A method for preparing tetrahydrofuranol by hydrogenation of a bio-based furan derivative

By using the reverse nickel-based catalyst aMOx/bNi to catalyze the preparation of tetrahydrofuran alcohol from bio-based furan derivatives at low temperatures, the problems of high energy consumption and high cost in the high-temperature and high-pressure preparation of tetrahydrofuran alcohol are solved, realizing the preparation of tetrahydrofuran alcohol with high efficiency and low cost. The catalyst is regenerable and has wide applicability.

CN123062415APending Publication Date: 2026-11-10HUNAN NORMAL UNIVERSITY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202611586560.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-14
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies require high temperature and pressure to prepare tetrahydrofuran alcohol, resulting in high energy consumption and expensive catalysts. This makes it difficult to achieve efficient one-pot hydrogenation of bio-based furan derivatives, and the applicability of the catalysts is limited.

Method used

Using the reversed nickel-based catalyst aMOx/bNi, and with hydrogen as the hydrogen source in the presence of solvent, tetrahydrofuran alcohol is prepared from bio-based furan derivatives in a one-pot process at 25-55℃. The catalyst is prepared by co-precipitation and loaded with a small amount of oxide on a metallic nickel substrate. The strong interaction between Ni and MgO is utilized to improve the hydrogenation performance.

Benefits of technology

Achieving high selectivity and high conversion rate in the preparation of tetrahydrofuranol under mild conditions, the catalyst preparation is simple, low-cost, widely applicable, and renewable, significantly reducing reaction energy consumption and equipment investment costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123062415A_ABST
    Figure CN123062415A_ABST
Patent Text Reader

Abstract

A method for preparing tetrahydrofuranol by hydrogenation of a bio-based furan derivative includes the following steps: using a bio-based furan derivative as a reactant, in the presence of a solvent, using hydrogen as a hydrogen source, and employing the catalyst aMO. x / bNi is used for catalytic hydrogenation to produce tetrahydrofuran alcohols in a one-pot process; the metal oxide loading in the catalyst is 5-40 wt% of the catalyst mass. This invention enables the one-step hydrogenation of bio-based furan derivatives to tetrahydrofuran alcohols under mild conditions. In a green medium such as water or alcohols, the hydrogenation process can be completed with high conversion and high selectivity at room temperature or a low reaction temperature (25-55°C). The catalytic system constructed in this invention, under the same reaction conditions, has the advantages of being mild and green, having a simple and low-cost catalyst preparation process, wide applicability, easy separation, and regeneration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for preparing tetrahydrofuranol, specifically a method for preparing tetrahydrofuranol from a bio-based furan derivative via catalytic conversion under hydrogenation conditions. Background Technology

[0002] Tetrahydrofuran alcohols, such as tetrahydrofurfural, 5-methyltetrahydrofurfural, or tetrahydrofurandimethyl, are important pharmaceutical and fine chemical intermediates, widely used as environmentally friendly solvents in fields such as electronics, semiconductors, coatings, inks, agriculture, and materials. Existing methods for preparing tetrahydrofuran alcohols typically use furfural aldehydes as raw materials, obtaining them through one or two-step complete hydrogenation. This process is limited by the high reaction energy barrier of the furan ring, and the reaction is usually carried out at high temperatures of 120-180°C and hydrogen pressures above 3-5 MPa. Furthermore, the catalysts often employ Pd, Ru, and Pt multi-component composite noble metal catalysts (see reference: Selective switching hydrogenation products of 5-hydroxymethylfurfural at high...). Substrate concentrations by regulating Pd-MgO interactions, Appl. Catal. B Environ., 2025, 361, 124578; Ru / TiO2 catalysts for selective formation of ring hydrogenation or ring-opening products from biomass-derived 5-hydroxymethylfurfural, Green Chem., 2026, 28, 7768-7781; and patent applications CN113651780A, CN119751385A, and CN111233797A), make it difficult to achieve a balance between the economic cost of the catalyst and the high stability of the catalyst.

[0003] Existing technologies involve the hydrogenation of furfural and furfuryl alcohol to prepare tetrahydrofurfuryl alcohol. Patent application CN121016814A discloses a noble metal catalyst, PdCo / SPC, supported on sunflower stem pith carbon. Under preferred process conditions (isopropanol as solvent, 2 MPa H2, reaction at 100℃ for 1 h), a furfural conversion rate of 99.9% and a tetrahydrofurfuryl alcohol selectivity are obtained. Patent application CN122558486A discloses a multi-component composite non-noble metal catalyst, NiLa / Al2O3-ZrO2. Under preferred process conditions (110℃, 3 MPa H2), a furfuryl alcohol conversion rate of 99.6% and a tetrahydrofurfuryl alcohol selectivity of 98.7% are achieved.

[0004] Patent CN117417313A discloses a method for using a commercial Raney nickel catalyst in combination with an Amberlyst 15 catalyst, in ethanol solvent, at 130°C, 5 MPa H2, for 5 h, to obtain a 96.57% conversion of 5-hydroxymethylfurfural and a 84.11% selectivity of 5-methyltetrahydrofurfural.

[0005] Compared to the preparation of 5-methyltetrahydrofurfuryl alcohol from furfural, there are fewer reports on the preparation of 5-methyltetrahydrofurfuryl alcohol from 5-methylfurfural and 5-methylfurfuryl alcohol. For example, there are reports by Zhang et al. (see reference: On-Demand, Highly Tunable, and Selective). 5-Hydroxymethylfurfural Hydrogenation to Furan Diols Enabled by Ni and Ni3Ga Alloy Catalysts (ACS Catal., 2023, 13, 803-814) employs a hydrotalcite-based Ni3Ga composite catalyst. 1.5 GaAl-LDO-700, in tetrahydrofuran solvent, at 120℃, 3MPa H2, for 2h, yielded 100% conversion of 5-methylfurfural and 94% selectivity of 5-methyltetrahydrofurfural.

