A positive electrode material and its preparation method, a positive electrode sheet, and a lithium-ion battery.
By constructing a composite coating layer of tannic acid bridging layer, conductive carbon layer and ion conductor layer on the surface of high-nickel layered ternary cathode material, the structural stability and interfacial reaction problems of high-nickel layered ternary cathode material are solved, thereby improving the cycle stability and battery performance of lithium-ion batteries.
Patent Information
- Application Number
- CN202611230083.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-13
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-08-13
AI Technical Summary
High-nickel layered ternary cathode materials exhibit poor structural stability, increased cation mixing, lattice oxygen release, and a transformation of the layered phase to the rock salt phase under high delithiation conditions. Furthermore, interfacial side reactions between the cathode material surface and the electrolyte lead to electrolyte decomposition, transition metal dissolution, CEI film instability, and increased interfacial impedance, all of which affect lithium-ion transport and battery performance.
A composite coating layer consisting of a tannic acid bridging layer, a conductive carbon layer, and an ion conductor layer is constructed. The phenolic hydroxyl groups of tannic acid coordinate with the metal elements on the surface of the ion conductor layer and form hydrogen bonds. The aromatic rings form π-π interactions with the surface of the conductive carbon material, thus constructing a stable conductive carbon layer. The residual lithium compounds on the surface of the layered lithium-containing cathode material substrate are used as the lithium source for the reaction, thereby realizing a composite coating layer with dual ion/electron functions.
It effectively reduces interfacial charge transfer impedance, improves the migration ability of lithium ions at the cathode/electrolyte interface, suppresses electrolyte side reactions and transition metal dissolution, and enhances the cycle stability and battery performance of lithium-ion batteries.
Smart Images

Figure CN122843350B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of cathode materials for lithium-ion batteries, and in particular to a cathode material with a tannic acid-bridged conductive carbon layer and an ion conductor synergistically coated, its preparation method, cathode sheet, and lithium-ion battery. Background Technology
[0002] High-nickel layered ternary cathode materials are among the preferred cathode materials for lithium-ion batteries. However, these materials suffer from poor structural stability, increased cation mixing, lattice oxygen release, and the transformation of the layered phase to the rock salt phase under high delithiation conditions. Simultaneously, interfacial side reactions between residual lithium compounds on the cathode material surface and the electrolyte lead to continuous electrolyte decomposition, transition metal dissolution, CEI film instability, and increased interfacial impedance, resulting in impaired lithium-ion transport, capacity decay, reduced rate performance, and deteriorated high-temperature storage performance.
[0003] Surface coating is an effective method to improve the interfacial stability of high-nickel ternary cathode materials. Oxide coatings such as TiO2, Al2O3, and ZrO2 can isolate the electrolyte and suppress side reactions, while lithium-ion conductive layers such as Li3BO3, LiNbO3, Li3PO4, and Li2ZrO3 have both protective and lithium-conducting functions. However, these coatings inevitably increase interfacial impedance, which can affect the rate performance and cycle stability of the battery.
[0004] It should be noted that the information disclosed in the background section above is only for understanding the background of this application, and therefore may include information that does not constitute prior art known to those skilled in the art. Summary of the Invention
[0005] To overcome the shortcomings of existing technologies, this invention provides a positive electrode material and its preparation method, a positive electrode sheet, and a lithium-ion battery.
[0006] The present invention adopts the following technical solution: In a first aspect, a cathode material is provided, comprising: a layered lithium-containing cathode material matrix and a composite coating layer covering the layered lithium-containing cathode material matrix; the composite coating layer comprises an ion conductor layer, a tannic acid bridging layer, and a conductive carbon layer; the ion conductor layer, coated on the surface of the layered lithium-containing cathode material matrix, is a lithium salt formed by an in-situ reaction of an ion conductor precursor and a lithium source through a first heat treatment, wherein the lithium source includes residual lithium compounds on the surface of the layered lithium-containing cathode material matrix; the tannic acid bridging layer is composed of tannic acid; the conductive carbon layer is formed by a second heat treatment conversion of conductive carbon material and a portion of tannic acid; wherein the phenolic hydroxyl groups of the tannic acid in the tannic acid bridging layer form coordination and hydrogen bonding with metal elements on the surface of the ion conductor layer, and its aromatic ring forms π-π interactions with the surface of the conductive carbon material to promote uniform adhesion of the conductive carbon material on the surface of the ion conductor layer, thereby ensuring that the conductive carbon layer is stably bonded to the surface of the ion conductor layer.
[0007] In a second aspect, a method for preparing the cathode material described in the first aspect is provided, comprising the following steps: S1. Provides a layered lithium-containing cathode material matrix; S2. The ion conductor precursor is mixed with the layered lithium-containing cathode material matrix and subjected to a first heat treatment in an oxygen-containing atmosphere, so that the ion conductor precursor reacts in situ with the residual lithium compounds on the surface of the layered lithium-containing cathode material matrix, and the ion conductor layer is coated on the surface of the layered lithium-containing cathode material matrix to obtain the first material. S3. Dissolve tannic acid in a buffer solvent to prepare a uniformly dispersed tannic acid solution; S4. Mix the conductive carbon material with the first material to obtain the second material; S5. The second material is mixed and stirred with the tannic acid solution to bridge the tannic acid molecules between the ion conductor layer and the conductive carbon material. After filtration, washing and drying, the third material is obtained. S6. The third material is subjected to a second heat treatment under an inert atmosphere. During the second heat treatment, the tannic acid undergoes partial carbonization and conversion into a poly(p-containing) form. 2 Oxygen-containing amorphous carbon with a carbon structure is used to form a composite carbon network together with the conductive carbon material to form a conductive carbon layer, thereby obtaining the cathode material.
[0008] Thirdly, a positive electrode sheet is provided, which includes the positive electrode material described in the first aspect.
[0009] Fourthly, a lithium-ion battery is provided, which includes the positive electrode sheet described in the third aspect.
