A method for the preparation of ceramic coatings based on H2O induction
By introducing H2O gas and combining it with CO2 laser irradiation during the aerosol deposition process, the problem of weak bonding between yttrium oxide and alumina ceramic materials was solved, and the densification and hardness improvement of the yttrium oxide coating were achieved.
Patent Information
- Application Number
- CN202611334088.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-10
AI Technical Summary
In existing technologies, yttrium oxide and alumina ceramic materials have weak adhesion to the substrate during aerosol deposition, making them prone to peeling or cracking. Furthermore, laser-assisted aerosol deposition has low efficiency and is difficult to form a dense coating.
The H2O-induced method is used to introduce 3-6 vol% H2O gas during the aerosol deposition process, combined with CO2 laser irradiation, to promote the fusion of yttrium oxide powder, lower the melting point, and enhance the density of the coating.
It significantly improves the hardness and density of the yttrium oxide coating, reduces porosity, and enhances the adhesion between the coating and the substrate.
Smart Images

Figure CN123062267A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of low-pressure solid-state high-speed deposition, and more particularly to a method for preparing ceramic coatings based on H2O-induced deposition. Background Technology
[0002] Aerosol deposition is a method of spraying at room temperature. Under low vacuum conditions, a carrier gas accelerates solid particles to supersonic speeds; due to the pressure difference, the particles impact the substrate, causing plastic deformation to form a coating. Compared with traditional spraying processes, this process requires no heat assistance and can produce a dense ceramic film from raw material powder at room temperature. In this invention, yttrium oxide powder has a Mohs hardness of 6.5-7, and alumina ceramic has a Mohs hardness of 9. Both are relatively hard materials, resulting in weak adhesion of the coating during aerosol deposition. The coating is prone to peeling or cracking, making it difficult to form an effective deposition.
[0003] Current research on methods to enhance the adhesion between coatings and substrates mainly includes: heating aerosols, high-energy ball milling of powder, and powder spray drying. These methods increase the energy of the aerosol to some extent, but do not significantly improve the adhesion to substrates with high hardness. Yttrium oxide powder has a refractive index of 1.93 and an effective absorption wavelength of 587.6 nm (power density: 500 W / cm²). 2 Commonly available lasers are infrared, visible, and ultraviolet, which are not conducive to absorbing laser energy. To be suitable for yttrium oxide powder, a shorter wavelength light source, such as a fiber laser or CO2 laser, must be selected. However, single laser-assisted aerosol deposition has low coupling efficiency, and some aerosol particles are not fully melted during laser irradiation. Furthermore, traditional methods for densifying yttrium oxide coatings mainly rely on doping modification (such as ZrO2, Al2O3) or high-temperature sintering, which suffer from high-temperature volatilization and grain boundary weakening. Summary of the Invention
[0004] To address the shortcomings of existing technologies, this invention proposes a method for preparing ceramic coatings based on H2O-induced coatings.
[0005] The technical solution of this invention is as follows: A method for preparing an H2O-induced ceramic coating includes the following steps: mixing metal oxide ceramic powder with pressurized carrier gas to form an aerosol, the aerosol being sprayed onto the surface of a substrate located in an aerosol deposition chamber through a first spray gun; simultaneously with the spraying, H2O gas is introduced into the deposition area through a second spray gun independent of the first spray gun, and a laser is simultaneously turned on to irradiate the deposition area, thereby obtaining an H2O-induced ceramic coating.
[0006] Furthermore, in the preparation method, the metal oxide ceramic powder is yttrium oxide powder.
[0007] Furthermore, the particle size of the yttrium oxide powder is selected from 0.1-10 μm.
[0008] Furthermore, in the preparation method, the pressurized carrier gas is He.
[0009] Furthermore, in the preparation method, the process parameters for aerosol spraying are as follows: pressurized carrier gas flow rate is 25-80 L / min, the moving speed of the first spray gun is 5-20 mm / s, the distance from the nozzle of the first spray gun to the substrate surface is 5-20 mm, the powder feeding rate of the first spray gun is 0.5-0.7 g / min, and the spraying time of the first spray gun is 190-240 min.
[0010] Furthermore, in the preparation method, the volume of H2O gas in the aerosol deposition chamber accounts for 3-6% of the total volume of the He and H2O mixture.
[0011] Furthermore, the laser is a CO2 laser.
[0012] Furthermore, the process parameters for the laser irradiation are: wavelength 10.6 μm, power density 500-1000 W / cm². 2 .