[0006] Patent application CN119771443A discloses a scheme using a noble metal composite catalyst, Pd / NiCoOx, under optimized process conditions (5-hydroxymethylfurfural as substrate, 60°C, 1MPa H2, 1.5h), achieving 100% conversion of 5-hydroxymethylfurfural and 91.1% selectivity for tetrahydrofurandimethyl. Further, using 2,5-furandimethyl as substrate (30°C, 1MPa H2, 4h), a 98% conversion of 2,5-furandimethyl and a 94.3% selectivity for tetrahydrofurandimethyl were obtained.

[0007] Compared to the aforementioned noble metal catalysts and structurally complex composite catalysts, non-noble metal nickel-based catalysts, which are cost-effective and exhibit good hydrogenation performance, have promising application potential. However, the intrinsic hydrogenation activity of nickel-based catalysts reported in existing technologies is relatively insufficient, typically requiring high temperature and pressure (100-160℃, 3-5MPa H2) to overcome the high activation energy barrier of furan ring hydrogenation, which further increases reaction energy consumption. Furthermore, non-noble metal systems often suffer from limited substrate applicability and difficulty in controlling side reactions (see reference: Surface Synergetic Effects of Ni-ReO). x for Promoting the Mild Hydrogenation of Furfural to Tetrahydrofurfuryl Alcohol, ACS Catal., 2023,13,11256–11267; Zn-modulated NiCe catalyst sselectively controls the hydrogenation of 5-hydroxymethylfurfural to (Dihydroxymethyl furan derivatives, Chem. Eng. J., 2025, 521, 167151). Therefore, achieving efficient one-pot full hydrogenation of bio-based furan derivatives with high selectivity for tetrahydrofuran alcohols at relatively low reaction temperatures and hydrogen pressures remains a significant technical challenge. Summary of the Invention

[0008] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a method for preparing tetrahydrofuran alcohol by hydrogenation of bio-based furan derivatives, with mild reaction conditions, low reaction temperature, low energy consumption, and low cost.

[0009] The technical solution adopted by this invention to solve its technical problem is a method for preparing tetrahydrofuranol by hydrogenation of bio-based furan derivatives, comprising the following steps:

[0010] Using bio-based furan derivatives as reactants, in the presence of a solvent, with hydrogen as the hydrogen source, and employing the catalyst aMO... x / bNi (a and b are the mass fractions of the corresponding components in the catalyst, where a is 5-40wt%, b is 60-95wt%, a+b=100%) is used for catalytic hydrogenation to produce tetrahydrofuran alcohols in a one-pot process; the temperature of the catalytic hydrogenation reaction is 25-55℃.

[0011] Furthermore, the bio-based furan derivative is one of furfural, furfuryl alcohol, 5-methylfurfural, 5-methylfurfural, 5-hydroxymethylfurfural, and 2,5-furandiethanol. The tetrahydrofuranol is the tetrahydrofuranol corresponding to the bio-based furan derivative, such as tetrahydrofurfural, 5-methyltetrahydrofurfural, and tetrahydrofurandiethanol; the tetrahydrofuranol corresponding to furfural and furfuryl alcohol is tetrahydrofurfural; the tetrahydrofuranol corresponding to 5-methylfurfural and 5-methylfurfural is 5-methyltetrahydrofurfural; and the tetrahydrofuranol corresponding to 5-hydroxymethylfurfural and 2,5-furandiethanol is tetrahydrofurandiethanol.

[0012] Furthermore, the reaction vessel is a batch reactor. More preferably, the batch reactor is a high-pressure reactor.

[0013] Furthermore, the solvent is at least one of methanol, ethanol, isopropanol, and water, with water being the preferred solvent.

[0014] Furthermore, the hydrogen pressure in the catalytic hydrogenation reaction is 0.5-2.8 MPa, and the reaction time is 0.5-4 h.

[0015] Furthermore, the temperature of the catalytic hydrogenation reaction is 40-50℃, the hydrogen pressure is 2-2.5MPa, and the reaction time is 1-2h.

[0016] Furthermore, the catalyst is a reverse nickel-based catalyst aMO x / bNi. This refers to a small amount of oxide supported on a metallic nickel substrate. In the active component, the oxide MO... x The catalyst is selected from at least one of magnesium oxide, aluminum oxide, zirconium oxide, lanthanum oxide, and yttrium oxide, with magnesium oxide being preferred. The loading of the metal oxide is 5-40 wt% (preferably 10-20 wt%) of the catalyst mass. The mass fraction of nickel metal in the catalyst is 60-95 wt% of the catalyst mass.

[0017] Furthermore, the catalyst was prepared using a co-precipitation method, and the preparation process included the following steps:

[0018] 1) Dissolve the M metal salt and Ni metal salt in water by stirring to obtain a metal salt solution; then prepare a precipitant solution separately for later use;

[0019] The amounts of the M and Ni metal salts are determined based on the catalyst aMO. x The corresponding mass fractions a and b in / bNi are used to determine this.

[0020] 2) Add the precipitant solution from step 1) dropwise to the metal salt solution, while simultaneously adding a dispersant. Titrate until the pH of the solution is 9-11. The amount of precipitant solution added is determined by the pH of the solution. Then let it stand, age, filter to obtain a solid product, wash, and dry to obtain a solid product.

[0021] 3) Grind the solid product obtained in step 2) into powder, and carry out a reduction reaction in the presence of hydrogen to obtain a catalyst.

[0022] Further, in step 1), M is at least one of magnesium, aluminum, zirconium, lanthanum, and yttrium; the magnesium metal salt is at least one of magnesium nitrate hexahydrate and magnesium chloride; the aluminum metal salt is at least one of aluminum nitrate nonahydrate and aluminum chloride; the zirconium metal salt is at least one of zirconium nitrate pentahydrate, zirconium tetrachloride, zirconium oxychloride, and zirconium sulfate; the lanthanum metal salt is at least one of lanthanum nitrate hexahydrate and lanthanum chloride; the yttrium metal salt is at least one of yttrium nitrate hexahydrate, yttrium chloride, and yttrium sulfate; and the nickel metal salt is at least one of nickel nitrate hexahydrate, nickel acetate, and nickel chloride.