[0010] This invention has the following beneficial effects: It achieves a stable bridge between the ion conductor layer and the conductive carbon layer by coordinating and hydrogen bonding between the phenolic hydroxyl groups of tannic acid molecules and the metal elements on the surface of the ion conductor layer, and simultaneously by forming π-π interactions between the aromatic ring structure of tannic acid and the conductive carbon layer material. This results in a continuous and uniform composite coating layer with dual ion / electron transport functions. Furthermore, it utilizes residual lithium compounds on the surface of the layered lithium-containing cathode material matrix as a lithium source for reaction, transforming harmful surface impurities into beneficial components of the ion conductor layer, thus achieving waste utilization. The composite coating layer provides both a good ion conduction channel and an electron conduction network, effectively reducing interfacial charge transfer impedance and improving the migration ability of lithium ions at the cathode / electrolyte interface. Simultaneously, it suppresses electrolyte side reactions, transition metal dissolution, and high-nickel cathode surface structure degradation. Therefore, this invention simultaneously achieves residual lithium conversion, uniform coating, and the construction of a dual ion / electrolyte interface, improving the cycle stability of lithium-ion batteries. Attached Figure Description
[0011] Figure 1 This is a schematic diagram of the structure of the cathode material in a specific embodiment of the present invention.
[0012] Figure 2a The diagram shows the cycle performance of batteries assembled from the cathode material samples of Examples 1-3 and Comparative Example 1 of this invention.
[0013] Figure 2b The diagram shows the cycle performance of batteries assembled from the cathode material samples of Comparative Examples 2-4 of this invention.
[0014] Figure 3 The images show the SEM morphology of the cathode material samples from Examples 1-3 and Comparative Example 1 of this invention.
[0015] Figure 4 The XRD phase diagrams are of TA-C / Nb@NCM in Example 3 and NCM in Comparative Example 1.
[0016] Figure 5a This is an EDS elemental distribution diagram of TA-C / B@NCM in Embodiment 1 of the present invention.
[0017] Figure 5b This is an EDS elemental distribution diagram of TA-C / Al@NCM in Embodiment 2 of the present invention.
[0018] Figure 5c This is an EDS elemental distribution diagram of TA-C / Nb@NCM in Embodiment 3 of the present invention.
[0019] Figure 6 The images show the Raman spectra of TA-C / B@NCM in Example 1, TA-C / Al@NCM in Example 2, and TA-C / Nb@NCM in Example 3 of this invention.
[0020] Figure 7 Infrared images of TA-C / Al@NCM in Example 2 and TA-C / Nb@NCM in Example 3 of the present invention.
[0021] Figure 8 The images show the SEM image and corresponding EDS spectrum of TA-C / Al@NCM in Example 2 of this invention.
[0022] Figure 9a This is a SEM image of TA-C / B@NCM in Embodiment 1 of the present invention.
[0023] Figure 9b This is a SEM image of TA-C / Al@NCM in Embodiment 2 of the present invention.
[0024] Figure 9c This is a SEM image of TA-C / Nb@NCM in Embodiment 3 of the present invention.
[0025] Figure 10a The image shows the Raman spectrum of TA-Al@NCM in Comparative Example 5 of this invention.
[0026] Figure 10b This is the Raman spectrum of TA-C / Al@NCM in Example 2 of the present invention. Detailed Implementation
[0027] The embodiments of the present invention are described in detail below. It should be emphasized that the following description is merely exemplary and not intended to limit the scope or application of the invention. Unless otherwise specified, the embodiments and features described in this application can be combined with each other. Room temperature in this document refers to 25-30°C.
[0028] Unless otherwise stated, the numerical values used in the specification and claims to indicate the amount of components, reaction temperature, reaction time, etc., are to be understood as approximate values. A numerical range indicated by endpoints includes all values within that range as well as subranges formed by any combination of endpoints.
[0029] This invention provides a positive electrode material, such as... Figure 1As shown, it includes: a layered lithium-containing cathode material substrate 1 and a composite coating layer covering the layered lithium-containing cathode material substrate 1; the composite coating layer includes an ion conductor layer 2, a tannic acid bridging layer 3, and a conductive carbon layer 4. The ion conductor layer 2 is coated on the surface of the layered lithium-containing cathode material substrate 1 and is a lithium salt formed by the in-situ reaction of an ion conductor precursor and a lithium source through a first heat treatment. The lithium source includes residual lithium compounds on the surface of the layered lithium-containing cathode material substrate. The tannic acid bridging layer 3 is composed of tannic acid, and the conductive carbon layer 4 is formed by the conversion of conductive carbon material and part of tannic acid through a second heat treatment. The phenolic hydroxyl groups of tannic acid in the tannic acid bridging layer form coordination and hydrogen bonding with the metal elements on the surface of the ion conductor layer 2, and its aromatic ring forms π-π interactions with the surface of the conductive carbon material to promote the uniform adhesion of the conductive carbon material in the conductive carbon layer 4 on the surface of the ion conductor layer, thereby the conductive carbon layer 4 is stably bonded to the surface of the ion conductor layer 2.
[0030] In some embodiments, the chemical formula of the layered lithium-containing cathode material matrix is LiNi. x Co y M 1-x-y O2, where 0.80≤x≤0.98, 0≤y≤0.20, and x+y<1, and M is at least one of Al, Mn, and Mg.
[0031] In some embodiments, the layered lithium-containing cathode material matrix is LiNi. 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.83 Co 0.11 Mn 0.06 O2, LiNi 0.9 Co 0.05 Mn 0.05 O2, LiNi 0.9 Co 0.05 Al 0.05 One of the components of O2.
[0032] In some embodiments, the ion conductor layer comprises LiBO2 and Li3BO2. 3、 At least one of LiNbO3, LiAlO2, LiPO3, and Li2SeO4.
[0033] In some embodiments, based on the mass of the layered lithium-containing cathode material matrix, the tannic acid content is 0.01-5 wt%, preferably 0.05-4 wt%. If the tannic acid content is too low, it is difficult to fully bond the conductive carbon layer and the ion conductor layer; if the content is too high, excessive organic decomposition residues may be introduced after heat treatment, or the composite coating layer may become too thick.
[0034] In some embodiments, the layered lithium-containing cathode material matrix is a high-nickel ternary cathode material, preferably NCM811, NCM83, NCM90 or NCA.
