A weather-resistant, acid and alkali-resistant fluorinated protective coating and its preparation method

By compounding materials such as fluoroolefin-vinyl ether copolymer resin and combining them with fluorinated organic-inorganic hybrid UV absorbers, a dense network structure is formed, which solves the contradiction between optical performance and weather resistance in outdoor building transparent protective coatings, and achieves coating effects with high transparency, acid and alkali resistance and long-term weather resistance.

CN123063009APending Publication Date: 2026-11-10ENXI NEW MATERIALS (SHANGHAI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611265895.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing transparent protective coatings for outdoor buildings cannot simultaneously meet the requirements of high visible and infrared transmittance, high ultraviolet blocking, resistance to strong acids and alkalis, long-term weather resistance, and high transparency without whitening. They suffer from problems such as contradictory optical properties, poor compatibility between additives and fluorine matrix, weak chemical corrosion resistance, and insufficient long-term weather resistance.

Method used

It adopts a fluoroolefin-vinyl ether copolymer resin, ethylene-tetrafluoroethylene copolymer, and polyvinylidene fluoride composite matrix, combined with fluorine-containing organic-inorganic hybrid UV absorbers, compatibilizers and functional additives to form a dense network structure, achieving full-band UV blocking, acid and alkali corrosion resistance and ultra-long weather resistance.

Benefits of technology

It achieves high transparency in UV blocking, resistance to acid and alkali corrosion, extends the protective life of the coating, solves problems such as whitening, powdering, and yellowing due to aging of the coating, and improves the storage stability and multi-substrate compatibility of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063009A_ABST
    Figure CN123063009A_ABST
Patent Text Reader

Abstract

This invention discloses a weather-resistant, acid- and alkali-resistant fluorinated protective coating and its preparation method. The weather-resistant, acid- and alkali-resistant fluorinated protective coating comprises a base component and a curing agent in a mass ratio of 4-10:1. By mass percentage, the base component comprises: 40%-70% fluorinated polymer, 1%-16% organic-inorganic hybrid UV absorber, 0.5%-10% functional additives, 5%-20% compatibilizer, and organic solvent to make up to 100%. The fluorinated polymer is a compound of fluoroolefin-vinyl ether copolymer resin, ethylene-tetrafluoroethylene copolymer, and polyvinylidene fluoride. The method is as follows: the fluorinated polymer is added to the organic solvent and stirred until completely dissolved and free of particles; the organic-inorganic hybrid UV absorber and compatibilizer are added in batches and emulsified and dispersed by high-speed stirring; the functional additives are added while stirring at low speed, the viscosity is adjusted to 15-60s in a Coat-4 viscosity cup (25℃), and the mixture is filtered under negative pressure to obtain the base material; the base material and curing agent are then packaged separately.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of coating technology, and in particular to a weather-resistant, acid and alkali-resistant fluorinated protective coating and its preparation method. Background Technology

[0002] Currently, outdoor transparent protective coatings for buildings fall into three technical systems, all designed to achieve substrate protection and outdoor weather resistance. These are transparent acrylic outdoor coatings, transparent polyurethane weather-resistant coatings, and ordinary transparent fluorinated coatings. However, none of these three solutions can simultaneously satisfy the requirements of high visible and infrared transmittance, high ultraviolet blocking, resistance to strong acids and alkalis, long-term weather resistance, and high transparency without whitening. Specific shortcomings are as follows:

[0003] Optical properties are contradictory, and light transmission and UV blocking cannot be achieved simultaneously: When acrylic and polyurethane coatings do not add UV absorbers, the UV blocking rate is only 10%-20%, and ultraviolet rays can directly penetrate and degrade the substrate; after adding absorbers to improve protection, the coating yellows, the haze increases dramatically, and the visible light transmittance drops to below 75%; Existing ordinary fluorinated coatings use unmodified nano titanium dioxide, which has serious powder agglomeration, resulting in a cloudy and white coating with an infrared transmittance of less than 78%, which destroys the transparent decorative effect of building facades and cannot be adapted to high-end transparent facades.

[0004] The additives have extremely poor compatibility with the fluorine matrix, and their protective performance deteriorates rapidly: Conventional organic UV absorbers have no fluorine-containing functional groups and their polarity differs greatly from that of fluorinated polymers. After film formation, they continue to migrate and precipitate onto the coating surface, resulting in whitening and powdering after 3-6 months of outdoor use; Unmodified inorganic nanoparticles have high surface polarity and agglomerate and precipitate inside low surface energy fluorinated resins, causing severe sedimentation during coating storage and a reduction of more than 40% in UV protection capability after long-term use.

[0005] It has poor resistance to chemical corrosion and is not resistant to strong acid and alkali corrosion: the main chain of acrylic and polyurethane contains a large number of ester bonds and amino polar groups, which are easily damaged by outdoor acid rain (dilute sulfuric acid), wall salt and alkali, and industrial alkaline dust. It will bubble and peel off after soaking in 10% sodium hydroxide solution for 72 hours. Ordinary single-component PVDF fluoropolymer coatings have many internal pores and low cross-linking density, allowing acid and alkali media to penetrate quickly. They are prone to corrosion and failure in long-term industrial outdoor environments.

[0006] Insufficient long-term weather resistance, yellowing and chalking due to outdoor aging: Non-fluorinated coatings have low carbon-carbon bond energy, which leads to chain degradation under long-term UV irradiation, accelerating aging; Existing fluorinated coatings have a single UV protection mechanism, which cannot block the free radical chain reaction of photoaging. Artificial accelerated aging for 3000 hours results in less than 55% gloss retention, and yellowing, cracking and delamination occur after 1-2 years of outdoor use.