[0013] Compared with the prior art, the present invention has at least the following advantages: This invention relates to a method for preparing a ceramic coating based on H2O induction. The method introduces 3-6 vol% H2O. Under CO2 laser irradiation, the introduced H2O gas helps lower the melting point of yttrium oxide, making it easier for yttrium oxide to fuse, significantly reducing porosity within the yttrium oxide coating, and enhancing its hardness. Attached Figure Description
[0014] To more clearly illustrate the specific embodiments of the present invention, the accompanying drawings used in the description of the specific embodiments or the prior art will be briefly introduced below.
[0015] Figure 1 This is a cross-sectional SEM image of the yttrium oxide coating from Example 1. Figure 2 This is a cross-sectional SEM image of a comparative yttrium oxide coating. Detailed Implementation
[0016] The present invention will now be described in further detail. It should be noted that the following specific embodiments are only used to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention. Those skilled in the art can make some non-essential improvements and adjustments to the present invention based on the above application content.
[0017] This invention provides a general and / or specific description of the materials and experimental methods used in the experiments. Unless otherwise specified, all experimental or testing methods are conventional methods; all reagents or instruments used, unless otherwise specified, are commercially available conventional products prepared or used using conventional methods.
[0018] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art.
[0019] Example 1
[0020] This embodiment provides a method for preparing a ceramic coating based on H2O induction, and the specific process is as follows.
[0021] A spraying system equipped with a Laval spray gun, a high-pressure gas spray gun, and a CO2 laser was employed. During aerosol deposition, pure helium (He) was used as the carrier gas for the Y₂O₃ powder. The pressure in the aerosol generation chamber was set to 100 kPa, and the carrier gas flow rate was 25 L / min. This accelerated the formation of an aerosol from the raw Y₂O₃ powder with a particle size of 0.1-10 μm, which was then sprayed onto the substrate through the Laval spray gun. Al₂O₃ particles with dimensions of 45 × 45 mm were selected as the deposition substrate and placed on an XY moving platform. The vacuum pressure in the deposition chamber was maintained at 80 Pa. The vertical distance between the Laval spray gun and the substrate was adjusted to 10 mm, and the moving speed of the platform relative to the spray gun was controlled at 5 mm / s for supersonic spraying impact. The powder feed rate was 0.5 g / min, and the deposition time was 200 min.
[0022] During powder coating, H2O gas is continuously introduced into the substrate deposition area through an independent high-pressure gas spray gun, forming a mixed atmosphere containing 5 vol% H2O gas. Simultaneously, a CO2 laser is activated to irradiate the yttrium oxide coating area being deposited. The CO2 laser spot is controlled to coincide with the powder spot area sprayed from the first spray gun. The CO2 laser irradiation process parameters are: wavelength 10.6 μm, power density 500 W / cm³. 2 Under laser irradiation, the temperature of the deposition area exceeds 100°C. Independently sprayed gaseous H2O acts on the surface of yttrium oxide particles, which helps to lower the melting point of yttrium oxide, promotes particle fusion, and produces a yttrium oxide coating.
[0023] Example 2
[0024] This embodiment provides a method for preparing a ceramic coating based on H2O induction, and the specific process is as follows.
[0025] A spraying system equipped with a Laval spray gun, a high-pressure gas spray gun, and a CO2 laser was employed. During aerosol deposition, pure He was used as the carrier gas for the Y₂O₃ powder. The pressure in the aerosol generation chamber was set to 400 kPa, and the carrier gas flow rate was 50 L / min. The raw Y₂O₃ powder with a particle size of 0.1-10 μm was accelerated to form an aerosol, which was then sprayed onto the substrate through the Laval spray gun. Al₂O₃ with dimensions of 45 × 45 mm was selected as the deposition substrate and placed on an XY moving platform. The vacuum pressure in the deposition chamber was maintained at 100 Pa. The vertical distance between the Laval spray gun and the substrate was adjusted to 10 mm, and the moving speed of the platform relative to the spray gun was controlled at 5 mm / s for supersonic spraying impact. The powder feed rate was 0.5 g / min, and the deposition time was 220 min.
[0026] During powder coating, H2O gas is continuously introduced into the substrate deposition area through an independent high-pressure gas spray gun, forming a mixed atmosphere containing 3 vol% H2O gas. Simultaneously, a CO2 laser is activated to irradiate the yttrium oxide coating area being deposited. The CO2 laser spot is controlled to coincide with the powder spot area sprayed from the first spray gun. The CO2 laser irradiation process parameters are: wavelength 10.6 μm, power density 500 W / cm³. 2 .
[0027] Example 3
[0028] This embodiment provides a method for preparing a ceramic coating based on H2O induction, and the specific process is as follows.