[0023] Further, in step 1), the precipitant is at least one of sodium hydroxide, ammonia, and sodium bicarbonate. The concentration of the precipitant solution is 0.2-2 mol·L⁻¹. -1 Studies have shown that excessively high precipitant concentrations can lead to rapid precipitation of metal salts, uneven particle dispersion, and consequently, performance degradation.

[0024] Further, in step 2), the washing operation is as follows: wash with deionized water until neutral. The drying operation is as follows: dry at 120-130℃ to constant weight.

[0025] Further, in step 2), the dispersant is at least one of polyethylene glycol 400, polyvinyl alcohol, and polyvinylpyrrolidone K30. The amount of dispersant added is calculated based on the total amount of substance of the M metal element in the raw material M metal salt and the Ni element in the Ni metal salt. When the total amount of substance is 0.1 mol, the amount of dispersant added is 3-5 mL. The addition of dispersant is beneficial to maintaining the uniform dispersion of M and Ni.

[0026] Furthermore, in step 2), the settling time is more than 0.5 hours; the aging temperature is 80-90℃, and the aging time is more than 8 hours.

[0027] Further, in step 3), the solid product obtained in step 2) is ground into powder using a mortar and pestle.

[0028] Furthermore, in step 3), the amount of hydrogen introduced is sufficient to reduce the nickel in the solid product that exists in a positive oxidation state (such as nickel hydroxide or nickel oxide) to elemental nickel. Generally, the amount of hydrogen introduced is excessive.

[0029] Furthermore, in step 3), hydrogen reduction is used, and the introduced gas can be hydrogen or a hydrogen-argon mixture. From a safety perspective, a hydrogen-argon mixture with a hydrogen volume ratio of 5-10% is preferred.

[0030] Furthermore, in step 3), the temperature of the reduction reaction is 400-650℃, and the heating rate is 2-5℃·min. -1 The reduction reaction time is 1-4 hours. Studies have shown that excessively low reduction temperatures are detrimental to the formation of strong interactions between Ni and oxides. Reduction times less than 1 hour are unfavorable for the formation of a metallic Ni substrate.

[0031] The reverse nickel-based catalyst of this invention has a nickel metal mass fraction of 60-95 wt% and an oxide mass fraction of 5-40 wt%. By reversing the traditional structure of loading active components onto metal oxides, a nickel-based catalyst with strong metal-oxide interactions is constructed, which significantly improves hydrogenation performance and enables the one-step full hydrogenation of furanaldehyde derivatives to tetrahydrofuranol at a lower reaction temperature.

[0032] In this invention, a small amount of oxide is supported on aNi substrate in aMO x The / bNi catalyst can efficiently catalyze the one-step complete hydrogenation of furan derivatives to tetrahydrofuranol at relatively low temperatures. Among them, the reversed-phase catalyst aMgO / bNi catalyst obtained by supporting MgO on a Ni substrate exhibits the best performance. This is because Ni and MgO more readily form a solid solution structure, and Ni is then subjected to high-temperature H2 to hydrogenate the Ni... 2+ Reduction leads to lattice distortion between Ni and MgO, inducing strong interactions between them and generating numerous electron-rich Ni sites. Simultaneously, the strongly basic sites provided by MgO effectively adsorb substrates and H2 molecules. The abundant metallic nickel in the reversed-phase structure enhances the H2 dissociation ability. Under the H overflow effect at the highly active reversed-phase Ni-O-Mg interface, efficient hydrogenation of aldehyde groups and furan rings is achieved. Furthermore, the unique structural design between Ni and MgO effectively stabilizes the active Ni sites, allowing for multiple cycles without deactivation under mild conditions.

[0033] This invention enables the one-step hydrogenation of bio-based furan derivatives to tetrahydrofuran alcohol under mild conditions. The method utilizes an economical and readily available reverse-phase nickel-based catalyst, MOx / Ni, in a green medium such as water or alcohols. The hydrogenation process achieves high conversion and high selectivity at room temperature or a relatively low reaction temperature (25-55°C). Compared to traditional supported catalysts, which suffer from high energy consumption, complex and costly catalyst preparation methods, the catalytic system developed in this invention offers advantages under the same reaction conditions. These advantages include a mild and green catalytic system, simple and low-cost catalyst preparation, wide applicability, easy separation, and regeneration. Furthermore, it exhibits significantly improved hydrogenation activity, excellent resistance to deactivation, and broad substrate versatility, substantially reducing reaction energy consumption and equipment investment costs. This makes it highly attractive for practical industrial applications and more conducive to large-scale industrial use.

[0034] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0035] 1. This invention provides a highly catalytically active reversed non-noble metal aMO x The preparation method of / bNi catalyst is simple and cost-effective. A precursor is prepared by co-precipitation of M and Ni metal salt solutions with precipitants such as sodium hydroxide, followed by direct high-temperature hydrogen reduction to obtain the catalyst aMO. x / bNi. This catalyst exhibits excellent catalytic performance and thermal stability in the full hydrogenation of bio-based furan derivatives such as furfural, furfuryl alcohol, 5-methylfurfural, 5-methylfurfural, 5-hydroxymethylfurfural, and 2,5-furandimethylethanol to the corresponding tetrahydrofuran alcohols. Furthermore, the catalyst is magnetically recyclable and possesses good regenerability.

[0036] 2. The catalyst of the present invention has a green and mild catalytic system, which can selectively produce tetrahydrofuran alcohol from bio-based furan derivatives in one step at room temperature and a relatively low reaction temperature (25-55°C) in water or green alcohol solvents. Compared with the high-cost catalysts and high-temperature, high-pressure and highly toxic organic solvents required in existing reaction processes, the method disclosed in the present invention has a lower cost and a milder and greener reaction system.