[0035] In some embodiments, the conductive carbon layer comprises at least one of graphene, graphene oxide, reduced graphene oxide, carbon nanotubes (such as multi-walled carbon nanotubes), carbon fibers (such as vapor-grown carbon fibers), and conductive carbon black (such as Ketjen black, Super P, and acetylene black).
[0036] In some embodiments, the thickness of the composite coating layer is 10-70 nm, preferably 15-40 nm. By controlling the total thickness of the composite coating layer, an effective protective layer can be formed without excessively hindering Li. + transmission.
[0037] In some embodiments, the residual lithium compounds on the surface of the layered lithium-containing cathode material matrix mainly include LiOH and Li2CO3; the lithium source also includes a supplementary lithium source, which includes at least one of LiOH·H2O, Li2CO3, LiNO3, CH3COOLi, and Li2O.
[0038] The present invention also provides a method for preparing the aforementioned cathode material, comprising the following steps: S1. Provides a layered lithium-containing cathode material matrix; S2. The ion conductor precursor is mixed with the layered lithium-containing cathode material matrix and subjected to a first heat treatment in an oxygen-containing atmosphere, so that the ion conductor precursor reacts in situ with the residual lithium compounds on the surface of the layered lithium-containing cathode material matrix, and the ion conductor layer is coated on the surface of the layered lithium-containing cathode material matrix to obtain the first material. S3. Dissolve tannic acid in a buffer solvent to prepare a uniformly dispersed tannic acid solution; S4. Mix the conductive carbon material with the first material to obtain the second material; S5. The second material is mixed and stirred with the tannic acid solution to bridge the tannic acid molecules between the ion conductor layer and the conductive carbon material. After filtration, washing and drying, the third material is obtained. S6. The third material is subjected to a second heat treatment under an inert atmosphere. During the second heat treatment, the tannic acid undergoes partial carbonization and conversion into a poly(p-containing) form. 2 The oxygen-containing amorphous carbon with a carbon structure, together with the conductive carbon material, constitutes a composite carbon network, forming a conductive carbon layer, thus obtaining the cathode material.
[0039] During the processing in step S5, the phenolic hydroxyl groups of tannic acid form coordination and hydrogen bonds with the metal elements on the surface of the ion conductor layer, and the aromatic rings of tannic acid form π-π interactions with the surface of the conductive carbon material. This plays an adhesive, bridging, and dispersing role between the ion conductor layer and the conductive carbon layer, promoting the uniform adhesion of the conductive carbon material on the surface of the ion conductor layer and improving the continuity, bonding strength, and interfacial charge transport capability of the ion / electron bifunctional interface layer. In addition to using tannic acid as an interfacial complexation inducer to tightly bind the ion conductor layer and the conductive carbon layer, in the heat treatment in step S6, some tannic acid molecules undergo dehydration condensation and aromatic structure recombination to form oxygen-containing amorphous carbon with defective sp² carbon structures. This oxygen-containing amorphous carbon and the conductive carbon material together constitute a composite carbon network to form a conductive carbon layer. Thus, the present invention simultaneously achieves residual lithium conversion, uniform coating, and the construction of an ion / electron bifunctional interface.
[0040] In some embodiments, in step S3, the buffer solvent is a Tris-HCl (tris-hydroxymethylaminomethane hydrochloride) buffer solution with a pH value set to 7-8. Preferably, the tannic acid concentration in the tannic acid solution prepared in step S3 is 0.1-20 g / L, more preferably 0.5-10 g / L. Preferably, the stirring in step S3 is carried out at room temperature, at a stirring speed of 700-900 rpm, and for 3-4 hours.
[0041] In some embodiments, the temperature of the first heat treatment in step S2 is 300-750°C, the heat treatment time is 6-12 hours, and the oxygen-containing atmosphere can be air, oxygen, or an oxygen-containing mixture. Preferably, the temperature of the first heat treatment is 450-650°C.
[0042] In some embodiments, the temperature of the second heat treatment in step S6 is 150-350°C, and the heat treatment time is 1-2 hours. Preferably, the temperature of the second heat treatment is 200-300°C. The degree of partial carbonization of tannic acid is controlled by the heat treatment temperature and time in a coordinated manner. More preferably, high-purity nitrogen is first introduced into the tube furnace to purge air for 5-10 minutes. Then, the third material obtained in S5 is evenly spread in a quartz boat and placed in the tube furnace. The temperature is increased to 150°C-350°C at a heating rate of 2°C / min-5°C / min and held for 1-2 hours to allow partial carbonization of tannic acid. The furnace is then cooled to room temperature, with nitrogen protection maintained during the cooling process.
[0043] In some embodiments, step S2 further includes adding a lithium source, wherein the added lithium source includes at least one selected from LiOH·H2O, Li2CO3, LiNO3, CH3COOLi, and Li2O; step S2 includes: mixing the ionic conductor precursor with the layered lithium-containing cathode material matrix and the added lithium source, and performing a first heat treatment, so that the ionic conductor precursor reacts in situ with the residual lithium compounds on the surface of the layered lithium-containing cathode material matrix and the added lithium source, thereby coating the surface of the layered lithium-containing cathode material matrix with an ionic conductor layer to obtain a first material. By adding a lithium source, sufficient lithium source for the formation reaction of the ionic conductor layer can be ensured, especially when there is insufficient residual lithium compound on the surface of the cathode material matrix. The content of the added lithium source can be adjusted according to the content of the residual lithium compound or a preset ratio. The residual lithium compound and the added lithium source together act as a lithium source to react in situ with the ionic conductor precursor to generate lithium salt.
[0044] In some embodiments, in step S2, the ionic conductor precursor includes at least one of a boron source, a niobium source, an aluminum source, a phosphorus source, and a selenium source; the boron source is at least one of H3BO3, B2O3, LiBO2, and Li2B4O7; the niobium source is at least one of Nb2O5, LiNbO3, ammonium niobate oxalate, and ammonium niobate; the aluminum source is at least one of Al2O3, Al(OH)3, Al(NO3)3, and aluminum isopropoxide; the phosphorus source is at least one of NH4H2PO4, LiH2PO4, and Li3PO4; and the selenium source is at least one of SeO2, Se, and Li2SeO4.
