A salt anion-mediated copper single-atom doped MOF-derived carbon material, its preparation method and application
By using copper single-atom doped MOF-derived carbon materials mediated by salt anions, the problems of large thickness, poor impedance matching, and limited dielectric properties of traditional microwave absorbing materials have been solved. This has achieved a multi-functional effect of wide-bandwidth electromagnetic wave absorption and antibacterial protection, and is suitable for fields such as intelligent medical monitors, hospital air purification, precision electronic instruments, and electromagnetic radiation protective clothing.
Patent Information
- Application Number
- CN202611400698.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-10
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-09-10
AI Technical Summary
Traditional ferrite and metal powder absorbing materials have large thickness, poor impedance matching, and narrow bandwidth; carbon-based materials have limited dielectric properties, making it difficult to balance impedance matching and attenuation; heteroatom doping strategies have poor controllability and cannot precisely regulate active sites; and they have limited functionality and lack comprehensive protection capabilities such as antibacterial properties, making it difficult to meet the multifunctional needs in complex electromagnetic environments.
A method for preparing copper single-atom doped MOF-derived carbon materials using salt anion-mediated doping is employed. By employing a salt anion-mediated doping strategy, the second-shell coordination of copper active sites is precisely adjusted and the electronic configuration of the microwave absorbing material is optimized, resulting in a spindle-shaped carbon matrix with nitrogen-doped carbon layer coating and cobalt nanoparticle embedding, exhibiting excellent microwave absorption performance.
The material achieves high-efficiency electromagnetic wave absorption performance, has a wide bandwidth and excellent antibacterial properties, has a simple synthesis route and is suitable for large-scale production, and is applicable to multifunctional electromagnetic compatibility and antibacterial applications.
Smart Images

Figure CN122897394B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electromagnetic materials technology, and particularly relates to a copper single-atom doped MOF-derived carbon material mediated by salt anions, its preparation method and application. Background Technology
[0002] With the rapid development of the 5G / 6G era, wireless communication devices have been widely used, accompanied by the continuous increase in electromagnetic waves (EMW) and the growing severity of electromagnetic pollution. Excessive electromagnetic exposure poses potential health risks to humans, such as impaired sleep quality, cumulative bioelectromagnetic effects, and tissue damage. Furthermore, strong electromagnetic waves can disrupt the normal operation of nearby electronic devices and cause signal loss or interruption. To address these issues, high-performance electromagnetic wave absorbing (EMA) materials have been extensively explored. The main goal is to achieve lightweight, thin, and highly efficient EMA absorbing materials.
[0003] Traditional EMA materials, represented by ferrite ceramics and metal powders, have been widely developed and utilized due to their inherent magnetic attenuation capabilities. However, these traditional absorbing materials suffer from serious drawbacks, including large thickness, poor impedance matching, narrow effective absorption bandwidth, and insufficient loss capability, which limit their practical applications. To overcome these limitations, carbon-based magnetic materials are considered an ideal alternative to traditional single-component absorbing materials.
[0004] Carbon-based materials possess significant advantages such as high conductivity, low density, and high-temperature stability. Furthermore, carbon-magnetic composite structures, formed by combining carbon materials with magnetic components, can effectively couple magnetic and dielectric loss mechanisms, thereby improving electromagnetic attenuation (EMA) performance. Metal-organic frameworks (MOFs) have been extensively explored as ideal precursors for the controllable preparation of high-performance carbon magnetic materials. Benefiting from their high surface area, tunable active sites, and controllable structure, MOFs can solve the problem of magnetic metal particle agglomeration during high-temperature pyrolysis, achieving uniform particle dispersion. Moreover, pyrolysis treatment can further optimize the microstructure and electronic properties of MOF-based materials, significantly improving their electromagnetic attenuation capability. However, traditional MOF-derived carbon materials still have limitations in dielectric property control, making it difficult to balance impedance matching characteristics and electromagnetic attenuation constants to adapt to complex electromagnetic environments. To overcome this limitation, targeted modification of the carbon layer is an effective strategy for precisely controlling dielectric parameters and optimizing absorption performance.
[0005] In recent years, single-atom doping engineering has become a cutting-edge modification strategy for high-efficiency electromagnetic absorbing (EMA) materials due to its theoretical 100% atomic utilization, uniformly dispersed atomic-level active sites, and unique electronic modulation characteristics. Experimental characterization and theoretical calculations have confirmed that single metal atoms anchored on a carbon matrix lead to a redistribution of local charges, thereby improving dielectric decay performance. However, anchored single atoms have limitations in the tunability of their intrinsic electronic states, hindering further optimization of charge polarization and electromagnetic decay capabilities. Coordination modulation can precisely adjust the local electronic environment around the metal active sites to enhance EMA performance. Currently, common heteroatom doping strategies include post-processing, vapor-phase doping, and in-situ doping during synthesis, but these conventional methods typically require additional dopants and complex operational procedures. Furthermore, these methods struggle to precisely control the atomic coordination of active sites, limiting the controllable design of high-performance electromagnetic wave absorbing materials. Summary of the Invention
[0006] The technical problems solved by this invention are: traditional ferrite and metal powder absorbing materials have large thickness, poor impedance matching and narrow bandwidth; the dielectric properties of carbon-based materials are limited, making it difficult to balance impedance matching and attenuation; the controllability of heteroatom doping strategies is poor, making it impossible to precisely control active sites; and they have single functions and lack comprehensive protection capabilities such as antibacterial properties, making it difficult to meet the multifunctional needs in complex electromagnetic environments.