[0037] 3. The method for preparing tetrahydrofuranol using the catalyst and hydrogenation of this invention achieves high yields (90-99%) of various target products. With the catalyst of this invention, under optimized process conditions (40℃, 10mL water, 2MPa H2, 1h), the yields of bio-based furan derivatives such as furfural, 5-methylfurfural, and 5-hydroxymethylfurfural to their corresponding tetrahydrofuranol compounds are all above 90%, and the yield remains above 80% even after 10 catalyst cycles. Furthermore, the catalyst retains its original catalytic performance after secondary hydrogen reduction, which is highly attractive for industrial applications. The catalyst is magnetically recoverable, stable, and has good regenerability, possessing potential for large-scale industrial application. Attached Figure Description

[0038] Figure 1 This is a high-resolution transmission electron microscope image of the reversed 0.1MgO / 0.9Ni catalyst obtained in Example 1;

[0039] Figure 2 The image shows the X-ray diffraction pattern of the reversed 0.1MgO / 0.9Ni catalyst obtained in Example 1.

[0040] Figure 3 The figure shows the hydrogen temperature-programmed reduction curve of the reversed 0.1MgO / 0.9Ni catalyst obtained in Example 1.

[0041] Figure 4The image shows the physical specimen of the reversed 0.1MgO / 0.9Ni catalyst obtained in Example 1.

[0042] Figure 5 This is a diagram of the reaction apparatus used to prepare the catalyst in Example 1;

[0043] Figure 6 Chemical reaction route for the hydrogenation of furfural / furfuryl alcohol to prepare tetrahydrofurfuryl alcohol;

[0044] Figure 7 Chemical reaction route for the hydrogenation of 5-methylfurfural / 5-methylfurfural to 5-methyltetrahydrofurfural;

[0045] Figure 8 A chemical reaction route for the preparation of tetrahydrofurandimethyl methanol from 5-hydroxymethylfurfural / 2,5-furandimethyl methanol by hydrogenation. Detailed Implementation

[0046] The present invention has been further described in detail above through specific embodiments.

[0047] Example 1

[0048] The preparation of the 0.1MgO / 0.9Ni catalyst (0.1 and 0.9 are mass fraction ratios) was carried out by co-precipitation method, and the preparation process included the following steps:

[0049] 1) Dissolve 0.636 g of magnesium nitrate hexahydrate and 4.490 g of nickel nitrate hexahydrate in 30 mL of water by stirring thoroughly to obtain a metal salt solution; then prepare 50 mL of a 0.5 mol·L⁻¹ solution separately. -1 The sodium hydroxide solution was prepared as a precipitant solution and was to be used later.

[0050] 2) At room temperature, the precipitant solution from step 1) was added dropwise to the metal salt solution, while 3 mL of dispersant polyethylene glycol 400 was added dropwise. The solution was titrated until the pH value was 10 ± 0.1. The amount of precipitant solution added was determined by the pH value of the solution. The solution was then allowed to stand for 0.5 h and then aged in an oil bath at 80 °C for 8 h. After the reaction, the solid product was obtained by filtration. The solid product was washed with deionized water until neutral and then dried at 120 °C to constant weight.

[0051] 3) Grind the solid product obtained in step 2) into powder using a mortar and pestle. Then, under a hydrogen-argon mixed atmosphere with a hydrogen volume ratio of 5% and a hydrogen flow rate of 50 mL / min... -1 The heating rate is 5℃·min -1 The catalyst was obtained by reducing it with hydrogen at 600℃ for 2 hours.

[0052] Figure 1 This is a high-resolution transmission electron microscope image of the reversed 0.1MgO / 0.9Ni catalyst obtained in Example 1;

[0053] Figure 2 The image shows the X-ray diffraction pattern of the reversed 0.1MgO / 0.9Ni catalyst obtained in Example 1.

[0054] Figure 3 The figure shows the hydrogen temperature-programmed reduction curve of the reversed 0.1MgO / 0.9Ni catalyst obtained in Example 1.

[0055] Figure 1 It was captured using a field emission transmission electron microscope (model: USA - Thermo Fisher-Talos F200X).

[0056] Figure 2 The X-ray diffraction (XRD) results were obtained using a high-power powder X-ray diffractometer (Rigaku Smart Lab SE) with Cu-Kα rays (λ = 1.5418 Å) at 40 kV and 50 mA (scanning range: 2θ = 5–90°, scan rate: 10°·min). -1 ).

[0057] Figure 3 The results were obtained using a ChemBET Pulsar PM20 instrument. Before testing, 80 mg of catalyst sample was weighed and placed in a U-shaped quartz tube, under an argon flow of 50 mL / min. -1 ) at 10℃·min -1 The temperature was increased to 200℃ and held for 1 hour to remove adsorbed water. After cooling to 50℃, a 10% (v / v) H2 / Ar mixture (50 mL / min) was introduced. -1 After stabilizing the baseline for 0.5 h, the mixture was then placed in an H2 / Ar mixed atmosphere with a volume ratio of 10% at 10 °C / min. -1 The temperature was increased to 800°C at a rate that allowed for the desorbed gas to be detected by a TCD detector.

[0058] Figure 4 The image shows the physical specimen of the reversed 0.1MgO / 0.9Ni catalyst obtained in Example 1.

[0059] Figure 5 This is a diagram of the reaction apparatus used to prepare the catalyst in Example 1.

[0060] Example 2

[0061] This embodiment describes a method for preparing tetrahydrofuranol by hydrogenation of a bio-based furan derivative:

[0062] The reaction vessel was a batch stainless steel reactor. 0.050 g of catalyst, 1 mmol of the substrate bio-based furan derivative, and 10 mL of solvent were added to the reactor. The reaction was carried out at 40 °C and 2 MPa H₂ pressure for 1 h. After the reaction, the reactor was immediately cooled to room temperature in an ice bath. The reaction solution was then removed, filtered through a 0.22 μm organic microporous membrane, and placed into a chromatographic sample vial. The products were analyzed and detected using a gas chromatograph (Nexis GC-2030).

