Methods for preparing titanium alloy rods using powder metallurgy and titanium alloy rods
By using segmented hot isostatic pressing (HIP) and pure titanium encapsulation, the problem of simultaneously achieving high density and fine grain refinement in titanium alloy bars was solved, improving the overall performance and corrosion resistance of titanium alloy bars while reducing processing difficulty and cost.
Patent Information
- Application Number
- CN202611130776.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-27
- Publication Date
- 2026-11-10
Smart Images

Figure CN123060098A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of powder metallurgy technology, specifically to a method for preparing titanium alloy rods using powder metallurgy and the titanium alloy rods themselves. Background Technology
[0002] Titanium alloys, due to their low density, high specific strength, excellent corrosion resistance, and good biocompatibility, have become indispensable key materials in aerospace, biomedicine, and defense industries. In applications such as aero-engines, spacecraft structural components, and human implants, related parts often need to withstand high loads, high-speed operation, and cyclic stress in extreme environments, placing extremely high demands on the reliability, precision, and performance consistency of the components. However, traditional titanium alloy manufacturing processes such as investment casting and forging have significant limitations: they are prone to producing coarse microstructures, and metallurgical defects (such as porosity, inclusions, and compositional segregation) are difficult to control, resulting in lower component performance and insufficient stability; at the same time, material utilization is low, processing procedures are complex, and costs are high.
[0003] Hot isostatic pressing (HIP), an advanced near-net-shape forming technology in powder metallurgy, utilizes a high-temperature, high-pressure inert gas (usually argon) to apply isotropic pressure to metal powder within a sealed envelope. This causes plastic deformation, diffusion creep, and densification under the coupled effects of temperature and pressure, resulting in near-fully dense sintering. Compared to traditional processes, this technology offers significant advantages: firstly, the product density can reach 100%, with a uniform and fine microstructure, and overall mechanical properties exceeding those of forgings; secondly, it enables near-net-shape forming of complex components, significantly reducing machining and increasing material utilization to over 50%; and thirdly, it has a short process cycle and effectively avoids compositional segregation and the formation of coarse casting structures. These advantages make HIP a crucial process for manufacturing high-performance titanium alloy components, particularly critical aerospace structural parts.
[0004] Although hot isostatic pressing technology has significant advantages in the preparation of titanium alloys, the inventors recognized that current powder metallurgy methods for preparing titanium alloy bars have the problem of not being able to effectively balance density and grain refinement, resulting in the need to improve the overall performance of titanium alloy bars. Summary of the Invention
[0005] The main objective of this invention is to provide a method for preparing titanium alloy rods using powder metallurgy and the titanium alloy rods themselves, in order to solve the technical problem of how to effectively balance the density and grain refinement of titanium alloy rods to improve their overall performance.
[0006] According to one aspect of the present invention, a method for preparing titanium alloy rods by powder metallurgy is provided, comprising the following steps: S1, providing titanium alloy powder; S2, loading the titanium alloy powder into a sleeve and forming a sealed sleeve; S3, subjecting the sealed sleeve to hot isostatic pressing to obtain an intermediate rod, wherein the hot isostatic pressing includes a first heat-holding and pressure-holding stage and a second heat-holding and pressure-holding stage performed sequentially, wherein the temperature and pressure of the first heat-holding and pressure-holding stage are greater than the temperature and pressure of the second heat-holding and pressure-holding stage, and the time of the first heat-holding and pressure-holding stage is less than the time of the second heat-holding and pressure-holding stage; S4, performing post-processing on the intermediate rod to obtain a finished titanium alloy rod.
[0007] According to one embodiment of the present invention, in step S3, the temperature of the first heat preservation and pressure preservation stage is 950~1000℃, the pressure is 130~150MPa, and the time is 30~60 minutes; the temperature of the second heat preservation and pressure preservation stage is 820~850℃, the pressure is 100~120MPa, and the time is 80~120 minutes.
[0008] According to one embodiment of the present invention, in step S3, the temperature is increased from room temperature to the temperature of the first heat preservation and pressure holding stage at a rate of 2~5℃ / min, and the pressure is increased to the pressure of the first heat preservation and pressure holding stage at a rate of 1~2MPa / min.