[0045] In some embodiments, in step S2, the amount of the ion conductor precursor added is 0.05-10 wt% based on the mass of the layered lithium-containing cathode material matrix, preferably 0.2-3 wt%.
[0046] In some embodiments, in step S4, the content of the conductive carbon material is 0.01-5 wt%, preferably 0.05-2 wt%, based on the mass of the layered lithium-containing cathode material matrix.
[0047] In some embodiments, in step S4, the conductive carbon material is a mixture of graphene oxide and multi-walled carbon nanotubes, with the amount of graphene oxide added being 0.5-2 wt% and the amount of multi-walled carbon nanotubes added being 0.5-5 wt%, based on the mass of the layered lithium-containing cathode material matrix.
[0048] In some embodiments, the mixing in step S4 is carried out using a planetary ball mill with anhydrous ethanol as the medium. The powder is immersed in anhydrous ethanol, the ball-to-powder ratio is 2:1-5:1, the rotation speed is 100-300 rpm, the mixing time is 10-30 min, and then the powder is placed in an oven at 30-60℃ to evaporate the ethanol.
[0049] In some embodiments, the drying temperature in step S5 is 60-80°C, and the time is 3-6 hours.
[0050] A specific embodiment of the present invention also provides a positive electrode sheet, which includes the aforementioned positive electrode material.
[0051] A specific embodiment of the present invention also provides a lithium-ion battery, which includes the aforementioned positive electrode sheet.
[0052] The following describes specific embodiments of the present invention.
[0053] Example 1 LiBO2 and conductive carbon materials (a mixture of graphene oxide (GO) and carbon nanotubes (CNT), referred to as GO-CNT) were used to coat NCM811 (LiNi). 0.8 Co 0.1 Mn 0.1 O 2 ), denoted as TA-C / B@NCM, its specific steps include: S1. Provide a layered NCM811 cathode material matrix (hereinafter referred to as "cathode material matrix").
[0054] S2, Ion conductor layer coated positive electrode material matrix 800 mg of the positive electrode material matrix was weighed and determined by dual-endpoint acid-base titration. The residual alkali on its surface was mainly composed of LiOH and Li₂CO₃, with LiOH content of 0.054 wt% and Li₂CO₃ content of 0.166 wt%. After conversion, the residual Li₂CO₃ content on the surface of 800 mg NCM811 is... + The content is approximately 0.054 mmol. With a specific surface area of 0.32 m² for NCM811... 2 / g, LiBO2 density is approximately 2.2g / cm³ 3 Theoretically, forming a 19-40 nm LiBO2 coating layer with 800 mg NCM811 requires approximately 10.7-22.5 mg of LiBO2, corresponding to the required Li... + Approximately 0.215-0.452 mmol. In this example, 21 mg of H3BO3 was added, and an intermediate thickness of approximately 30 nm was chosen as the target coating thickness. This corresponds to approximately 16.9 mg of LiBO2 required, and the 21 mg of H3BO3 requires approximately 16.9 mg of Li. +Approximately 0.340 mmol. Since the residual alkali on the NCM811 surface can only provide approximately 0.054 mmol of Li. + Therefore, 12 mg of LiOH·H2O was added as a lithium source. 800 mg of the cathode material matrix, 21 mg of H3BO3, 12 mg of LiOH·H2O, and 3 ml of ethanol were mixed using a planetary ball mill at a ball-to-material ratio of 2:1, a speed of 300 rpm, for 30 min. The mixture was then placed in a 30°C oven to evaporate the ethanol. Next, the resulting powder was placed in an oxygen atmosphere in a tube furnace and heated to 600°C at a rate of 5°C / min, held for 12 h, and then cooled with the furnace to obtain the first material, denoted as B@NCM. In step S2, the main chemical reaction is: LiOH + H3BO3 = LiBO2 + 2H2O.
[0055] S3. Preparation of tannic acid solution: Dissolve 30 mg of tannic acid in 3 ml of Tris-HCl solvent to obtain a uniformly dispersed orange-yellow solution with pH 7-8. Stir at room temperature for 10 min at a speed of 600 rpm.
[0056] S4, Addition of conductive carbon material The first material obtained in step S2 was mixed with the conductive carbon material, which was a mixture of 10 mg of graphene oxide and 2 mg of multi-walled carbon nanotubes. 3 ml of ethanol was added, and the mixture was mixed using a planetary ball mill with a ball-to-material ratio of 2:1 at 300 rpm for 30 min. The mixture was then placed in a 30°C oven to evaporate the ethanol, thus obtaining the second material.
[0057] S5, a combination of conductive carbon layer and ion conductor layer Add the tannic acid solution prepared in step S3 to the second material obtained in step S4, stir magnetically at 700 rpm for 4 hours, wash three times with anhydrous ethanol during the filtration process to remove unbound free components, and vacuum dry at 80°C for 3 hours to obtain the third material.
[0058] S6, Low-temperature carbonization coating The third material was placed in a tube furnace and heated to 280°C at a rate of 5°C / min. The temperature was maintained for 1 hour to partially carbonize the tannic acid. The material was then cooled to room temperature with the furnace under nitrogen protection to obtain a cathode material with dual ion / electron coating, denoted as TA-C / B@NCM.
[0059] Example 2 The specific steps for coating NCM811 with LiAlO2 and conductive carbon material (GO-CNT), denoted as TA-C / Al@NCM, are as follows: S1. Provide the same layered NCM811 cathode material matrix as in Example 1.
[0060] S2, Ion conductor layer coated positive electrode material matrix 800 mg of the positive electrode material matrix was weighed out, and the same measurement and calculation methods as in Example 1 were used. The density of LiAlO2 was 2.62 g / cm³. 3 Based on the expected thickness requirement of 30 nm, 15.6 mg Al₂O₃, 10.5 mg LiOH·H₂O, and 3 ml ethanol were added and mixed using a planetary ball mill at a ball-to-powder ratio of 2:1 at 300 rpm for 30 min. The mixture was then placed in a 30°C oven to evaporate the ethanol. Next, the resulting powder was placed in an oxygen atmosphere in a tube furnace and heated to 750°C at 5°C / min for 12 h, followed by furnace cooling to obtain the first material, denoted as Al@NCM. In step S2, the main chemical reactions are: 2LiOH = Li₂O + 2H₂O; Li₂O + Al₂O₃ = 2LiAlO₂.