[0063] Example 3

[0064] The 0.1MgO / 0.9Ni catalyst obtained in Example 1 was used to catalyze the one-pot conversion of 5-hydroxymethylfurfural to tetrahydrofurandiethanol. The catalyst was 0.050 g of the 0.1MgO / 0.9Ni catalyst obtained in Example 1, and the substrate, a bio-based furan derivative, was 0.126 g of 5-hydroxymethylfurfural. Methanol, ethanol, isopropanol, or water were used as solvents, and other operating conditions were the same as in Example 2. The products were analyzed, and the conversion rate of 5-hydroxymethylfurfural, the selectivity of 2,5-furandiethanol, and the selectivity of tetrahydrofurandiethanol are shown in Table 1.

[0065] Table 1. Results of the catalytic production of tetrahydrofurandimethyl from 5-hydroxymethylfurfural under different reaction solvents.

[0066]

[0067] Table 1 shows that the solvent significantly affects the selectivity of tetrahydrofurandiethanol. Water or isopropanol exhibits better catalytic performance, primarily due to their strong hydrogen-bonding ability, enabling them to interact with the catalyst surface and promote proton transfer, thus facilitating the reaction between the reactants and hydrogen. Furthermore, the strong polarity of water and isopropanol optimizes the adsorption strength of 5-hydroxymethylfurfural on the catalyst surface, preventing premature desorption of the reaction intermediate 2,5-furandiethanol. Additionally, water is more conducive to the subsequent separation of the product.

[0068] Example 4

[0069] The 0.1MgO / 0.9Ni catalyst obtained in Example 1 was used to catalyze the one-pot conversion of 5-hydroxymethylfurfural to tetrahydrofurandiethanol. The catalyst was 0.050 g of the 0.1MgO / 0.9Ni catalyst obtained in Example 1, the substrate was the bio-based furan derivative 5-hydroxymethylfurfural (0.126 g), and the solvent was water. The reaction temperatures were 25℃, 30℃, 40℃, 50℃, and 55℃, respectively, with other conditions the same as in Example 2. The conversion rate of 5-hydroxymethylfurfural, the selectivity of 2,5-furandiethanol, and the selectivity of tetrahydrofurandiethanol were analyzed and are shown in Table 2.

[0070] Table 2. Results of the catalytic production of tetrahydrofurandimethyl from 5-hydroxymethylfurfural at different reaction temperatures.

[0071]

[0072] As shown in Table 2, the 0.1MgO / 0.9Ni catalyst exhibits excellent hydrogenation performance, achieving a 52.4% conversion of 5-hydroxymethylfurfural and a 61.9% selectivity for tetrahydrofurandiethanol at room temperature. Furthermore, the conversion of 5-hydroxymethylfurfural and the selectivity for tetrahydrofurandiethanol gradually increase with increasing reaction temperature, reaching optimal catalytic performance at 40℃. Further increases in reaction temperature lead to an increase in side reactions, primarily including the hydrogenation and deoxygenation of 5-hydroxymethylfurfural to produce 5-methylfurfural and the further hydrogenolysis of tetrahydrofurandiethanol to produce 1,2,6-hexanetriol, resulting in a decrease in the selectivity of tetrahydrofurandiethanol.

[0073] Example 5

[0074] The 0.1MgO / 0.9Ni catalyst obtained in Example 1 was applied to the one-pot conversion of 5-hydroxymethylfurfural to tetrahydrofurandiethanol. The catalyst was 0.050 g of the 0.1MgO / 0.9Ni catalyst obtained in Example 1, the substrate was the bio-based furan derivative 5-hydroxymethylfurfural (0.126 g), the solvent was water, and the hydrogen pressure was 0.5 MPa, 1 MPa, 1.5 MPa, 2 MPa, 2.5 MPa, and 3 MPa, respectively. Other operating conditions were the same as in Example 2. The conversion rate of 5-hydroxymethylfurfural, the selectivity of 2,5-furandiethanol, and the selectivity of tetrahydrofurandiethanol were analyzed and are shown in Table 3.

[0075] Table 3. Results of the catalytic production of tetrahydrofurandimethyl from 5-hydroxymethylfurfural under different hydrogen pressures.

[0076]

[0077] As shown in Table 3, the selectivity of tetrahydrofurandiethanol first increases and then decreases with increasing hydrogen pressure. The selectivity of tetrahydrofurandiethanol is highest at a hydrogen pressure of 2 MPa, with a yield of 91.2%. With further increases in pressure, side reactions increase, and the selectivity of tetrahydrofurandiethanol decreases.

[0078] Example 6

[0079] The 0.1MgO / 0.9Ni catalyst obtained in Example 1 was applied to the one-pot conversion of 5-hydroxymethylfurfural to tetrahydrofurandiethanol. The catalyst was 0.050 g of the 0.1MgO / 0.9Ni catalyst obtained in Example 1, the substrate was the bio-based furan derivative 5-hydroxymethylfurfural (0.126 g), and the solvent was water. The reaction times were 0.25 h, 0.5 h, 1 h, 1.5 h, 2 h, 3 h, and 4 h, respectively, with other conditions the same as in Example 2. The products were analyzed, and the conversion rates of 5-hydroxymethylfurfural, the selectivity of 2,5-furandiethanol, and the selectivity of tetrahydrofurandiethanol are shown in Table 4.

[0080] Table 4. Results of the catalytic production of tetrahydrofurandimethyl from 5-hydroxymethylfurfural at different reaction times.

[0081]

[0082] Table 4 shows that the hydrogenation reaction pathway follows the reaction sequence of 5-hydroxymethylfurfural—2,5-furandiethanol—tetrahydrofurandiethanol, with 2,5-furandiethanol being the intermediate. As the reaction time increases, the selectivity of tetrahydrofurandiethanol first increases and then decreases. The decrease is mainly due to the further hydrogenolysis of tetrahydrofurandiethanol to yield 1,2,6-hexanetriol and other byproducts.