[0009] According to one embodiment of the present invention, in step S3, after the first heat preservation and pressure holding stage is completed, the temperature is reduced to the temperature of the second heat preservation and pressure holding stage at a rate of 2~3℃ / min.
[0010] According to one embodiment of the present invention, in step S2, the material of the sheath is pure titanium; in step S4, the post-processing includes removing the oxide layer on the surface of the intermediate rod to obtain a finished titanium alloy rod containing a pure titanium layer.
[0011] According to one embodiment of the present invention, in step S4, the thickness of the oxide layer removed is less than the wall thickness of the sheath; the wall thickness of the sheath is 2~4 mm, and the thickness of the oxide layer removed is 1~2 mm.
[0012] According to one embodiment of the present invention, in step S1, the particle size range of the titanium alloy powder is 15~53μm, and the sphericity is greater than 93%; the titanium alloy powder is prepared by gas atomization.
[0013] According to one embodiment of the present invention, in step S1, the chemical composition of the titanium alloy powder, by mass percentage, satisfies the following: Al: 5.6%~6.2%, V: 3.8%~4.2%, Fe<0.05%, C<0.005%, N<0.011%, H<0.005%, O: 0.1%~0.12%.
[0014] According to one embodiment of the present invention, in step S2, the material of the sheath is pure titanium and its chemical composition by mass percentage satisfies: Fe < 0.02%, C < 0.015%, N < 0.008%, H < 0.03%, O < 0.05%.
[0015] According to another aspect of the present invention, a titanium alloy rod is provided, which is prepared by the above method. The titanium alloy rod has a yield strength >900MPa, a tensile strength >950MPa, and an elongation after fracture >12% at room temperature; the tensile strength of the titanium alloy rod at 400°C is >680MPa; and the creep time at 400°C and 560MPa exceeds 300 hours.
[0016] In the technical solution of this invention, the high-temperature and high-pressure short-time treatment in the first heat-holding and pressure-holding stage causes rapid plastic deformation and particle rearrangement of titanium alloy powder, achieving rapid closure of large-sized pores and preliminary metallurgical bonding. Simultaneously, the short-time heat-holding inhibits grain coarsening and growth. Then, the relatively low-temperature and high-pressure long-time treatment in the second heat-holding and pressure-holding stage utilizes a creep mechanism to continuously eliminate the micropores remaining from the first stage, achieving near-full densification of the bar. Simultaneously, due to the low temperature in this stage, the driving force for grain growth is extremely weak, and the fine-grained structure is preserved. The two processes work synergistically to overcome the technical contradiction of simultaneously achieving densification and grain refinement during hot isostatic pressing, achieving near-full densification (close to 100%) while effectively controlling grain size, thereby significantly improving the overall mechanical properties of the bar. Attached Figure Description
[0017] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0018] Figure 1 A flowchart illustrating a method for preparing titanium alloy rods using powder metallurgy according to an embodiment of the present invention is shown. Figure 2 The microstructure of a titanium alloy bar prepared according to an embodiment of the present invention is shown. Detailed Implementation
[0019] To make the objectives, technical solutions, and advantages of the present invention clearer, the embodiments of the present invention will be further described in detail below with reference to specific examples and the accompanying drawings.
[0020] It should be noted that all uses of "first" and "second" in the embodiments of the present invention are for the purpose of distinguishing two entities or parameters with the same name but different names. It is clear that "first" and "second" are only for the convenience of expression and should not be construed as limiting the embodiments of the present invention. Subsequent embodiments will not explain this in detail.
[0021] As mentioned in the background section above, the inventors of this application recognize that in the powder metallurgy preparation of titanium alloy rods, there is a problem of not being able to effectively balance density and grain refinement. Specifically, to achieve sufficient diffusion and pore closure between powder particles, high temperatures and long holding times are usually required, but this inevitably leads to grain coarsening, which in turn impairs the material's room temperature plasticity and fatigue properties. Conversely, if the temperature is lowered or the time is shortened to maintain a fine grain structure, sufficient metallurgical bonding between powder particles is difficult to achieve, resulting in insufficient density. Residual pores will become crack initiation sources, significantly reducing strength and reliability. To solve the above-mentioned problems in the prior art, this application proposes the following technical solution.