[0061] S3, Preparation of Tannic Acid Solution 30 mg of tannic acid was dissolved in 3 ml of Tris-HCl solvent to obtain a uniformly dispersed orange-yellow solution with a pH of 7-8. The solution was stirred at room temperature for 10 min at a speed of 600 rpm.
[0062] S4, Addition of conductive carbon material The first material obtained in step S2 was mixed with the conductive carbon material, which was a mixture of 10 mg of graphene oxide and 2 mg of multi-walled carbon nanotubes. 3 ml of ethanol was added, and the mixture was mixed using a planetary ball mill with a ball-to-material ratio of 2:1 at 300 rpm for 30 min. The mixture was then placed in a 30°C oven to evaporate the ethanol, thus obtaining the second material.
[0063] S5, a combination of conductive carbon layer and ion conductor layer Add the tannic acid solution prepared in step S3 to the second material obtained in step S4, stir magnetically at 700 rpm for 4 hours, wash three times with anhydrous ethanol during the filtration process to remove unbound free components, and vacuum dry at 80°C for 3 hours to obtain the third material.
[0064] S6, Low-temperature carbonization coating The third material was placed in a tube furnace and heated to 280°C at a rate of 5°C / min. The temperature was maintained for 1 hour to partially carbonize the tannic acid. The material was then cooled to room temperature with the furnace under nitrogen protection to obtain a cathode material with ion / electron bifunctional coating, denoted as TA-C / Al@NCM.
[0065] Example 3 The process of coating NCM811 with LiNbO3 and conductive carbon material (GO-CNT), denoted as TA-C / Nb@NCM, is as follows: S1. Provide the same layered NCM811 cathode material matrix as in Example 1.
[0066] S2, Ion conductor layer coated positive electrode material matrix 800 mg of the positive electrode material matrix was weighed and measured using the same methods as in Example 1. The density of LiNbO3 was 4.64 g / cm³. 3 Based on the expected thickness requirement of 30 nm, 31.9 mg Nb₂O₅, 7.8 mg LiOH·H₂O, and 3 ml ethanol were added and mixed using a planetary ball mill at a ball-to-powder ratio of 2:1 at 300 rpm for 30 min. The mixture was then placed in a 30°C oven to evaporate the ethanol. Next, the resulting powder was placed in an oxygen atmosphere in a tube furnace and heated to 600°C at 5°C / min for 12 h, followed by furnace cooling to obtain the first material, denoted as Nb@NCM. The main chemical reaction occurring in step S2 is: 2LiOH + Nb₂O₅ = 2LiNbO₃ + H₂O.
[0067] S3, Preparation of Tannic Acid Solution 30 mg of tannic acid was dissolved in 3 ml of Tris-HCl solvent to obtain a uniformly dispersed orange-yellow solution with a pH of 7-8. The solution was stirred at room temperature for 10 min at a speed of 600 rpm.
[0068] S4, Addition of conductive carbon material The first material obtained in step S2 was mixed with the conductive carbon material, which was a mixture of 10 mg of graphene oxide and 2 mg of multi-walled carbon nanotubes. 3 ml of ethanol was added, and the mixture was mixed using a planetary ball mill with a ball-to-material ratio of 2:1 at 300 rpm for 30 min. The mixture was then placed in a 30°C oven to evaporate the ethanol, thus obtaining the second material.
[0069] S5, a combination of conductive carbon layer and ion conductor layer Add the tannic acid solution prepared in step S3 to the second material obtained in step S4, stir magnetically at 700 rpm for 4 hours, wash three times with anhydrous ethanol during the filtration process to remove unbound free components, and vacuum dry at 80°C for 3 hours to obtain the third material.
[0070] S6, Low-temperature carbonization coating The third material was placed in a tube furnace and heated to 280°C at a rate of 5°C / min. The temperature was maintained for 1 hour to partially carbonize the tannic acid. The material was then cooled to room temperature with the furnace under nitrogen protection to obtain a cathode material with ion / electron bifunctional coating, denoted as TA-C / Nb@NCM.
[0071] Comparative Example 1: Uncoated NCM811 The difference between Comparative Example 1 and Example 1 is that the layered NCM811 cathode material substrate was not coated, and is referred to as NCM. This cathode material is in direct contact with the electrolyte, which easily leads to side reactions and a decrease in cycle life.
[0072] Comparative Example 2: LiBO2-coated NCM811 (B@NCM) The difference between Comparative Example 2 and Example 1 is that conductive carbon material and tannic acid are not added. That is, Comparative Example 2 only includes steps S1 and S2 of Example 1, and a LiBO2 coating layer is formed after heat treatment in step S2. This coating layer has a certain interface protection effect, but the interface electron transport capability is relatively limited.
[0073] Comparative Example 3: LiAlO2-coated NCM811 (Al@NCM) The difference between Comparative Example 3 and Example 2 is that conductive carbon material and tannic acid are not added. That is, Comparative Example 3 only includes steps S1 and S2 of Example 2, and a LiAlO2 coating layer is formed after the heat treatment in step S2. This coating layer has a certain interface protection effect, but the interface electron transport capability is relatively limited.
[0074] Comparative Example 4: LiNbO3-coated NCM811 (Nb@NCM) The difference between Comparative Example 4 and Example 3 is that conductive carbon material and tannic acid are not added. That is, Comparative Example 4 only includes steps S1 and S2 of Example 3, and a LiNbO3 coating layer is formed after heat treatment in step S2. This coating layer has a certain interface protection effect, but the interface electron transport capability is relatively limited.
[0075] Comparative Example 5: Tannic acid and LiAlO2 coating of NCM811 (TA-Al@NCM) The difference between Comparative Example 5 and Example 2 is that no conductive carbon material is added.
[0076] The following tests were conducted on each embodiment and comparative example.
[0077] 1. Electrochemical performance testing Positive electrode sheets and coin cells were prepared using the positive electrode material samples obtained in Examples 1-3 and Comparative Examples 1-4.