[0007] In view of the technical problems existing in the prior art, this invention designs a salt anion-mediated copper single-atom doped MOF-derived carbon material, its preparation method, and its application. This invention utilizes a salt anion-mediated doping strategy to precisely adjust the second-shell coordination of copper active sites and optimize the electronic configuration of the microwave absorbing material. By uniformly incorporating atomic copper sites and chlorine / sulfur heteroatoms, a spindle-shaped carbon matrix with nitrogen-doped carbon layer coating and cobalt nanoparticle embedding, exhibiting excellent microwave absorption performance, was successfully prepared.
[0008] It should be noted that, in this invention, unless otherwise specified, the specific meaning of "comprising" in relation to composition definition and description includes both open-ended meanings such as "comprising," "including," etc., and closed-ended meanings such as "composed of," etc., and similar meanings.
[0009] To solve the aforementioned technical problems, the present invention adopts the following solution: [First technical solution] A method for preparing copper single-atom-doped MOF-derived carbon materials mediated by salt anions includes the following steps: Step 1: Preparation of Co-MOF precursors Cobalt salt solution and 2-methylimidazole solution were prepared by dissolving cobalt salt and 2-methylimidazole in solvents, respectively. Cobalt salt solution was added to 2-methylimidazole solution, the reaction was stirred, and the mixture was centrifuged, washed, and dried to obtain the Co-MOF precursor. Step 2: Polydopamine coating and heteroatom modification The Co-MOF precursor obtained in step 1 was dispersed in a solvent to obtain a Co-MOF dispersion; Dopamine hydrochloride was dissolved in a buffer solution, and copper salt was added to it to obtain a dopamine hydrochloride solution containing copper salt. Add the copper salt-containing dopamine hydrochloride solution to the Co-MOF dispersion and adjust the pH to alkaline. The reaction was stirred, centrifuged, washed, and dried to complete the polydopamine coating and heteroatom modification, yielding a copper-doped PDA@Co-MOF intermediate. Step 3: Preparation of copper single-atom doped MOF-derived carbon materials mediated by salt anions The copper-doped PDA@Co-MOF intermediate obtained in step 2 was subjected to high-temperature carbonization under an inert atmosphere. After natural cooling, the product was collected to obtain the copper single-atom-doped MOF-derived carbon material mediated by the salt anion.
[0010] Furthermore, in step 1, the cobalt salt is at least one of cobalt acetate, cobalt nitrate, or cobalt chloride; The molar ratio of cobalt salt to 2-methylimidazole is 1:6-10; The stirring reaction time is 2-8 hours, and the reaction temperature is 10-30℃.
[0011] Furthermore, in step 2, the copper salt is at least one of copper nitrate, copper chloride, or copper sulfate; The mass ratio of Co-MOF precursor to dopamine hydrochloride is 4-7:3; The mass ratio of copper salt to dopamine hydrochloride is 0.03-0.06:1.
[0012] Furthermore, in step 2, the solvent used to disperse the Co-MOF precursor is a solvent prepared by mixing ethanol and ultrapure water at a volume ratio of 7:3. The buffer solution for dissolving dopamine hydrochloride is Tris-HCl buffer, and the solution is alkaline; The stirring reaction time is 12-24 hours.
[0013] Furthermore, in step 3, the high-temperature carbonization temperature is 600-900℃; The heat preservation time for high-temperature carbonization is 1-4 hours.
[0014] Furthermore, in step 3, the heating rate for high-temperature carbonization is 1-10℃ / min.
[0015] Furthermore, in step 3, the inert atmosphere is argon or nitrogen.
[0016] In this invention, the efficient synthetic route does not require additional heteroatom-containing chemicals and can flexibly adjust the second shell coordination environment for anchoring single atoms.
[0017] First, a spindle-shaped Co-MOF precursor was prepared by a simple co-precipitation strategy.
[0018] Subsequently, a uniform polydopamine coating is grown on the Co-MOF surface, during which copper salt-derived copper species and anionic heteroatoms are introduced into the composite system. After pyrolysis, the magnetic Co particles can be well embedded in the N-doped carbon matrix, while the external PDA-derived carbon layer achieves co-doping of Cu single atoms and anions.
[0019] Introducing Cu single atoms into a carbon matrix effectively optimizes the dielectric properties of MOF-derived spindle-shaped materials, thereby improving EMW attenuation performance.
[0020] This invention constructs a core-shell structure with magnetic Co particles embedded in an N-doped carbon matrix and an external PDA-derived carbon layer co-doped with Cu single atoms and anions through a three-step method of Co-MOF precursor + PDA coating + high-temperature carbonization, thereby achieving a synergistic effect of magnetic loss and dielectric decay.