[0022] refer to Figure 1 This invention proposes a method for preparing titanium alloy rods using powder metallurgy, comprising the following steps: S1 provides titanium alloy powder; S2, titanium alloy powder is loaded into a sleeve and a sealed sleeve is made; S3, hot isostatic pressing is performed on the sealing sleeve to obtain the intermediate bar. The hot isostatic pressing process includes a first heat preservation and pressure holding stage and a second heat preservation and pressure holding stage performed sequentially. The temperature and pressure of the first heat preservation and pressure holding stage are greater than the temperature and pressure of the second heat preservation and pressure holding stage, and the time of the first heat preservation and pressure holding stage is less than the time of the second heat preservation and pressure holding stage. S4. Post-process the intermediate bar to obtain the finished titanium alloy bar.
[0023] In the technical solution of this invention, the high-temperature and high-pressure short-time treatment in the first heat-holding and pressure-holding stage causes rapid plastic deformation and particle rearrangement of titanium alloy powder, achieving rapid closure of large-sized pores and preliminary metallurgical bonding. Simultaneously, the short-time heat-holding inhibits grain coarsening and growth. Then, the relatively low-temperature and high-pressure long-time treatment in the second heat-holding and pressure-holding stage utilizes creep mechanisms to continuously eliminate residual micropores from the first stage, achieving near-full densification of the bar. Furthermore, due to the low temperature in this stage, the driving force for grain growth is extremely weak, allowing the fine-grained structure to be preserved. The two processes work synergistically to overcome the technical contradiction of simultaneously achieving densification and grain refinement during hot isostatic pressing, achieving near-full densification while effectively controlling grain size, thereby significantly improving the overall mechanical properties of the bar.
[0024] In some embodiments, in step S3, the temperature of the first heat preservation and pressure holding stage is 950~1000℃, the pressure is 130~150MPa, and the time is 30~60 minutes; the temperature of the second heat preservation and pressure holding stage is 820~850℃, the pressure is 100~120MPa, and the time is 80~120 minutes. By limiting the temperature, pressure, and time to the above ranges, it is possible to effectively suppress grain coarsening while ensuring sufficient powder densification, thereby obtaining titanium alloy rods with both excellent mechanical properties and high-temperature creep resistance.
[0025] In some embodiments, in step S3, a simultaneous heating and pressurization process is used to achieve the temperature and pressure of the first heat-holding and pressurization stage. Specifically, the temperature is increased from room temperature to the temperature of the first heat-holding and pressurization stage at a rate of 2~5℃ / min, while the pressure is increased to the pressure of the first heat-holding and pressurization stage at a rate of 1~2MPa / min. Through the simultaneous heating and pressurization process and appropriate heating and pressurization rates, the cladding can maintain its structural integrity throughout the hot isostatic pressing process, while ensuring that heat and pressure are transferred synchronously and uniformly to the interior of the powder, causing uniform plastic deformation and densification of the powder particles in each region.
[0026] In some embodiments, in step S3, after the first heat preservation and pressure holding stage is completed, the temperature is reduced to the temperature of the second heat preservation and pressure holding stage at a rate of 2~3℃ / min, so as to avoid the generation of thermal stress concentration inside the bar due to excessive cooling and the initiation of microcracks, while providing sufficient time for the uniform nucleation and precipitation of the α phase during the cooling process, thereby ensuring the uniformity of the final bar structure.
[0027] In some embodiments, in step S2, the sheath is made of pure titanium; in step S4, the post-processing includes removing the oxide layer from the surface of the intermediate bar to obtain a finished titanium alloy bar containing a pure titanium layer. The thickness of the oxide layer removed is less than the wall thickness of the sheath, for example, if the wall thickness of the sheath is 2-4 mm, the thickness of the oxide layer removed is 1-2 mm, thereby ensuring that the remaining sheath provides a pure titanium layer.