[0029] A spraying system equipped with a Laval spray gun, a high-pressure gas spray gun, and a CO2 laser was employed. During aerosol deposition, pure He was used as the carrier gas for the Y₂O₃ powder. The pressure in the aerosol generation chamber was set to 600 kPa, and the carrier gas flow rate was 80 L / min. This accelerated the formation of an aerosol from the raw Y₂O₃ powder with a particle size of 0.1-10 μm, which was then sprayed onto the substrate through the Laval spray gun. Al₂O₃ particles with dimensions of 45 × 45 mm were selected as the deposition substrate and placed on an XY moving platform. The vacuum pressure in the deposition chamber was maintained at 600 Pa. The vertical distance between the Laval spray gun and the substrate was adjusted to 10 mm, and the platform's relative movement speed to the spray gun was controlled at 5 mm / s for supersonic spraying impact. The powder feed rate was 0.7 g / min, and the deposition time was 200 min.
[0030] During powder coating, H2O gas is continuously introduced into the substrate deposition area through an independent high-pressure gas spray gun, forming a mixed atmosphere containing 6 vol% H2O gas. Simultaneously, a CO2 laser is activated to irradiate the yttrium oxide coating area being deposited. The CO2 laser spot is controlled to coincide with the powder spot area sprayed from the first spray gun. The CO2 laser irradiation process parameters are: wavelength 10.6 μm, power density 500 W / cm³.2 .
[0031] Comparative Example The difference between this comparative example and Example 1 is that H2O gas is not introduced into the deposition chamber, while the other steps are the same.
[0032] Test case After the above steps, a dense ceramic coating is formed. The microstructure and porosity of the coating cross-sections prepared in Example 1 and the comparative example are observed using SEM (scanning electron microscopy). The results are as follows: Figure 1-2 As shown.
[0033] The hardness of the ceramic coatings prepared in Example 1 and the comparative example was tested according to GB / T 39687-2020 "Vickers Hardness Test Method for Fine Ceramic Coatings". The porosity test method was TEM image scanning, performed according to GB / T 20724-2021. In the laser-assisted aerosol deposition process of this invention, 3-6 vol% H2O is used as the reactant gas. The introduced H2O gas, under CO2 laser irradiation, acts on the surface of yttrium oxide particles, effectively reducing the melting point of yttrium oxide. Due to the lower melting point, yttrium oxide particles are more likely to fuse after absorbing laser energy, and the high-temperature volatilization of yttrium oxide is reduced, improving the coating density. As tested in Example 1, the ceramic coating prepared by the method of this invention has a hardness of 12.1 GPa and a porosity of 2.5%, while the ceramic coating prepared in the comparative example has a hardness of 8.9 GPa and a porosity of 10.9%.
[0034] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be covered within the scope of the claims and specification of the present invention.
Claims
1. A method for preparing a ceramic coating based on H2O-induced coating, characterized in that, Includes the following steps: Metal oxide ceramic powder is mixed with pressurized carrier gas to form an aerosol. The aerosol is sprayed onto the surface of a substrate located in the aerosol deposition chamber through a first spray gun. At the same time as the spraying, H2O gas is simultaneously introduced into the deposition area through a second spray gun independent of the first spray gun, and the deposition area is simultaneously irradiated by a laser to obtain an H2O-induced ceramic coating.
2. The method for preparing a ceramic coating according to claim 1, characterized in that, In the preparation method, the metal oxide ceramic powder is yttrium oxide powder.
3. The method for preparing a ceramic coating according to claim 2, characterized in that, The particle size of the yttrium oxide powder is selected from 0.1-10 μm.
4. The method for preparing a ceramic coating according to claim 1, characterized in that, In the preparation method, the pressurized carrier gas is He.
5. The method for preparing a ceramic coating according to claim 1, characterized in that, In the preparation method, the process parameters for aerosol spraying are as follows: pressurized carrier gas flow rate is 25-80 L / min, the moving speed of the first spray gun is 5-20 mm / s, the distance from the nozzle of the first spray gun to the substrate surface is 5-20 mm, the powder feeding rate of the first spray gun is 0.5-0.7 g / min, and the spraying time of the first spray gun is 190-240 min.
6. The method for preparing a ceramic coating according to claim 4, characterized in that, In the preparation method, the volume of H2O gas in the aerosol deposition chamber accounts for 3-6% of the total volume of the He and H2O mixture.
7. The method for preparing a ceramic coating according to claim 1, characterized in that, The laser is a CO2 laser.
8. The method for preparing a ceramic coating according to claim 1, characterized in that, The laser irradiation process parameters are: wavelength 10.6 μm, power density 500-1000 W / cm². 2 .