[0021] Furthermore, the doped anions further modulate the electronic structure of Cu atoms. Therefore, MOF-derived magneto-dielectric synergistic materials can achieve minimal reflection loss and the widest effective absorption bandwidth.
[0022] [Second Technical Solution] A salt anion-mediated copper single-atom doped MOF-derived carbon material is prepared according to the above-described preparation method.
[0023] Furthermore, the copper single-atom doped MOF-derived carbon material has a core-shell structure, with Co particles embedded in an N-doped carbon matrix inside and a carbon layer co-doped with Cu single atoms and anions on the outside. In the copper single-atom doped MOF-derived carbon material, Cu is dispersed in the carbon matrix in the form of single atoms; The copper single-atom doped MOF-derived carbon material has a spindle-shaped morphology.
[0024] [Third technical solution] The use of the above-mentioned salt anion-mediated copper single-atom doped MOF-derived carbon material in the preparation of electromagnetic wave absorbing materials and / or antibacterial materials.
[0025] The specific applications of the materials of this invention are illustrated by examples. These applications can be adjusted according to specific circumstances and are not limited to the scenarios described below: Firstly, the radiation-proof packaging of intelligent medical monitors. For devices that come into close contact with the skin, such as health monitoring patches, materials can be incorporated into silicone or textile fibers to create flexible absorbing pads or fabric components. These not only attenuate the near-field electromagnetic radiation generated by the devices but also inhibit the growth of pathogens on the skin surface, achieving integrated "radiation protection + antibacterial" protection.
[0026] Secondly, air purification filters for high-risk environments within hospitals. The material is loaded onto polypropylene or nonwoven fibers to create a multi-layer filter for use in ventilation systems or portable air purifiers. On one hand, the porous carbon layer adsorbs harmful gases from the air; on the other hand, the material catalyzes the generation of active oxygen in humid airflow, effectively inactivating airborne bacteria, making it suitable for operating rooms and other environments with strict microbial control requirements.
[0027] Third, electromagnetic compatibility (EMC) absorbing pads inside precision electronic instruments. In the confined space between RF modules and high-speed digital circuit boards, materials can be mixed with polymers and injection molded into gaskets or films of specific shapes, which are then filled between the chip and the shielding cover. Utilizing their excellent impedance matching characteristics, these materials suppress multiple reflections of high-frequency harmonics within the cavity, preventing signal crosstalk.
[0028] Fourth, antibacterial medical device surface coatings This material can be applied to the surfaces of urinary catheters, wound dressings, and surgical instruments via dip coating or spin coating. The carbon-based film formed after drying exerts antibacterial effects in the physiological environment without the risk of drug resistance, making it particularly suitable for preventing nosocomial infections such as catheter-related bloodstream infections.
[0029] Fifth, electromagnetic radiation protective clothing and smart textile fabrics. By incorporating materials as functional fillers into polyester or nylon spinning solutions, fibers with wave-absorbing properties are prepared, which are then woven into fabrics. This type of protective clothing can be worn by personnel at radar stations and high-voltage power line inspection stations. It can attenuate environmental electromagnetic waves and inhibit bacterial growth in sweat through its antibacterial properties, improving both comfort and hygiene.
[0030] The mechanism by which this invention can achieve successful preparation is as follows: The successful preparation of this invention relies on a three-step synergistic mechanism of “Co-MOF template induction + PDA coating confinement + high-temperature carbonization conversion”.
[0031] First, Co-MOFs, as precursors, possess high specific surface area, tunable active sites, and controllable structure, effectively suppressing the aggregation of magnetic Co particles during high-temperature pyrolysis and achieving uniform particle dispersion. Co-MOFs prepared by the co-precipitation method exhibit a spindle-shaped structure, providing an ideal template for the subsequent construction of core-shell structures.
[0032] Secondly, the introduction of a polydopamine (PDA) coating is crucial. PDA can be uniformly polymerized and grown on the Co-MOF surface to form a core-shell structure. During this process, copper species derived from copper salts and anionic heteroatoms are simultaneously introduced into the composite system. The PDA coating not only serves as a carbon and nitrogen source, but more importantly, it plays a "confined anchoring" role—restricting copper ions within the PDA layer and preventing them from migrating and agglomerating during subsequent high-temperature carbonization.
[0033] Finally, high-temperature carbonization achieved a triple transformation: (1) the Co-MOF core was transformed into magnetic Co particles embedded in an N-doped carbon matrix; (2) the PDA shell was transformed into an N-doped carbon layer; and (3) copper species were uniformly dispersed in single-atom form under the confinement of the carbon layer. This differentiated design of "core transformation + shell doping" is the key to the successful preparation of copper single-atom doped MOF-derived carbon materials in this invention.
[0034] The mechanism by which this invention has unique and superior effects lies in:
[0035] The unique effect of this invention originates from a triple synergistic mechanism of "magnetic dielectric synergy + single-atom regulation + anion coordination".