[0083] Example 7

[0084] The preparation method of the 0.05MgO / 0.95Ni catalyst is the same as in Example 1, except that the amounts of nickel nitrate hexahydrate and magnesium nitrate hexahydrate are 4.740 g and 0.318 g, respectively.

[0085] Example 8

[0086] The preparation method of the 0.2MgO / 0.8Ni catalyst is the same as in Example 1, except that the amounts of nickel nitrate hexahydrate and magnesium nitrate hexahydrate are 3.396 g and 1.272 g, respectively.

[0087] Example 9

[0088] The preparation method of the 0.3MgO / 0.7Ni catalyst is the same as in Example 1, except that the amounts of nickel nitrate hexahydrate and magnesium nitrate hexahydrate are 3.472 g and 1.803 g, respectively.

[0089] Example 10

[0090] The preparation method of the 0.4MgO / 0.6Ni catalyst is the same as in Example 1, except that the amounts of nickel nitrate hexahydrate and magnesium nitrate hexahydrate are 2.990 g and 2.410 g, respectively.

[0091] Example 11

[0092] The preparation method of the 0.9MgO / 0.1Ni catalyst is the same as in Example 1, except that the amounts of nickel nitrate hexahydrate and magnesium nitrate hexahydrate are 0.499 g and 5.724 g, respectively.

[0093] Example 12

[0094] The catalysts from Examples 1 and 7-11 were used to catalyze the one-pot conversion of 5-hydroxymethylfurfural to tetrahydrofurandiethanol. The substrate was 0.126 g of the bio-based furan derivative 5-hydroxymethylfurfural, and the solvent was water. Other conditions were the same as in Example 2. The products were analyzed, and the conversion rates of 5-hydroxymethylfurfural, the selectivity of 2,5-furandiethanol, and the selectivity of tetrahydrofurandiethanol are shown in Table 5.

[0095] Table 5. Results of the production of tetrahydrofurandimethyl from 5-hydroxymethylfurfural using different catalysts.

[0096]

[0097] As shown in Table 5, compared with the traditional nickel-based supported catalyst (Example 11), the reversed nickel-based catalyst exhibits superior catalytic activity. At a low temperature of 40°C, the traditional supported catalyst 0.9MgO / 0.1Ni only achieves a 5-hydroxymethylfurfural conversion of 20.8% and a 2,5-furandiethanol conversion of 100%. However, in the reversed catalyst, the 5-hydroxymethylfurfural conversion gradually increases with the increase of the Ni substrate mass ratio, and the product is further hydrogenated from 2,5-furandiethanol to tetrahydrofurandiethanol. 0.05MgO / 0.95Ni and 0.1MgO / 0.9Ni show excellent hydrogenation performance, with corresponding tetrahydrofurandiethanol selectivity exceeding 90%. This is mainly attributed to the strong interaction between the supported MgO and the Ni substrate, which promotes the dissociation of H2, thus facilitating the deep hydrogenation of 5-hydroxymethylfurfural. As the loading ratio of MgO increases, the interaction between Ni and MgO gradually weakens, resulting in the product mainly being 2,5-furandiethanol after hydrogenation of 5-hydroxymethylfurfural aldehyde.

[0098] Example 13

[0099] The 0.1MgO / 0.9Ni catalyst obtained in Example 1 was used to catalyze the one-pot conversion of 5-hydroxymethylfurfural to tetrahydrofurandiethanol. The catalyst was 0.050 g of the 0.1MgO / 0.9Ni catalyst obtained in Example 1, the substrate bio-based furan derivative was 0.126 g of 5-hydroxymethylfurfural, the solvent was water, and other implementation conditions were the same as in Example 2.

[0100] After the reaction was completed, the catalyst was separated and recovered: the catalyst after the reaction was filtered through a magnetic stir bar, thoroughly washed with anhydrous ethanol, and then dried in a vacuum drying oven. It was reused a total of 10 times after recovery. After the 10th use, the catalyst was recovered and subjected to a second hydrogen reduction: the dried catalyst was placed back into a tube furnace for hydrogen reduction, under the same conditions as step 3 in Example 1, specifically: in a hydrogen-argon mixed atmosphere with a hydrogen volume ratio of 5%, the hydrogen flow rate was 50 mL / min. -1 The heating rate is 5℃·min -1 Hydrogen reduction at 600℃ for 2 hours.

[0101] After each reaction, the products were analyzed and detected. The conversion rate of 5-hydroxymethylfurfural, the selectivity of 2,5-furandiethanol, and the selectivity of tetrahydrofurandiethanol are shown in Table 6.

[0102] Table 6. Results of the catalytic production of tetrahydrofurandiethanol from 5-hydroxymethylfurfural at different catalyst cycle numbers.

[0103]

[0104] As shown in Table 6, the catalyst exhibits good thermal stability and regenerability. After 10 cycles, the selectivity for tetrahydrofurandiethanol remains above 80%, and the catalyst retains its original catalytic activity after secondary hydrogen reduction. Furthermore, the catalyst is magnetic, facilitating separation, recovery, and reuse.

[0105] Example 14

[0106] The 0.1MgO / 0.9Ni catalyst obtained in Example 1 was used to catalyze the one-pot conversion of bio-based furan derivatives to tetrahydrofuranol. The catalyst was 0.050 g of the 0.1MgO / 0.9Ni catalyst obtained in Example 1. The bio-based furan derivative substrate consisted of 0.096 g of furfural, 0.098 g of furfuryl alcohol, 0.110 g of 5-methylfurfural, 0.112 g of 5-methylfurfural, 0.126 g of 5-hydroxymethylfurfural, or 0.128 g of 2,5-furandimethylethanol. The solvent was water, and other conditions were the same as in Example 2. The product analysis and detection results, including substrate conversion and tetrahydrofuranol selectivity, are shown in Table 7.