[0028] The inventors of this application recognized that while titanium alloys possess excellent comprehensive mechanical properties, their corrosion resistance is inferior to that of pure titanium. This invention, by employing a pure titanium cladding and removing only the surface oxide layer after hot isostatic pressing (HIP) rather than completely peeling off the cladding, enables the final bar to form a composite structure with pure titanium (e.g., TA1) as the outer layer and a titanium alloy (e.g., TC4) as the core. The excellent corrosion resistance of the pure titanium layer enhances the overall corrosion resistance of the bar, while the TC4 core ensures the bar's high strength and toughness. Furthermore, during HIP, the pure titanium cladding and the internal titanium alloy powder belong to the same titanium and titanium alloy alloy system, with similar coefficients of thermal expansion. This avoids excessive thermal stress or poor bonding at the interface caused by significant differences in the cladding and powder materials. Therefore, the above steps result in a finished bar that possesses both excellent mechanical properties and surface corrosion resistance. Meanwhile, due to the near-net-shape forming process, the intermediate bar is close to the finished size. After hot isostatic pressing, only 1-2 mm of surface oxide layer needs to be removed to obtain the finished product, which can significantly reduce the amount of machining. Furthermore, since the hardness and work hardening tendency of the outer pure titanium are lower than those of titanium alloy, the tool wear is less and the cutting is smoother when machining the bar, such as turning, thus significantly reducing the machining difficulty and cost of the bar.
[0029] In step S2, laser welding technology can be used to form the casing, followed by an airtightness test. Titanium alloy powder is then injected through the powder injection port, and the compaction density is achieved with vibration assistance. After powder injection, the inside of the casing is vacuum degassed, and finally the powder injection port is vacuum-sealed to obtain a sealed casing.
[0030] In some embodiments, in step S1, the titanium alloy powder is prepared by gas atomization. The particle size of the titanium alloy powder ranges from 15 to 53 μm, and the sphericity is greater than 93%. This ensures that the powder has good flowability and uniform filling, achieving uniform plastic deformation and densification in subsequent hot isostatic pressing, thereby obtaining a high-density and uniformly structured rod.
[0031] In some embodiments, in step S1, the chemical composition of the titanium alloy powder, by mass percentage, satisfies the following: Al: 5.6%~6.2%, V: 3.8%~4.2%, Fe < 0.05%, C < 0.005%, N < 0.011%, H < 0.005%, O: 0.1%~0.12%. By controlling the chemical composition of the TC4 titanium alloy powder within the above range, the solid solution strengthening effect of Al, V, and O can be utilized to ensure the strength level of the bar, while strictly controlling the content of interstitial elements (Fe, C, N, H, O) to avoid significant deterioration of plasticity, thus achieving both high strength and good room temperature plasticity.
[0032] In some embodiments, in step S2, the cladding material is pure titanium and its chemical composition, by mass percentage, satisfies: Fe < 0.02%, C < 0.015%, N < 0.008%, H < 0.03%, O < 0.05%. By controlling the chemical composition of the pure titanium cladding, sufficient plasticity and low deformation resistance are ensured, allowing for synchronized deformation with the titanium alloy powder during hot isostatic pressing. Simultaneously, excessive diffusion of impurity elements from the cladding into the titanium alloy powder at high temperatures is avoided, preventing the deterioration of the mechanical properties of the core titanium alloy due to impurity contamination.
[0033] In some embodiments of the present invention, the titanium alloy rods prepared by the above method have a yield strength >900 MPa, a tensile strength >950 MPa, and an elongation after fracture >12% at room temperature; the tensile strength of the titanium alloy rods at 400°C is >680 MPa; and the creep rupture time at 400°C and 560 MPa exceeds 300 hours. Compared to titanium alloy powder, the content deviation of impurity elements in the finished product is strictly controlled to: C ±0.001%, O ±0.01%, N ±0.002%, Fe ±0.01%. Figure 2 The microstructure of a titanium alloy rod prepared according to an embodiment of the present invention is shown, such as... Figure 2 As shown, the grain structure is fine and uniform, with a grain size of less than 10 μm; no obvious pores or defects are observed, indicating that the bar has a high density.
[0034] In summary, this invention provides a method for preparing multilayer titanium alloy rods using powder metallurgy. By optimizing process parameters and flow design, it improves surface corrosion resistance and overall mechanical properties while reducing processing difficulty.
[0035] By adopting the above technical solution, the present invention can achieve the following beneficial effects: 1. By precisely controlling the powder particle size and oxygen content, and combining it with a unique segmented hot isostatic pressing process, titanium alloy rods with fine grain structure (<10μm), uniform composition, and excellent mechanical properties can be obtained.
[0036] 2. The two-stage heat preservation and pressure preservation process of "high temperature for short time and then low temperature for long time" promotes the uniform plastic deformation of powder, effectively eliminates porosity, and significantly improves the density and uniformity of the parts.