[0036] First, the synergistic effect of magneto-dielectric properties. After high-temperature carbonization, the magnetic Co particles in the core provide magnetic loss capability, while the N-doped carbon layer in the outer shell provides dielectric loss capability (dipole polarization and interfacial polarization). The synergistic effect between the two significantly enhances the electromagnetic wave attenuation capability. The formation of numerous heterogeneous interfaces in the MOF-derived porous carbon matrix further promotes interfacial polarization loss.
[0037] Second, the dielectric modulation effect of copper single atoms. The embedding of Cu single atoms into a carbon matrix leads to a redistribution of local charges among surrounding atoms, improving conductivity, dipole moment, and dielectric decay performance. Both experimental characterization and theoretical calculations confirm that the introduction of Cu single atoms can induce charge redistribution and improve conductivity, thereby optimizing impedance matching and dielectric loss. Simultaneously, single-atom doping achieves 100% atomic utilization, with each Cu atom becoming an effective active site.
[0038] Third, the electronic structure modulation effect of anions. Doped anions further modulate the electronic structure of Cu atoms. The introduction of different anions can change the second-shell coordination environment of Cu single atoms, thereby finely controlling the dielectric parameters of the material and ultimately achieving an optimized balance between impedance matching and attenuation constant.
[0039] Fourth, excellent antibacterial effect. The antibacterial performance is attributed to the electronic modulation of Cu single-atom sites through second-shell coordination modification. S / Cl heteroatom doping rearranges the coordination environment of the Cu active center, constructing a structure with asymmetric charge distribution and electron-rich active sites. Thanks to the optimized electronic configuration, peroxidase-like catalytic activity and glutathione consumption capacity are enhanced. This promotes the efficient generation of cytotoxic reactive oxygen species, ultimately disrupting bacterial membrane integrity and endowing the material with excellent antibacterial properties.
[0040] This invention provides a salt anion-mediated copper single-atom doped MOF-derived carbon material, its preparation method, and its application, which have the following beneficial effects: 1. This invention uses a salt anion-mediated doping strategy to precisely introduce Cu single atoms and anions (Cl or S) into a carbon matrix, achieving 100% atomic utilization and overcoming the poor controllability of traditional doping methods.
[0041] 2. The material synthesized in this invention has reliable antibacterial activity. The released copper ions can destroy the cell membrane of microorganisms and inhibit bacterial proliferation, giving the material the dual functions of electromagnetic radiation inhibition and antibacterial protection.
[0042] 3. This invention presents a simple salt anion-mediated doping synthesis method that does not require additional heteroatom-containing chemical substances. The synthesis route is efficient and easy to operate, making it suitable for large-scale production and promising for application in advanced electronic devices. Attached Figure Description
[0043] Figure 1 This is a schematic diagram of the preparation process of copper single-atom doped MOF-derived carbon material mediated by salt anion in Example 1 of the invention; Figure 2 The images show the scanning electron microscope (SEM) morphology of a) Co-MOF precursor, b) PDA@Co-MOF intermediate, and c) CoCu@SNC material prepared in Example 1 of this invention, and the transmission electron microscope (TEM) morphology of d) Co-MOF material. Figure 3 : Elemental valence and coordination characteristics of the salt anion-mediated copper single-atom doped MOF-derived carbon material prepared in Example 1 of this invention; CoCu@NC, copper foil, CuO, and Cu2O a) normalized Cu K-edge XANES spectrum and b) FT-EXAFS spectrum in R space; experimental and fitted EXAFS spectra of CoCu@NC in c) K space and d) R space; e) WT contour plots of CoCu@NC, copper foil, and CuO; Figure 4: 3D plots of reflection loss curves of a) Co@NC, b) CoCu@ClNC and c) CoCu@SNC prepared in Comparative Example 1 and Examples 1-3 of the present invention; 3D plots of impedance matching of d) Co@NC, e) CoCu@ClNC and f) CoCu@SNC. Figure 5 The figure shows the antibacterial activity test results of the Co@NC, CoCu@ClNC and CoCu@SNC materials prepared in Examples 1-3 of this invention against a) Escherichia coli and b) Staphylococcus aureus. Detailed Implementation
[0044] The present invention will be further described below with reference to specific embodiments and accompanying drawings: Regarding the materials used in the embodiments of this invention: Dopamine hydrochloride (DA, 98%), cobalt acetate tetrahydrate (Co(CH3COO)2•4H2O, 99.5%), copper nitrate hydrate (Cu(NO3)2•xH2O, AR grade) and ethanol (95%) were purchased from Maclin.
[0045] 2-Methylimidazole (2-MeIm, 98%), copper chloride (CuCl2, 98%), and Tris hydrochloride buffer (1M, pH 8.5) were supplied by Aladdin. Copper sulfate (CuSO4, 99%) was purchased from Sigma-Aldrich. All reagents were used directly without further purification. Example 1
[0046] Step 1. Preparation of Co-MOF precursor
[0047] In this invention, Co-MOF is prepared by co-precipitation.
[0048] Under continuous magnetic stirring, 0.01 mol of cobalt acetate tetrahydrate and 0.08 mol of 2-MeIm were dissolved in 30 mL and 200 mL of distilled water, respectively, to prepare cobalt salt solution and 2-methylimidazole solution.
