size 8000~10000 nm), adjust the pH to 4 with 1 mol / L acetic acid, add 2 parts of 3-aminopropyltriethoxysilane, heat to 70℃ and react for 4 h under stirring, and obtain 3-aminopropyltriethoxysilane modified nano silica by centrifugation, washing and drying.
[0027] (2) Take 5 parts of 3-aminopropyltriethoxysilane-modified nano-silica and disperse it in 70 parts of deionized water. Then add 15 parts of methacrylamide, 10 parts of sodium methacrylate sulfonate, 5 parts of 4-[(3-methacrylamidopropyl)dimethylammonium]butane-1-sulfonate, and 1 part of N,N'-(1,2-dihydroxyethylene)bisacrylamide. Adjust the pH of the solution to 7 with potassium hydroxide. Transfer the aqueous solution to a three-necked flask, purge with nitrogen and heat to 60°C. Add 0.5 parts of potassium persulfate and react at 60°C for 6 hours. Dry the reaction mixture thoroughly, pulverize, grind, and sieve (200 mesh) to obtain a high-temperature resistant composite drilling plugging agent.
[0028] Comparative Example 1 Except for the absence of γ-(2,3-epoxypropoxy)propyltrimethoxysilane modified nano-silica, the other components, proportions, and preparation methods are the same as in Example 3.
[0029] Comparative Example 2 Except for the absence of N,N'-(1,2-dihydroxyethylene)bisacrylamide, the other components, proportions, and preparation methods are the same as in Example 3.
[0030] Comparative Example 3 The difference from Example 3 is that N,N'-(1,2-dihydroxyethylene)bisacrylamide is replaced with bisacrylamide.
[0031] The performance of the prepared plugging material during drilling is evaluated below through specific embodiments.
[0032] The plugging performance of Examples 1, 2, 3, 4, and 5 in bentonite slurry was evaluated. After aging at 200℃ for 16 hours, the pressure filtration loss of API and the filtration loss of PPA were measured according to the provisions of GB / T16783.1-2014 Drilling Fluid Field Testing. The composition of the slurry was evaluated as follows: Drilling fluid preparation: Add 400mL of tap water to a high-speed stirring cup, add 1.2g of sodium bicarbonate and stir to dissolve. While stirring continuously, add 16g of bentonite quantitatively and stir for 20 minutes, stopping at least twice during the process to scrape off the clay adhering to the container wall. Cure in a sealed container for 24 hours to obtain a clay slurry.
[0033] 4% Soil slurry + 3% sulfonyl phenolic resin (SPNH) + 5% sulfonyl phenolic resin (SMP-2) + 0.3% NaOH + 1.5% polyacrylamide copolymer (AP220) + 3% silane coupling agent KH-n + 3% fluorocarbon surfactant (FT-3000) + 4% ultrafine calcium carbonate + barite (density ≥ 4.30 g / cm³) 3 The density was adjusted to 1.60 g / cm³. 3 The base slurry is obtained.
[0034] Add 5% by weight of the sealing agent to the base slurry, stir at 8000 rpm until homogeneous, age at 200℃ for 16 h, and then test the rheological properties at room temperature. The results are shown in Table 1.
[0035] Leakage plugging experiments were conducted on quartz sand beds using 20-40 mesh, 40-60 mesh, and 60-80 mesh sieves (200℃, 3.5MPa) to determine the plugging effect of adding 5% of the plugging agents prepared in Examples 1-5 and Comparative Examples 1-2. The results are shown in Table 2.
[0036] Table 1. Drilling fluid properties after aging at 200℃ for 16 hours
[0037] As shown in Table 1, compared with the base slurry, the drilling fluid's shear strength and viscosity slightly increased and HTHP filtration loss slightly decreased after adding the plugging agents prepared in Examples 1-5 of this invention before aging. After aging at 200℃ for 16 hours, the shear strength and viscosity decreased slightly compared with before aging, and the HTHP filtration loss slightly increased, but were still significantly better than the performance of the base slurry after aging. Among them, Example 3 showed the best effect, with API filtration loss decreasing to 3.0 mL after aging (compared to 4.2 mL after aging of the base slurry) and HTHP filtration loss decreasing to 9.0 mL (compared to 12.4 mL after aging of the base slurry), representing reductions of 28.6% and 27.4%, respectively. Simultaneously, the plugging agent exhibited good compatibility with the drilling fluid and did not cause drastic changes in rheological properties. The HTHP filtration loss of Comparative Example 1 (lacking modified nano silica) and Comparative Example 2 (lacking N,N'-(1,2-dihydroxyethylene)bisacrylamide) after aging was 11.0 mL and 11.5 mL, respectively, which was significantly higher than that of the examples. This demonstrates that the synergistic effect of modified nano silica and N,N'-(1,2-dihydroxyethylene)bisacrylamide is crucial for improving the temperature-resistant sealing performance.