[0037] 3. By using pure titanium encapsulation to encapsulate TC4 powder and performing hot isostatic pressing, composite titanium alloy rods with the outer layer having the corrosion resistance of pure titanium, the core having the high strength and toughness of TC4, and good overall processing performance can be directly prepared.
[0038] The following description is based on specific embodiments.
[0039] Example 1 Powder parameters: TC4 titanium alloy powder prepared by gas atomization, with a particle size of 15~53μm and a sphericity of 95%. Chemical composition (mass fraction, %): Al: 6.0, V: 4.0, Fe: 0.03, C: 0.003, N: 0.008, H: 0.003, O: 0.11.
[0040] Encasing and Powder Filling: A TA1 pure titanium encasing with a wall thickness of 3.0mm is used. After the encasing is laser welded and passes the airtightness test, the above-mentioned powder is injected and vibrated to compact it, followed by vacuum degassing and sealing.
[0041] Hot isostatic pressing (HIP) process: Simultaneous heating and pressurization are employed. The temperature is increased to 980℃ at a rate of 3℃ / min, while the pressure is increased to 140MPa at a rate of 1MPa / min. This temperature and pressure are maintained for 45 minutes. Subsequently, the temperature is decreased to 835℃ at a rate of 2.5℃ / min, and the pressure is adjusted to 110MPa, with the pressure maintained for another 100 minutes. After completion, the furnace is cooled.
[0042] Machining and performance: The finished bar stock is obtained by turning and removing approximately 1.5 mm of the outer surface.
[0043] Testing revealed that the finished bar stock has a room temperature yield strength of 930 MPa, a tensile strength of 980 MPa, and an elongation after fracture of 14%. The tensile strength at 400℃ is 700 MPa, and the creep rupture time under 400℃ / 560 MPa conditions is 320 hours. Impurity elements are well controlled, the grain size is 8 μm, the density is close to 100%, and the surface exhibits corrosion resistance comparable to pure titanium.
[0044] Example 2 Powder parameters: TC4 titanium alloy powder prepared by gas atomization, with a particle size of 15~53μm and a sphericity of 94%. Chemical composition (mass fraction, %): Al: 5.8, V: 3.9, Fe: 0.04, C: 0.004, N: 0.010, H: 0.004, O: 0.105.
[0045] Encasing and Powder Filling: A TA1 pure titanium encasing with a wall thickness of 2.5mm is used. After the encasing is laser welded and passes the airtightness test, the above-mentioned powder is injected and vibrated to compact it, followed by vacuum degassing and sealing.
[0046] Hot isostatic pressing (HIP) process: The temperature is increased to 995℃ at a rate of 4℃ / min, while the pressure is simultaneously increased to 145MPa. This temperature and pressure are maintained for 50 minutes. Subsequently, the temperature is decreased to 845℃ at a rate of 2℃ / min, and the pressure is adjusted to 115MPa. This temperature and pressure are maintained for 110 minutes. The furnace is then cooled after the process.
[0047] Machining and performance: Turning removes approximately 1.2 mm of the outer surface.
[0048] Testing revealed that the finished bar stock has a room temperature yield strength of 910 MPa, a tensile strength of 965 MPa, and an elongation after fracture of 13%. The tensile strength at 400℃ is 690 MPa, and the creep rupture time under 400℃ / 560 MPa conditions reaches 350 hours. The microstructure is uniform, with a grain size of 7 μm.
[0049] Example 3 Powder parameters: TC4 titanium alloy powder prepared by gas atomization, with a particle size of 15~53μm and a sphericity of 93.5%. Chemical composition (mass fraction, %) is: Al: 6.1, V: 4.1, Fe: 0.02, C: 0.002, N: 0.007, H: 0.002, O: 0.10.
[0050] Encasing and Powder Filling: A TA1 pure titanium encasing with a wall thickness of 3.5mm is used. After the encasing is laser welded and passes the airtightness test, the above-mentioned powder is injected and vibrated to compact it, followed by vacuum degassing and sealing.