[0049] Then, the cobalt acetate tetrahydrate solution was added to the 2-MeIm solution and stirred at room temperature for 4 hours. The resulting product was centrifuged at 5000 rpm for 15 minutes at 30°C, washed twice with distilled water, dried and collected to obtain the Co-MOF precursor.
[0050] Step 2. Polydopamine (PDA) coating and heteroatom modification
[0051] First, 0.5 g of the Co-MOF prepared in step 1 was dispersed in 70 mL of ethanol / ultrapure water (v / v=7:3).
[0052] Meanwhile, under ultrasonic treatment, 0.3 g of dopamine hydrochloride was dissolved in 20 mL of 10 mmol / L Tris buffer (100-fold dilution of the 1M original solution).
[0053] For copper-doped samples, 9 mg of Cu(NO3)2 was added separately to a Tris solution containing PDA.
[0054] The PDA-Tris solution was then added to the Co-MOF suspension. The total volume of the mixed suspension was brought to 100 mL using ultrapure water and the original Tris solution, while maintaining the final Tris concentration at 10 mM.
[0055] After stirring for 12 hours, the mixture was centrifuged at 6500 rpm for 10 minutes at 10°C, washed with ethanol, and dried. The polydopamine coating and heteroatom modification were completed, yielding a copper-doped PDA@Co-MOF intermediate.
[0056] Step 3. Preparation of copper single-atom-doped MOF-derived carbon materials mediated by salt anions
[0057] The copper-doped PDA@Co-MOF precursor obtained in step 2 was subjected to high-temperature pyrolysis in a tube furnace under an argon atmosphere.
[0058] The coated sample was heated to 800°C at a rate of 5°C / min, held at that temperature for 2 hours, and then naturally cooled to room temperature under a continuous argon flow.
[0059] When the copper salt is copper nitrate, a Cu-doped material is obtained (Cu(NO3)2-derived Cu doping), denoted as CoCu@NC. Example 2
[0060] While keeping all other experimental steps the same as in Example 1, step 2 of that example... For copper-doped samples, 9 mg of Cu(Cl)2 was added separately to a Tris solution containing PDA.
[0061] When the copper salt is copper chloride, a Cu / Cl co-doped material is obtained (Cu / Cl co-doped material derived from CuCl2), denoted as CoCu@ClNC; Example 3
[0062] While keeping all other experimental steps the same as in Example 1, step 2 of that example... For copper-doped samples, 9 mg of CuSO4 was added separately to a Tris solution containing PDA.
[0063] When the copper salt is copper sulfate, a Cu / S co-doped material is obtained (Cu / S co-doped material derived from CuSO4), denoted as CoCu@SNC.
[0064] Comparative Example 1
[0065] While keeping all other experimental steps the same as in Example 1, only the step of adding copper sample in step 2 was omitted, i.e., no copper salt was added, and the resulting powder was collected and named Co@NC. Example 4
[0066] Step 1. Preparation of Co-MOF precursor
[0067] In this invention, Co-MOF is prepared by co-precipitation.
[0068] Under continuous magnetic stirring, 0.01 mol of cobalt acetate tetrahydrate and 0.06 mol of 2-MeIm were dissolved in 30 mL and 200 mL of distilled water, respectively, to prepare cobalt salt solution and 2-methylimidazole solution.
[0069] Then, the cobalt acetate tetrahydrate solution was added to the 2-MeIm solution and stirred at room temperature for 2 hours. The resulting product was centrifuged at 5000 rpm for 15 minutes at 25°C, washed twice with distilled water, dried and collected to obtain the Co-MOF precursor.
[0070] Step 2. Polydopamine (PDA) coating and heteroatom modification
[0071] First, 0.4 g of the Co-MOF prepared in step 1 was dispersed in 70 mL of ethanol / ultrapure water (v / v=7:3).
[0072] Meanwhile, under ultrasonic treatment, 0.3 g of dopamine hydrochloride was dissolved in 20 mL of 10 mmol / L Tris buffer (100-fold dilution of the 1M original solution).
[0073] For copper-doped samples, 18 mg of Cu(NO3)2 was added separately to a Tris solution containing PDA.
[0074] The PDA-Tris solution was then added to the Co-MOF suspension. The total volume of the mixed suspension was brought to 100 mL using ultrapure water and the original Tris solution, while maintaining the final Tris concentration at 10 mM.
[0075] After stirring for 15 hours, the mixture was centrifuged at 6500 rpm for 10 minutes at 10°C, washed with ethanol, and dried. The polydopamine coating and heteroatom modification were completed, yielding a copper-doped PDA@Co-MOF intermediate.
[0076] Step 3. Preparation of copper single-atom-doped MOF-derived carbon materials mediated by salt anions
[0077] The copper-doped PDA@Co-MOF intermediate obtained in step 2 was subjected to high-temperature pyrolysis in a tube furnace under an argon atmosphere.