[0038] Table 2. Experimental results of sand bed leakage at 200℃ and 3.5MPa
[0039] As shown in Table 2, in the sand bed plugging evaluation test at 200℃ and 3.5MPa, the drilling plugging agents prepared in Examples 1-5 of this invention exhibited low sand bed leakage, which was significantly less than that of the base slurry and the comparative example, indicating that they possess excellent temperature-resistant plugging performance. Among them, Example 3 showed the best overall performance. The leakage of the sand bed in Comparative Example 1 (without modified nano-silica) and Comparative Example 2 (without N,N'-(1,2-dihydroxyethylene)bisacrylamide) was significantly increased compared to the examples. This indicates that the synergistic effect of modified nano-silica and N,N'-(1,2-dihydroxyethylene)bisacrylamide is crucial for improving the temperature resistance and sealing strength of the plugging agent. Although the polymer system of Comparative Example 1 retained the chemical cross-linking network constructed by N,N'-(1,2-dihydroxyethylene)bisacrylamide, it lacked the inorganic reinforcing phase provided by nano-silica. At a high temperature of 200°C, the chain segments between the cross-linking points loosened, resulting in a significant decrease in the density and mechanical rigidity of the network structure. Comparative Example 2 completely lacked the chemical cross-linking structure, and the polymer was in the form of linear molecular chains. During high-temperature aging, the linear polymer molecular chains were prone to untangling, overhydration, and even partial dissolution. Lacking the anchoring and constraint of the cross-linking network, agglomeration or phase separation occurred, resulting in the sealing layer basically losing its mechanical integrity, and the leakage of the sand bed was close to the level of the base slurry. In Comparative Example 3, after replacing the hydroxyl-containing crosslinking agent with conventional bisacrylamide, the hydrogen bonding at the organic-inorganic interface disappeared, compatibility decreased, the synergistic sealing effect weakened, and leakage of sand beds of all mesh sizes increased significantly, resulting in sealing performance that was significantly inferior to that of the embodiments of the present invention. The above-mentioned differences in molecular structure fully demonstrate that the three-dimensional network constructed by chemical crosslinking is the skeletal basis for the high-temperature stability of the sealing agent, and the inorganic reinforcement of nano-silica is a key supplement to improve mechanical strength; both are indispensable.
[0040] Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A high-temperature resistant composite leak-proof agent for drilling, characterized in that, Its raw materials include: The mixture contains 10-15 parts of acrylamide monomers, 5-10 parts of sulfonic acid monomers, 5-10 parts of 4-[(3-methacrylamidopropyl)dimethylammonium]butane-1-sulfonate, 0.5-1 parts of N,N'-(1,2-dihydroxyethylene)bisacrylamide, 2-5 parts of silane coupling agent modified nano-silica, 0.2-0.5 parts of initiator, and 60-80 parts of water. The acrylamide monomer and the sulfonic acid monomer are any one of the following combinations: N,N-dimethylacrylamide and 2-acrylamide-2-methylpropanesulfonic acid, N,N-diethylacrylamide and sodium p-styrenesulfonate, acrylamide and sodium vinylsulfonate, or a combination of methacrylamide and sodium methpropylenesulfonate.
2. The high-temperature resistant composite leak-proof agent for drilling as described in claim 1, characterized in that, The silane coupling agent modified nano-silica is one or more of aminosilane modified nano-silica, epoxysilane modified nano-silica, or methacryloxysilane modified nano-silica.
3. The high-temperature resistant composite leak-proof agent for drilling as described in claim 1, characterized in that, The preparation method of the silane coupling agent modified nano-silica includes: dispersing nano-silica in an alcohol-water mixed solvent to obtain a dispersion; adjusting the dispersion to acidity to obtain an acidified dispersion; adding a silane coupling agent to the acidified dispersion, stirring and heating, and then maintaining the temperature for reaction; separating the reaction product into solid and liquid components; collecting the solid components from the solid-liquid separation; and washing and drying the solid components to obtain the silane coupling agent modified nano-silica.
4. The high-temperature resistant composite leak-proof agent for drilling as described in claim 3, characterized in that, The weight ratio of the nano-silica to the silane coupling agent is 9-11:2-3; the particle size of the nano-silica is 500-10000 nm; the reaction temperature is 50-80℃, and the reaction time is 3-5 h.
5. The high-temperature resistant composite leak-proof agent for drilling as described in claim 1, characterized in that, The initiator is persulfate.
6. A method for preparing a high-temperature resistant composite leak-proof agent as described in any one of claims 1-5, characterized in that, The preparation method includes: Silane coupling agent-modified nano-silica was dispersed in water, and then acrylamide monomers, sulfonic acid monomers, 4-[(3-methacrylamidopropyl)dimethylammonium]butane-1-sulfonate and N,N'-(1,2-dihydroxyethylene)bisacrylamide were added to obtain a mixed solution. The pH of the mixed solution is adjusted to 6-8, an inert gas is introduced into the pH-adjusted mixed solution, and then an initiator is added to initiate the polymerization reaction. After the polymerization reaction is completed, the product of the polymerization reaction is dried and pulverized to obtain the high-temperature resistant composite drilling plugging agent.
7. The preparation method of the high-temperature resistant composite drilling plugging agent according to claim 6, characterized in that, The polymerization reaction is carried out at a temperature of 50-70°C for 6-8 hours.
8. The application of the high-temperature resistant composite plugging agent according to any one of claims 1-5 in drilling fluid.
Citation Information
Patent Citations
Microspherical while-drilling plugging system suitable for fractured formation
CN115785918A
Method for producing plugging agent while drilling for drilling fluid by utilizing leftovers of agricultural and forestry byproducts
CN122234772A
Wall-fixing leakproof water-based drilling fluid for myriameter deep well as well as preparation method and application thereof
CN120737821A
Zwitterionic polymer clay protective agent as well as preparation method and application thereof
CN122483257A