[0078] (1) Preparation of positive electrode sheet The above-mentioned positive electrode material samples were each prepared into positive electrode sheets according to the following steps: First, 100 mg of binder (PVDF) was dissolved in 2400 mg of N-methylpyrrolidone (NMP), and the mixture was magnetically stirred at 600 rpm for 3 h at room temperature to obtain a 4 wt% PVDF solution; then, 800 mg of the positive electrode material sample and 100 mg of conductive agent (SP) were added, and the mixture was stirred at 700 rpm for 4 h to obtain a uniform positive electrode slurry. The positive electrode slurry was coated onto a 16 μm aluminum foil using a scraper to obtain a positive electrode sheet with a total thickness of 216 μm. The coated positive electrode sheet was first dried in a 60 ℃ forced-air drying oven for 30 min, and then transferred to a 110 ℃ vacuum drying oven for 12 h. After drying, the positive electrode sheet was cut into circular pieces with a diameter of 12 mm for later use.
[0079] (2) Button battery assembly A 15.6 mm diameter lithium metal sheet was used as the negative electrode, and a Celgard 2500 membrane with a diameter of 19 mm was used as the separator material. The electrolyte was 1.0 M LiPF6 dissolved in an EC / DMC mixed solvent with a 1:1 volume ratio. 15 μL of electrolyte was added to each battery. The batteries were assembled in the following order: negative electrode shell, spring contact, gasket, lithium sheet, separator, positive electrode plate, and positive electrode shell.
[0080] After the assembled batteries were left to stand for 12 hours, performance tests were conducted, including cycle capacity tests. The test steps are shown in Table 1. The effect of the composite coating on cycle stability was evaluated by comparing the cycle capacity retention rates of the examples and comparative examples.
[0081] Table 1 Figure 2a and 2b These are cycle performance graphs of batteries assembled from various cathode material samples, such as... Figure 2a As shown, compared to the unmodified NCM (Comparative Example 1), the capacity after 50 cycles at 1C was 125.95 mAh / g, and the coulombic efficiency was 68%. The modified TA-C / B@NCM, TA-C / Nb@NCM, and TA-C / Al@NCM in the examples all exhibited higher discharge specific capacity and more stable cycle retention, with capacities of 162.61, 179.07, and 171.61 mAh / g, and coulombic efficiencies of 98.8%, 98.58%, and 99.01%, respectively. Among them, TA-C / Nb@NCM showed the most outstanding capacity performance, maintaining a high specific capacity (179.07 mAh / g at 1C) after 50 cycles, indicating that the TA-C / LiNbO3 composite coating layer can effectively improve the material interface stability. In contrast, as... Figure 2bAs shown, while samples modified with only LiBO2, LiNbO3, or LiAlO2 can improve cycle performance to some extent, their overall capacity retention is lower than that of samples modified with TA-C synergistic modification. These results indicate that the carbon nanotube / graphene oxide conductive network constructed with tannic acid has a good synergistic effect with the ion-conducting layer, which not only helps improve electrode interface stability but also promotes electron / ion transport, thereby enhancing the cycle performance of NCM cathode materials.
[0082] 2. Sample Characterization like Figure 3 The image shows SEM morphology images of the cathode material samples from Examples 1-3 and Comparative Example 1. It can be seen that there are no obvious large particle agglomerates in each cathode sample.
[0083] XRD observation revealed the integrity of the layered cathode material and the ion mixing. Figure 4 The XRD phase diagrams are those of TA-C / Nb@NCM in Example 3 and NCM in Comparative Example 1. Figure 4 In the samples, both exhibited a typical α-NaFeO2 layered structure (R-3m space group), corresponding to diffraction peaks on the (003), (101), (006) / (102), (104), (015), (107), (108), and (110) crystal planes. The positions of each diffraction peak remained largely unchanged after coating, indicating that the in-situ coating process did not damage the main NCM crystal structure. Meanwhile, the (006) / (102) and (108) / (110) diffraction peaks remained clearly separated, indicating that the material still possesses a good layered ordered structure and high crystallinity. Furthermore, the (003) peak maintained a higher intensity ratio than the (104) peak, indicating that the Li⁺ / Ni 2+ The degree of cation mixing is low, and the layered structure of the layered cathode material matrix is stable. No characteristic diffraction peaks of ionic conductors were observed in the XRD pattern. Figures 5a-5c EDS and Figure 6 The Raman spectra were further used for characterization.
[0084] Figure 5a , 5b Figures 5 and 5c are EDS elemental distribution diagrams of TA-C / B@NCM from Example 1, TA-C / Al@NCM from Example 2, and TA-C / Nb@NCM from Example 3, respectively. The EDS results show that aluminum, niobium, and boron are uniformly distributed on the surface of the cathode material substrate.
[0085] pass Figure 6 Raman spectroscopy further characterized the composition of the ion conductor layers of Examples 1-3. Figure 6The Raman spectra of different modified samples showed significant differences. The TA-C / Al@NCM sample in Example 2 exhibited a strong vibrational peak in the approximately 560-660 cm⁻¹ region, which can be attributed to AlO₂. -1 The associated Al-O vibrational signals indicate that Al species were successfully introduced and participated in surface structure construction. The TA-C / B@NCM sample from Example 1 exhibited a broadened characteristic peak at approximately 820-880 cm⁻¹, corresponding to BO₂. -1 The vibrational modes of the functional groups indicate the formation of BO bond structures. NbO3 was observed in the TA-C / Nb@NCM sample of Example 3 at approximately 610 cm⁻¹ and 870-900 cm⁻¹. -1 The presence of Nb-O characteristic peaks confirms that Nb-based species have been effectively loaded onto the material surface. These results indicate that Al, B, and Nb modifications can all form corresponding metal / non-metal oxide bonding structures on the NCM surface, which helps to regulate the surface chemical environment of the cathode material matrix and improve interfacial stability, suggesting that the expected LiAlO2, LiNbO3, and Li3BO3 were formed during the heat treatment process.