[0078] The coated sample was heated to 600℃ at a rate of 1℃ / min, held at this temperature for 4 hours, and then naturally cooled to room temperature under a continuous argon flow to obtain copper single-atom doped MOF-derived carbon material. Example 5
[0079] Step 3. Preparation of copper single-atom-doped MOF-derived carbon materials mediated by salt anions
[0080] In this invention, Co-MOF is prepared by co-precipitation.
[0081] Under continuous magnetic stirring, 0.01 mol of cobalt acetate tetrahydrate and 0.1 mol of 2-MeIm were dissolved in 30 mL and 200 mL of distilled water, respectively, to prepare cobalt salt solution and 2-methylimidazole solution.
[0082] Then, the cobalt acetate tetrahydrate solution was added to the 2-MeIm solution and stirred at room temperature for 8 hours. The resulting product was centrifuged at 5000 rpm for 15 minutes at 10 °C, washed twice with distilled water, dried and collected to obtain the Co-MOF precursor.
[0083] Step 2. Polydopamine (PDA) coating and heteroatom modification
[0084] First, 0.7g of the Co-MOF prepared in step 1 was dispersed in 70mL of ethanol / ultrapure water (v / v=7:3).
[0085] Meanwhile, under ultrasonic treatment, 0.3 g of dopamine hydrochloride was dissolved in 20 mL of 10 mmol / L Tris buffer (100-fold dilution of the 1M original solution).
[0086] For copper-doped samples, 15 mg of Cu(NO3)2 was added separately to a Tris solution containing PDA.
[0087] The PDA-Tris solution was then added to the Co-MOF suspension. The total volume of the mixed suspension was brought to 100 mL using ultrapure water and the original Tris solution, while maintaining the final Tris concentration at 10 mM.
[0088] After stirring for 24 hours, the mixture was centrifuged at 6500 rpm for 10 minutes at 10°C, washed with ethanol, and dried. This completed the polydopamine coating and heteroatom modification, yielding a copper-doped PDA@Co-MOF precursor.
[0089] Step 3. Preparation of copper single-atom-doped MOF-derived carbon materials mediated by salt anions
[0090] The copper-doped PDA@Co-MOF intermediate obtained in step 2 was subjected to high-temperature pyrolysis in a tube furnace under an argon atmosphere.
[0091] The coated sample was heated to 900℃ at a rate of 10℃ / min, held at this temperature for 1 hour, and then naturally cooled to room temperature under a continuous argon flow to obtain copper single-atom doped MOF-derived carbon material.
[0092] Regarding performance testing and explanation:
[0093] Regarding characterization methods
[0094] Morphological observation was performed using scanning electron microscopy (SEM, Thermo-science Apreo 2S) and field emission transmission electron microscopy (TEM, Talos-F200S).
[0095] X-ray absorption spectroscopy (XAS) measurements were performed at Beamline 07A1 of the Taiwan Light Source (TLS).
[0096] Regarding electromagnetic performance testing:
[0097] Electromagnetic parameters Co@NC were measured in the 2–18 GHz frequency range using a vector network analyzer (VNA, Agilent E5071C, USA) with the coaxial method.
[0098] Co@NC mixed the material with paraffin at a mass ratio of 35 wt%, and then compressed the mixture into a ring-shaped specimen with an outer diameter of 7.00 mm, an inner diameter of 3.04 mm, and a thickness of 2 mm. The reflection loss (RL) was calculated using the following equation based on transmission line theory: (1) (2) Among them, Z in Z0 and Z0 represent the input impedance and free space impedance (377Ω), respectively; ε r =ε'-jε” and μr=μ'-jμ” are the complex permittivity and complex permeability, respectively; f is the frequency of EMW; d is the thickness of the absorbing material; c is the speed of light in vacuum.
[0099] Regarding antibacterial activity testing:
[0100] Co@NC uses Escherichia coli and Staphylococcus aureus as model bacteria to evaluate materials, and uses the plate count method to quantify bacterial survival rate.
[0101] Bacteria were co-cultured with different complexes, with untreated bacteria serving as a control group. After incubation, the bacterial suspensions were spread on agar plates and incubated at 37°C for 24 hours, after which the number of viable colonies was counted.
[0102] Further comparison can be made using the accompanying diagrams in the instruction manual: Figure 1 This is a schematic diagram of the preparation process of copper single-atom doped MOF-derived carbon material mediated by salt anion in Example 1 of the present invention; from Figure 1 As can be seen, the preparation process of the material of the present invention mainly consists of three steps: First, a Co-MOF precursor with a spindle-shaped morphology is prepared by co-precipitation using cobalt salt and 2-methylimidazole as raw materials; second, a polydopamine coating is coated on the surface of Co-MOF under weakly alkaline conditions, and copper salt and anions are introduced simultaneously during the coating process to form a PDA@Co-MOF intermediate product; finally, high-temperature carbonization is carried out under an inert atmosphere to obtain the final product. Figure 1 The complete transformation pathway from Co-MOF precursor to salt anion-mediated copper single-atom doped MOF-derived carbon materials is clearly demonstrated.