[0107] Table 7 Results of the catalytic synthesis of tetrahydrofuranol from different reaction substrates

[0108]

[0109] Note: Tetrahydrofuranol obtained by hydrogenating furfural and furfuryl alcohol is tetrahydrofuranol; tetrahydrofuranol obtained by hydrogenating 5-methylfurfural and 5-methylfurfural alcohol is 5-methyltetrahydrofuranol; tetrahydrofuranol obtained by hydrogenating 5-hydroxymethylfurfural and 2,5-furandiethanol is tetrahydrofurandiethanol.

[0110] As shown in Table 7, the 0.1MgO / 0.9Ni catalyst exhibits excellent hydrogenation performance for bio-based furan derivatives under near-room temperature conditions, with selectivity for the corresponding tetrahydrofuran alcohols all exceeding 90%. Furthermore, the hydrogenation activity of the substrates follows the order: furan alcohols > furan aldehydes, and furfural / furfuryl alcohol > 5-methylfurfural / 5-methylfurfuryl alcohol > 5-hydroxymethylfurfural / 2,5-furandimethyl. This is mainly attributed to the increase in reaction steps. Simultaneously, with the introduction of methyl and hydroxymethyl groups, steric hindrance gradually increases, affecting the adsorption strength of the substrate and reducing the hydrogenation activity.

[0111] Example 15

[0112] The preparation of the 0.1Al2O3 / 0.9Ni catalyst was carried out in the same way as in Example 1, except that the magnesium salt was replaced with the corresponding aluminum metal salt. Specifically, the amounts of nickel nitrate hexahydrate and aluminum nitrate nonahydrate were 4.490 g and 0.842 g, respectively.

[0113] Example 16

[0114] The preparation method of the 0.1ZrO2 / 0.9Ni catalyst is the same as in Example 1, except that the magnesium salt is replaced with the corresponding zirconium metal salt. Specifically, the amounts of nickel nitrate hexahydrate and zirconium nitrate pentahydrate are 4.490 g and 0.348 g, respectively.

[0115] Example 17

[0116] The preparation method of the 0.1La2O3 / 0.9Ni catalyst is the same as in Example 1, except that the magnesium salt is replaced with the corresponding lanthanum metal salt. Specifically, the amounts of nickel nitrate hexahydrate and lanthanum nitrate hexahydrate are 4.490 g and 0.267 g, respectively.

[0117] Example 18

[0118] The preparation method of the 0.1Y2O3 / 0.9Ni catalyst is the same as in Example 1, except that the magnesium salt is replaced with the corresponding yttrium metal salt. Specifically, the amounts of nickel nitrate hexahydrate and yttrium nitrate hexahydrate are 4.490 g and 0.339 g, respectively.

[0119] Example 19

[0120] The catalysts prepared in Examples 1 and 15-18 were used to catalyze the one-pot conversion of furfural to tetrahydrofurfuryl alcohol. The substrate, a bio-based furan derivative, was 0.096 g of furfural, and the catalyst was 0.050 g. The solvent was water, and other operating conditions were the same as in Example 2. The products were analyzed, and the results of different catalysts catalyzing the conversion of furfural to tetrahydrofurfuryl alcohol are shown in Table 8.

[0121] Table 8 Results of furfural to tetrahydrofurfural catalysis using different catalysts

[0122]

[0123] As shown in Table 8, both 1MOx / 9Ni catalysts can effectively catalyze the conversion of furfural to tetrahydrofurfuryl alcohol. The order of hydrogenation performance is MgO>Al2O3>ZrO2>Y2O3>La2O3. This is attributed to the strong interaction between MgO and nickel, which can regulate the electronic state of Ni, enhance the adsorption and activation capacity of Ni for H2, and reduce the energy barrier of hydrogenation reaction.

[0124] Example 20

[0125] The catalysts prepared in Examples 1 and 15-18 were used to catalyze the one-pot conversion of 5-hydroxymethylfurfural to tetrahydrofurandimethyl. The substrate, a bio-based furan derivative, was 0.126 g of 5-hydroxymethylfurfural, and the catalyst was 0.050 g. The solvent was water, and other conditions were the same as in Example 2. The products were analyzed, and the results of different catalysts catalyzing the conversion of 5-hydroxymethylfurfural to tetrahydrofurandimethyl are shown in Table 9.

[0126] Table 9. Results of the production of tetrahydrofurandimethyl from 5-hydroxymethylfurfural using different catalysts.

[0127]

[0128] As can be seen from Table 9, the reversed-phase MOx / Ni catalysts with different metal oxides supported on nickel all exhibited the same catalytic conversion behavior as the full hydrogenation reaction of furfural, indicating that the catalytic system has good substrate applicability.

[0129] As can be seen, the inverted aMO of the present invention x / bNi catalyst can efficiently catalyze the one-pot conversion of bio-based furan derivatives into tetrahydrofuran alcohols under mild conditions (40℃, water solvent, 2MPa H2, 1h, product yield greater than 90%). Moreover, the catalyst is simple to prepare, cost-effective, thermally stable and regenerable, and has the potential for large-scale application.

[0130] Figure 6 Chemical reaction route for the hydrogenation of furfural / furfuryl alcohol to prepare tetrahydrofurfuryl alcohol;

[0131] Figure 7 Chemical reaction route for the hydrogenation of 5-methylfurfural / 5-methylfurfural to 5-methyltetrahydrofurfural;

[0132] Figure 8 A chemical reaction route for the preparation of tetrahydrofurandimethyl methanol from 5-hydroxymethylfurfural / 2,5-furandimethyl methanol by hydrogenation.