[0086] Figure 7 As shown, Fourier transform infrared spectroscopy (FTIR) was used to detect the presence of tannic acid in the TA-C / Al@NCM samples of Example 2 and the TA-C / Nb@NCM samples of Example 3. Figure 7 As can be seen, both samples exhibit a broad absorption peak near 3413–3423 cm⁻¹, corresponding to the O–H stretching vibration. Tannic acid molecules contain numerous phenolic hydroxyl groups; therefore, this broad peak indicates the presence of abundant hydroxyl structures on the material surface, which can be attributed to the phenolic hydroxyl groups in tannic acid, and may also include a small contribution from adsorbed water. The absorption peak near 2973–2985 cm⁻¹ is attributed to the C–H stretching vibration, indicating the presence of an organic structure in the sample. The absorption peak near 1654–1664 cm⁻¹ can be attributed to aromatic ring skeletal vibrations (or C=C related vibrations), consistent with the galloyl aromatic structure in tannic acid. The absorption peak observed near 1457–1462 cm⁻¹ can also be attributed to aromatic ring skeletal vibrations, similarly indicating the presence of an aromatic organic structure in the sample. Furthermore, a distinct absorption peak was observed near 1236–1243 cm⁻¹, which can be attributed to the C–O–C / C–O stretching vibration. This is an important characteristic absorption region of phenolic hydroxyl groups and ester bonds in tannic acid molecules. In summary, a large number of functional groups, including hydroxyl groups, aromatic rings, and C–O bonds, were detected on the sample surface. The positions of their absorption peaks are consistent with the typical FTIR characteristics of tannic acid, indicating that tannic acid has been successfully introduced into the cathode material.
[0087] Figure 8The images show the SEM images and corresponding ESD spectra of TA-C / Al@NCM from Example 2. In the high-magnification SEM images, the size markings show that the composite coating layer is distributed at the nanoscale. The measured thicknesses of the composite coating layer at local magnifications are 29.57 nm and 37.58 nm, indicating the formation of a relatively thin composite coating layer on the surface of the NCM811 particles. Furthermore, the presence of the composite coating layer is further confirmed by the elemental composition of the NCM811 matrix. NCM811 is mainly composed of transition metal elements such as Ni, Co, and Mn, with atomic numbers of 28, 27, and 25 for Ni, Co, and Mn, respectively. In contrast, the atomic number of Al in LiAlO2 is 13, and the atomic numbers of Li and O are even lower. Therefore, in backscattered electron imaging, a significant difference in atomic number contrast occurs between LiAlO2 and the high-atomic-number NCM811 matrix. The difference in contrast between the heterogeneous regions on the particle surface and the matrix in the figure indicates the presence of low atomic number materials on the surface that differ from the NCM811 matrix. Meanwhile, Figure 8 A significant Al element signal was detected in the EDS spectrum, while NCM811 itself does not contain Al. Therefore, the Al signal should originate from the LiAlO2 coating layer. Combining the nanoscale coating thickness, the difference in backscattered contrast, and the Al element signal, it can be further proved that LiAlO2 has been successfully coated on the surface of the NCM811 cathode material.
[0088] like Figure 9a , 9bTable 9c shows SEM images of the cathode materials of Examples 1-3, used to measure the thickness of the composite coating layer. The thickness of the composite coating layer in Examples 1-3 was measured using ImageJ, and the results are shown in Table 2. Combining the SEM images and multi-point thickness statistics, it can be seen that nanoscale composite coating layers were formed on the surfaces of TA-C / B@NCM in Example 1, TA-C / Al@NCM in Example 2, and TA-C / Nb@NCM in Example 3. The composite coating layer thickness of TA-C / B@NCM in Example 1 is mainly distributed between 19.682-32.74 nm, with an average thickness of approximately 27.95 nm; the composite coating layer thickness of TA-C / Al@NCM in Example 2 is 29.24-37.58 nm, with an average thickness of approximately 32.17 nm; and the composite coating layer thickness of TA-C / Nb@NCM in Example 3 is 20.67-29.21 nm, with an average thickness of approximately 23.32 nm. This demonstrates that the method of the present invention can form a thin and continuous nanoscale organic-inorganic composite coating layer on the surface of NCM811. Specifically, the TA-C / Nb@NCM composite coating layer in Example 3 is relatively thin, while the composite TA-C / Al@NCM coating layer in Example 2 is slightly thicker, but all three are within a reasonable range of tens of nanometers. A coating layer of suitable thickness helps to isolate the electrolyte from direct contact with the NCM811 active material, suppressing surface side reactions, and also avoids increasing Li⁺ transport resistance due to an excessively thick composite coating layer, thereby improving the interfacial stability and cycle performance of the cathode material.
[0089] Table 2: Thickness of composite coating layer at different locations (6 locations were randomly selected) in the cathode material samples of Examples 1-3 To investigate the structural transformation of tannic acid and the formation of the composite carbon layer during low-temperature heat treatment, Raman spectroscopy analysis was performed on the TA-Al@NCM samples in Comparative Example 5 and the TA-C / Al@NCM samples in Example 2. Figure 10a and 10b As shown, both samples exhibit distinct D and G peaks at approximately 1350 cm⁻¹ and 1580 cm⁻¹, respectively, corresponding to the vibrational characteristics of defective / disordered sp² carbon structures and graphitized sp² carbon skeletons in carbon materials. This indicates that tannic acid undergoes dehydration condensation and aromatization processes after low-temperature heat treatment, forming oxygen-containing amorphous carbon with sp² carbon structures. Specifically, the I peak of the TA-Al@NCM sample in Comparative Example 5... D / I GThe value is 0.242, indicating that the oxygen-containing amorphous carbon formed by the partial heat treatment of tannic acid has a high degree of defect; after introducing conductive carbon materials (carbon nanotubes (CNTs) and graphene oxide (GO), the I of TA-C / Al@NCM in Example 2... D / I G The value is 0.237, which is basically consistent with TA-Al@NCM, indicating that the added conductive carbon material did not destroy the oxygen-containing amorphous carbon formed by the low-temperature heat treatment of tannic acid, but instead formed a stable composite carbon network together with the oxygen-containing amorphous carbon.