[0103] Figure 2 The images show the scanning electron microscope (SEM) morphology of a) Co-MOF precursor, b) PDA@Co-MOF intermediate and c) CoCu@SNC material prepared in Example 1 of this invention, and the transmission electron microscope (TEM) morphology of d) Co-MOF precursor and c) CoCu@SNC material. from Figure 2 It can be seen that the prepared Co-MOF precursor exhibits a regular spindle-shaped morphology. Figure 2 Part a). After being coated with PDA ( Figure 2 In part b), the surface roughness of the material increases, but the overall spindle-shaped skeletal structure is well preserved. Further high-temperature carbonization treatment ( Figure 2 (Part c) The CoCu@SNC material still maintains the spindle morphology of the precursor, indicating that the synthesis route has good controllability over the morphology. Figure 2 A distinct core-shell structure can be observed in the middle d section, where the dark area consists of magnetic Co nanoparticles embedded in a nitrogen-doped carbon matrix, and the light area consists of a carbon outer shell layer co-doped with Cu single atoms and anions.
[0104] Figure 3The image shows the elemental valence and coordination characteristics of the salt anion-mediated copper single-atom doped MOF-derived carbon material prepared in Example 1 of this invention; a) normalized Cu K-edge XANES spectrum and b) FT-EXAFS spectrum in R space for CoCu@NC, copper foil, CuO, and Cu2O; experimental and fitted EXAFS spectra of CoCu@NC in c) K space and d) R space; e) WT contour plots of CoCu@NC, copper foil, and CuO. from Figure 3 It can be seen that, compared with metallic copper foil, the Cu K-edge XANES spectrum of the CoCu@NC sample shows a slight shift towards higher absorption energies. Figure 3 Part a) reveals a significant interfacial electron transfer between Cu and nitrogen atoms. The absorption edge energy of CoCu@NC is between that of CuO and Cu2O, indicating that the average valence state of Cu in this sample is between +1 and +2.
[0105] like Figure 3 Part b shows that CoCu@NC exhibits a prominent peak at approximately 1.53 Å, which likely corresponds to the first-shell coordination scattering signal of Cu sites. This peak is located between the peaks of CuO and Cu₂O. Simultaneously, CoCu@NC shows no Cu-Cu scattering path at approximately 2.23 Å. These results confirm that there is no significant Cu nanoparticle aggregation in CoCu@NC.
[0106] By fitting EXAFS curves in R-space and K-space, the structural parameters and average coordination number of the first shell were further analyzed. Figure 3 Part C Figure 3 (Part d in the middle).
[0107] The best-fit results confirm that the coordination configuration in the first shell follows the Cu-N scattering path. The average coordination number of the CoCu@NC material is 4, and the bond length is 1.94 Å, verifying the stable structure of the Cu-N4 configuration.
[0108] Wavelet transform (WT) plots further confirm the Cu-N scattering path in the CoCu@NC material. Figure 3 (Part e in the middle).
[0109] Figure 4 The images show 3D plots of the reflection loss curves of a) Co@NC, b) CoCu@ClNC and c) CoCu@SNC prepared in Comparative Example 1 and Examples 1-3 of this invention; and 3D plots of the impedance matching of d) Co@NC, e) CoCu@ClNC and f) CoCu@SNC.
[0110] from Figure 4As can be seen, the electromagnetic wave absorption performance of the prepared Co@NC and CoCu@NC materials was evaluated based on transmission line theory. For example... Figure 4 As shown in the middle section (ac), the minimum reflection loss of Co@NC (RL) is... min The effective absorption bandwidth (EAB) is -33.2 dB, and at a matched thickness of 1.9 mm, it exhibits an effective absorption bandwidth (EAB) of 7.6 GHz. CoCu@ClNC and CoCu@SNC are obtained by doping copper with chlorine or sulfur into the NC support, and their RL... min The bandwidth was increased to -56.8 dB and -74.5 dB respectively, and the corresponding EAB was broadened to 9.6 GHz with a thickness of 2.3 mm and to 11.0 GHz with a thickness of 2.6 mm respectively.
[0111] Such as impedance matching in three dimensions ( Figure 4 As shown in sections d, e, and f, CoCu@SNC exhibits the widest and most continuous region within the ideal matching range (0.8–1.2) at various frequencies and thicknesses, indicating its excellent impedance matching characteristics. In contrast, the overlap region of Co@NC within this range is much smaller, suggesting higher surface reflection and lower wave penetration efficiency.
[0112] Figure 5 The graph shows the antibacterial activity test results of the Co@NC, CoCu@ClNC and CoCu@SNC materials prepared in Examples 1-3 of this invention against a) Escherichia coli and b) Staphylococcus aureus.
[0113] from Figure 5 It can be seen that all materials exhibited certain antibacterial effects against both tested strains, and the antibacterial activity was significantly enhanced with the introduction of Cu single atoms and Cl / S anions. Plate colony counting results showed that CoCu@SNC was effective against *Escherichia coli* (…). Figure 5 Part a) and Staphylococcus aureus ( Figure 5 The bacterial survival rates in part b were as low as 9.3% and 40.8%, respectively, the lowest among all samples. This was mainly attributed to the enhanced peroxidase-like catalytic activity conferred by the optimized electronic configuration of Cu single-atom sites after regulation by the second-shell anion.