[0051] Hot isostatic pressing (HIP) process: The temperature is increased to 960℃ at a rate of 2.5℃ / min, while the pressure is simultaneously increased to 135MPa. This temperature and pressure are maintained for 60 minutes. Subsequently, the temperature is decreased to 825℃ at a rate of 3℃ / min, and the pressure is adjusted to 105MPa. This temperature and pressure are maintained for 90 minutes. The furnace is then cooled after the process.
[0052] Machining and performance: Turning removes approximately 1.8 mm of the outer surface.
[0053] Testing revealed that the finished bar stock has a room temperature yield strength of 920 MPa, a tensile strength of 960 MPa, and an elongation after fracture of 12.5%. The tensile strength at 400℃ is 685 MPa, and the creep rupture time under 400℃ / 560 MPa conditions is 310 hours. Impurity element deviations are strictly controlled (e.g., O content deviation ±0.008%), resulting in excellent compositional uniformity and a grain size of 9 μm.
[0054] Those skilled in the art should understand that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the invention (including the claims) is limited to these examples. Within the framework of the invention, technical features of the above embodiments or different embodiments can be combined, and many other variations of the different aspects of the invention as described above exist, which are not provided in the details for the sake of brevity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the invention should be included within the protection scope of the invention.
Claims
1. A method for preparing titanium alloy rods using powder metallurgy, characterized in that, Includes the following steps: S1 provides titanium alloy powder; S2, The titanium alloy powder is loaded into a sleeve and a sealed sleeve is formed; S3, the sealing sleeve is subjected to hot isostatic pressing to obtain an intermediate bar, wherein the hot isostatic pressing includes a first heat preservation and pressure holding stage and a second heat preservation and pressure holding stage performed sequentially, the temperature and pressure of the first heat preservation and pressure holding stage are greater than the temperature and pressure of the second heat preservation and pressure holding stage, and the time of the first heat preservation and pressure holding stage is less than the time of the second heat preservation and pressure holding stage. S4. The intermediate bar is post-processed to obtain the finished titanium alloy bar.
2. The method according to claim 1, characterized in that, In step S3, the temperature of the first heat preservation and pressure holding stage is 950~1000℃, the pressure is 130~150MPa, and the time is 30~60 minutes; the temperature of the second heat preservation and pressure holding stage is 820~850℃, the pressure is 100~120MPa, and the time is 80~120 minutes.
3. The method according to claim 1, characterized in that, In step S3, the temperature is increased from room temperature to the temperature of the first heat preservation and pressure holding stage at a rate of 2~5℃ / min, and the pressure is increased to the pressure of the first heat preservation and pressure holding stage at a rate of 1~2MPa / min.
4. The method according to claim 1, characterized in that, In step S3, after the first heat preservation and pressure holding stage ends, the temperature is reduced to the temperature of the second heat preservation and pressure holding stage at a rate of 2~3℃ / min.
5. The method according to claim 1, characterized in that, In step S2, the sheath is made of pure titanium; in step S4, the post-processing includes removing the oxide layer on the surface of the intermediate rod to obtain a finished titanium alloy rod containing a pure titanium layer.
6. The method according to claim 5, characterized in that, In step S4, the thickness of the oxide layer removed is less than the wall thickness of the casing; the wall thickness of the casing is 2~4mm, and the thickness of the oxide layer removed is 1~2mm.
7. The method according to claim 1, characterized in that, In step S1, the titanium alloy powder has a particle size range of 15~53μm and a sphericity greater than 93%; the titanium alloy powder is produced by gas atomization.
8. The method according to claim 1, characterized in that, In step S1, the chemical composition of the titanium alloy powder, by mass percentage, satisfies the following: Al: 5.6%~6.2%, V: 3.8%~4.2%, Fe<0.05%, C<0.005%, N<0.011%, H<0.005%, O: 0.1%~0.12%.
9. The method according to claim 1, characterized in that, In step S2, the material of the casing is pure titanium and its chemical composition by mass percentage satisfies: Fe < 0.02%, C < 0.015%, N < 0.008%, H < 0.03%, O < 0.05%.
10. A titanium alloy rod, characterized in that, The titanium alloy bar is prepared by the method described in any one of claims 1-9, and has a yield strength > 900 MPa, a tensile strength > 950 MPa, and an elongation after fracture > 12% at room temperature; the tensile strength of the titanium alloy bar at 400°C is > 680 MPa; and the creep rupture time at 400°C and 560 MPa exceeds 300 hours.