Claims

1. A method for preparing tetrahydrofuranol by hydrogenation of a bio-based furan derivative, characterized in that, Includes the following steps: Using bio-based furan derivatives as reactants, in the presence of a solvent, with hydrogen as the hydrogen source, and employing the catalyst aMO... x / bNi undergoes catalytic hydrogenation to produce tetrahydrofuran alcohols in a one-pot process; where a and b are the mass fractions of the corresponding components in the catalyst, wherein a is 5-40 wt%, b is 60-95 wt%, and a+b=100%; The temperature for the catalytic hydrogenation reaction is 25-55℃; The bio-based furan derivative is one of furfural, furfuryl alcohol, 5-methylfurfural, 5-methylfurfural alcohol, 5-hydroxymethylfurfural, and 2,5-furandimethyl alcohol; the tetrahydrofuran alcohol is the tetrahydrofuran alcohol corresponding to the bio-based furan derivative; the tetrahydrofuran alcohol corresponding to furfural and furfuryl alcohol is tetrahydrofurfural alcohol. The tetrahydrofuranol corresponding to 5-methylfurfural and 5-methylfurfural alcohol is 5-methyltetrahydrofurfural alcohol; the tetrahydrofuranol corresponding to 5-hydroxymethylfurfural and 2,5-furandiethanol is tetrahydrofurandiethanol. The catalyst is a reverse nickel-based catalyst aMO x / bNi; Oxide MO x It is at least one of magnesium oxide, aluminum oxide, zirconium oxide, lanthanum oxide, and yttrium oxide.

2. The method for preparing tetrahydrofuranol by hydrogenation of bio-based furan derivatives according to claim 1, characterized in that, The loading of the metal oxide is 10-20 wt% of the catalyst mass; the solvent is at least one of methanol, ethanol, isopropanol, and water.

3. The method for preparing tetrahydrofuranol by hydrogenation of bio-based furan derivatives according to claim 1 or 2, characterized in that, The hydrogen pressure in the catalytic hydrogenation reaction is 0.5-2.8 MPa, and the reaction time is 0.5-4 h.

4. The method for preparing tetrahydrofuranol by hydrogenation of bio-based furan derivatives according to claim 3, characterized in that, The catalytic hydrogenation reaction is carried out at a temperature of 40-50℃, a hydrogen pressure of 2-2.5MPa, and a reaction time of 1-2h.

5. The method for preparing tetrahydrofuranol by hydrogenation of bio-based furan derivatives according to claim 1 or 2, characterized in that, The catalyst was prepared by co-precipitation, and the preparation process included the following steps: 1) Dissolve the M metal salt and Ni metal salt in water by stirring to obtain a metal salt solution; then prepare a precipitant solution separately for later use; In step 1), M is at least one of magnesium, aluminum, zirconium, lanthanum, and yttrium; the magnesium metal salt is at least one of magnesium nitrate hexahydrate and magnesium chloride; the aluminum metal salt is at least one of aluminum nitrate nonahydrate and aluminum chloride; the zirconium metal salt is at least one of zirconium nitrate pentahydrate, zirconium tetrachloride, zirconium oxychloride, and zirconium sulfate; the lanthanum metal salt is at least one of lanthanum nitrate hexahydrate and lanthanum chloride; the yttrium metal salt is at least one of yttrium nitrate hexahydrate, yttrium chloride, and yttrium sulfate; and the nickel metal salt is at least one of nickel nitrate hexahydrate, nickel acetate, and nickel chloride. The amounts of the M and Ni metal salts are determined based on the catalyst aMO. x The corresponding mass fractions a and b in / bNi are used to determine this; 2) Add the precipitant solution from step 1) dropwise to the metal salt solution, while simultaneously adding the dispersant. Titrate until the pH of the solution is 9-11. The amount of precipitant solution added is determined by the pH of the solution. Then let it stand, age, filter to obtain a solid product, wash, and dry to obtain a solid product. 3) Grind the solid product obtained in step 2) into powder, and carry out a reduction reaction in the presence of hydrogen to obtain a catalyst.

6. The method for preparing tetrahydrofuranol by hydrogenation of bio-based furan derivatives according to claim 5, characterized in that, In step 1), the precipitant is at least one of sodium hydroxide, ammonia, and sodium bicarbonate; the concentration of the precipitant solution is 0.2-2 mol·L⁻¹. -1 .

7. The method for preparing tetrahydrofuranol by hydrogenation of bio-based furan derivatives according to claim 5, characterized in that, In step 2), the washing operation is to wash with deionized water until neutral; the drying operation is to dry at 120-130℃ until constant weight.

8. The method for preparing tetrahydrofuranol by hydrogenation of bio-based furan derivatives according to claim 5, characterized in that, In step 2), the dispersant is at least one of polyethylene glycol 400, polyvinyl alcohol, and polyvinylpyrrolidone K30; the amount of dispersant added is based on the total amount of substance of the M metal element in the raw material M metal salt and the Ni element in the Ni metal salt. When the total amount of substance is 0.1 mol, the amount of dispersant added is 3-5 mL.

9. The method for preparing tetrahydrofuranol by hydrogenation of bio-based furan derivatives according to claim 5, characterized in that, In step 2), the settling time is more than 0.5 hours; the aging temperature is 80-90℃ and the aging time is more than 8 hours.

10. The method for preparing tetrahydrofuranol by hydrogenation of bio-based furan derivatives according to claim 5, characterized in that, In step 3), the temperature of the reduction reaction is 400-650℃, and the heating rate is 2-5℃·min. -1 The reduction reaction takes 1-4 hours.

Citation Information

Patent Citations

  • Preparation method of 2, 5-tetrahydrofuran dimethanol

    CN111233797A

  • Preparation method of 2,5-tetrahydrofurandimethanol (THFDM)

    CN113651780A

  • A method for preparing 2,5-tetrahydrofuran dimethanol by hydrogenating 5-hydroxymethylfurfural

    CN119751385A

  • Pd / NiCoOx catalyst, preparation method and method for catalytically hydrogenating furan aldehyde alcohol compound

    CN119771443A

  • Preparation method and application of biomass-based carbon material loaded bimetallic catalyst

    CN121016814A