[0114] This invention utilizes a salt anion-mediated doping method to precisely introduce Cu single atoms and anions into a carbon matrix, achieving uniform dispersion at the single-atom level. The material prepared by this invention exhibits low reflection loss and a wide effective absorption bandwidth, while also possessing excellent antibacterial activity. The preparation process of this invention is simple, green, and efficient, and has broad application prospects in the fields of electromagnetic wave absorption and antibacterial protection.
[0115] The present invention has been described above by way of example with reference to the embodiments and accompanying drawings. Obviously, the implementation of the present invention is not limited to the above-described manner. Any improvements made by adopting the inventive concept and technical solution of the present invention, or the direct application of the inventive concept and technical solution of the present invention to other occasions without modification, are all within the protection scope of the present invention.
Claims
1. A method for preparing copper single-atom-doped MOF-derived carbon materials mediated by salt anions, characterized in that, Includes the following steps: Step 1: Preparation of Co-MOF precursors Cobalt salt solution and 2-methylimidazole solution were prepared by dissolving cobalt salt and 2-methylimidazole in solvents, respectively. Cobalt salt solution was added to 2-methylimidazole solution, the reaction was stirred, and the mixture was centrifuged, washed, and dried to obtain the Co-MOF precursor. Step 2: Polydopamine coating and heteroatom modification The Co-MOF precursor obtained in step 1 was dispersed in a solvent to obtain a Co-MOF dispersion; Dopamine hydrochloride was dissolved in a buffer solution, and copper salt was added to it to obtain a dopamine hydrochloride solution containing copper salt. Add the copper salt-containing dopamine hydrochloride solution to the Co-MOF dispersion and adjust the pH to alkaline. The reaction was stirred, centrifuged, washed, and dried to complete the polydopamine coating and heteroatom modification, yielding a copper-doped PDA@Co-MOF intermediate. Step 3: Preparation of copper single-atom doped MOF-derived carbon materials mediated by salt anions The copper-doped PDA@Co-MOF intermediate obtained in step 2 was subjected to high-temperature carbonization under an inert atmosphere. After natural cooling, the product was collected to obtain the copper single-atom-doped MOF-derived carbon material mediated by the salt anion. In step 2, the copper salt is at least one of copper chloride or copper sulfate.
2. The method for preparing copper single-atom-doped MOF-derived carbon materials mediated by salt anion according to claim 1, characterized in that: In step 1, the cobalt salt is at least one of cobalt acetate, cobalt nitrate, or cobalt chloride; The molar ratio of cobalt salt to 2-methylimidazole is 1:6-10; The stirring reaction time is 2-8 hours, and the reaction temperature is 10-30℃.
3. The method for preparing copper single-atom-doped MOF-derived carbon materials mediated by salt anion according to claim 1, characterized in that: The mass ratio of Co-MOF precursor to dopamine hydrochloride is 4-7:3; The mass ratio of copper salt to dopamine hydrochloride is 0.03-0.06:
1.
4. The method for preparing copper single-atom doped MOF-derived carbon materials mediated by salt anion according to claim 3, characterized in that: In step 2, the solvent used to disperse the Co-MOF precursor is a solvent prepared by mixing ethanol and ultrapure water at a volume ratio of 7:
3. The buffer solution for dissolving dopamine hydrochloride is Tris-HCl buffer, and the solution is alkaline; The stirring reaction time is 12-24 hours.
5. The method for preparing copper single-atom doped MOF-derived carbon materials mediated by salt anion according to claim 1, characterized in that: In step 3, the high-temperature carbonization temperature is 600-900℃; The heat preservation time for high-temperature carbonization is 1-4 hours.
6. The method for preparing copper single-atom doped MOF-derived carbon materials mediated by salt anion according to claim 5, characterized in that: In step 3, the heating rate for high-temperature carbonization is 1-10℃ / min.
7. The method for preparing copper single-atom-doped MOF-derived carbon materials mediated by salt anion according to claim 6, characterized in that: In step 3, the inert atmosphere is argon or nitrogen.
8. A copper single-atom-doped MOF-derived carbon material mediated by salt anion, characterized in that: It is prepared according to the preparation method described in any one of claims 1-7.
9. The salt anion-mediated copper single-atom doped MOF-derived carbon material according to claim 8, characterized in that: The copper single-atom doped MOF-derived carbon material has a core-shell structure, with Co particles embedded in an N-doped carbon matrix inside and a carbon layer co-doped with Cu single atoms and anions on the outside. In the copper single-atom doped MOF-derived carbon material, Cu is dispersed in the carbon matrix in the form of single atoms; The copper single-atom doped MOF-derived carbon material has a spindle-shaped morphology.
10. Use of the salt anion-mediated copper single-atom doped MOF-derived carbon material of claim 8 in the preparation of electromagnetic wave absorbing materials and / or antibacterial materials.
Citation Information
Patent Citations
Cobalt-based nitrogen-doped carbon nano composite material with hollow cubic structure as well as preparation method and application thereof
CN120957404A
Preparation method and application of multifunctional two-dimensional diatomic nano-enzyme material