[0090] Furthermore, the TA-C / Al@NCM in Example 2 still maintained a significant D / G characteristic peak after washing, indicating that the conductive carbon component can stably exist in the composite coating layer, rather than being simply physically adsorbed onto the material surface. Combined with the abundant phenolic hydroxyl groups and aromatic structures in tannic acid molecules, it can promote the interfacial assembly between the inorganic ionic conductor and the conductive carbon material before heat treatment. After heat treatment, some of the tannic acid is further converted into oxygen-containing amorphous carbon, thereby enhancing the structural stability of the composite coating layer and promoting the construction of electron transport channels.
[0091] The above description provides a further detailed explanation of the present invention in conjunction with specific / preferred embodiments, and it should not be construed that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art, various substitutions or modifications can be made to these described embodiments without departing from the concept of the present invention, and all such substitutions or modifications should be considered within the scope of protection of the present invention. In the description of this specification, the reference to terms such as "an embodiment," "some embodiments," "preferred embodiment," "example," "specific example," or "some examples," etc., indicates that the specific features, structures, materials, or characteristics described in connection with that embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described can be combined in any suitable manner in one or more embodiments or examples. Without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification and the features of different embodiments or examples. Although the embodiments of the present invention and their advantages have been described in detail, it should be understood that various changes, substitutions, and modifications can be made herein without departing from the scope of protection of the patent application.
Claims
1. A positive electrode material, characterized in that, include: A layered lithium-containing cathode material matrix and a composite coating layer covering the layered lithium-containing cathode material matrix; the composite coating layer includes an ion conductor layer, a tannic acid bridging layer and a conductive carbon layer; The ion conductor layer is coated on the surface of the layered lithium-containing cathode material matrix and is a lithium salt formed by the in-situ reaction of the ion conductor precursor and the lithium source through a first heat treatment. The lithium source includes residual lithium compounds on the surface of the layered lithium-containing cathode material matrix. The tannic acid bridging layer is composed of tannic acid; The conductive carbon layer is formed by converting conductive carbon material and a portion of tannic acid through a second heat treatment. In the tannic acid bridging layer, the phenolic hydroxyl groups of tannic acid form coordination and hydrogen bonding with the metal elements on the surface of the ion conductor layer, and its aromatic ring forms π-π interactions with the surface of the conductive carbon material to promote the uniform adhesion of the conductive carbon material on the surface of the ion conductor layer, thereby the conductive carbon layer is stably bonded to the surface of the ion conductor layer.
2. The cathode material according to claim 1, characterized in that, The chemical formula of the layered lithium-containing cathode material matrix is LiNi. x Co y M 1-x-y O2, where 0.80≤x≤0.98, 0≤y≤0.20, and x+y<1, and M is at least one of Al, Mn, and Mg.
3. The cathode material according to claim 1, characterized in that, The ion conductor layer contains LiBO2 and Li3BO2. 3、 The lithium source includes at least one of LiNbO3, LiAlO2, LiPO3, and Li2SeO4; the lithium source also includes a supplementary lithium source, which includes at least one of LiOH·H2O, Li2CO3, LiNO3, CH3COOLi, and Li2O.
4. The cathode material according to claim 1, characterized in that, The conductive carbon material comprises at least one of graphene, graphene oxide, reduced graphene oxide, carbon nanotubes, carbon fibers, and conductive carbon black; based on the mass of the layered lithium-containing cathode material matrix, the content of tannic acid is 0.01-5 wt%, and the content of the conductive carbon material is 0.01-5 wt%.
5. A method for preparing a cathode material as described in any one of claims 1 to 4, characterized in that, Includes the following steps: S1. Provides a layered lithium-containing cathode material matrix; S2. The ion conductor precursor is mixed with the layered lithium-containing cathode material matrix and subjected to a first heat treatment in an oxygen-containing atmosphere, so that the ion conductor precursor reacts in situ with the residual lithium compounds on the surface of the layered lithium-containing cathode material matrix, and the ion conductor layer is coated on the surface of the layered lithium-containing cathode material matrix to obtain the first material. S3. Dissolve tannic acid in a buffer solvent to prepare a uniformly dispersed tannic acid solution; S4. Mix the conductive carbon material with the first material to obtain the second material; S5. The second material is mixed and stirred with the tannic acid solution to bridge the tannic acid molecules between the ion conductor layer and the conductive carbon material. After filtration, washing and drying, the third material is obtained. S6. The third material is subjected to a second heat treatment under an inert atmosphere. During the second heat treatment, the tannic acid undergoes partial carbonization and conversion into a poly(p-containing) form. 2 Oxygen-containing amorphous carbon with a carbon structure is used to form a composite carbon network together with the conductive carbon material to form a conductive carbon layer, thereby obtaining the cathode material.
6. The method according to claim 5, characterized in that, In step S2, the temperature of the first heat treatment is 300-750℃ and the heat treatment time is 6-12h; in step S6, the temperature of the second heat treatment is 150-350℃ and the heat treatment time is 1-2h.
7. The method according to claim 5, characterized in that, Step S2 further includes adding a lithium source, wherein the lithium source includes at least one of LiOH·H2O, Li2CO3, LiNO3, CH3COOLi, and Li2O; Step S2 includes: mixing the ion conductor precursor with the layered lithium-containing cathode material matrix and the lithium source, and performing a first heat treatment, so that the ion conductor precursor reacts in situ with the residual lithium compounds on the surface of the layered lithium-containing cathode material matrix and the lithium source, thereby coating the surface of the layered lithium-containing cathode material matrix with an ion conductor layer to obtain a first material.
8. The method according to claim 5, characterized in that, In step S4, the conductive carbon material is a mixture of graphene oxide and multi-walled carbon nanotubes. Based on the mass of the layered lithium-containing cathode material matrix, the amount of graphene oxide added is 0.5-2 wt%, and the amount of multi-walled carbon nanotubes added is 0.5-5 wt%. The mixing in step S4 is carried out using a planetary ball mill with anhydrous ethanol as the medium, a ball-to-material ratio of 2:1-5:1, a rotation speed of 100-300 rpm, and a mixing time of 10-30 min.
9. A positive electrode sheet, characterized in that, The cathode material includes any one of claims 1 to 4.
10. A lithium-ion battery, characterized in that, Includes the positive electrode sheet as described in claim 9.
Citation Information
Patent Citations
Modified positive electrode material and preparation method therefor, and positive electrode sheet
WO2025107725A1