[0007] Poor compatibility of preparation process and low stability of finished product: Existing fluoropolymer coatings have low dispersion speed and no compatible system for formulation, resulting in large batch color difference and haze variation; single-component thermoplastic film formation has weak adhesion, with adhesion to aluminum alloy and concrete substrates below 3MPa and low construction error tolerance. Summary of the Invention

[0008] The technical problem to be solved by this invention is that existing solutions cannot simultaneously satisfy the requirements of high visible and infrared transmittance, high ultraviolet blocking, resistance to strong acids and alkalis, long-term weather resistance, and high transparency without whitening. This invention discloses a weather-resistant and acid-alkali-resistant fluorinated protective coating. This invention also discloses a method for preparing a weather-resistant and acid-alkali-resistant fluorinated protective coating. The coating is prepared by using a fluorinated olefin-vinyl ether copolymer resin, ethylene-tetrafluoroethylene copolymer, and polyvinylidene fluoride compounded with a fluorinated polymer matrix, and adding fluorinated organic-inorganic hybrid ultraviolet absorbers, compatibilizers, and functional additives. This coating achieves a comprehensive effect of high transparency, full-band ultraviolet blocking, resistance to acid and alkali corrosion, ultra-long weather resistance, and stable storage without precipitation, thereby overcoming the defects caused by existing technologies.

[0009] To solve the above-mentioned technical problems, the present invention provides the following technical solution:

[0010] In the first aspect, a weather-resistant and acid- and alkali-resistant fluorinated protective coating, comprising a base component and a curing agent in a mass ratio of 4-10:1;

[0011] By mass percentage, the base material composition comprises: 40%-70% fluoropolymer, 1%-16% organic-inorganic hybrid UV absorber, 0.5%-10% functional additives, 5%-20% compatibilizer, and organic solvents to bring the total to 100%.

[0012] The aforementioned weather-resistant and acid / alkali-resistant fluorinated protective coating comprises a fluorinated polymer composed of fluoroolefin-vinyl ether copolymer (FEVE), ethylene-tetrafluoroethylene copolymer (ETFE), and polyvinylidene fluoride (PVDF). The fluorine content in the fluoroolefin-vinyl ether copolymer is ≥30%, the fluorine content in the ethylene-tetrafluoroethylene copolymer is ≥55%, and the fluorine content in the polyvinylidene fluoride is ≥50%. A ternary compound is used to improve the matrix, enhancing acid and alkali resistance and overall weather resistance. The fluorine-carbon bond energy is 485 kJ / mol, far exceeding the energy of ultraviolet photons and the activation energy of acid-base hydrolysis. Cross-linking forms a dense network structure, blocking the penetration of corrosive media. Test data shows that after immersion in 10% sulfuric acid and 10% sodium hydroxide at room temperature for 500 hours, the coating exhibits no blistering, peeling, or discoloration. Existing acrylic coatings blister after 72 hours, and ordinary single-component fluorinated coatings show slight whitening after 120 hours, indicating a 72% or more improvement in chemical corrosion resistance. Simultaneously, the resin itself has a light transmittance of ≥95%, preserving the appearance and texture of the base material.

[0013] The aforementioned weather-resistant, acid and alkali-resistant fluorinated protective coating comprises an organic-inorganic hybrid UV absorber, which is a compound of a fluorinated triazine organic UV absorber and a fluorinated coupling agent-modified nano-inorganic powder in a mass ratio of 1:1-4. The fluorinated coupling agent-modified nano-inorganic powder is selected from one or more of 20-50nm modified rutile titanium dioxide and modified zinc oxide. The improved fluorinated hybrid UV absorption system balances light transmission and UV protection, with a particle size smaller than half the wavelength of visible light, effectively preventing light scattering, and a coating haze ≤1.2%. The visible light transmittance is ≥91%, and the infrared transmittance is ≥83%, achieving near-complete penetration. Inorganic reflection, organic conversion, and free radical capture result in a full-band UV blocking rate ≥95%. Compared with existing transparent fluorinated coatings, the UV blocking capability is improved by 27%, and the light transmittance is improved by 11%, completely resolving optical contradictions.

[0014] In the above-mentioned weather-resistant, acid and alkali-resistant fluorinated protective coating, the functional additive is one or more of the following: polymer block dispersant, polyether siloxane wetting agent, polyester leveling agent, silicone defoamer, and hindered amine light stabilizer.

[0015] In the above-mentioned weather-resistant, acid and alkali-resistant fluorinated protective coating, the compatibilizer is polymethyl methacrylate.

[0016] The functional additives and compatibilizers are combined to solve the defects of additive precipitation and agglomeration, eliminate the interfacial tension between additives and resins, and prevent stratification and precipitation after 3 months of storage; no surface precipitation or whitening after 2 years of outdoor use; compared with existing ordinary UV additive systems, the coating protection attenuation rate is reduced from 41% to 6%, which significantly extends the service life; at the same time, it does not negatively affect the coating hardness and adhesion.

[0017] The above-mentioned weather-resistant, acid and alkali-resistant fluorinated protective coating is wherein the organic solvent is a mixture of butyl acetate, methyl ethyl ketone, and S100 aromatic hydrocarbons in a mass ratio of 3:2:2.

[0018] In the above-mentioned weather-resistant, acid and alkali-resistant fluorinated protective coating, the curing agent is an aliphatic HDI trimer curing agent.

[0019] The aforementioned weather-resistant, acid and alkali-resistant fluorinated protective coating has a 38% higher crosslinking density and a multi-substrate adhesion ≥5.2MPa; after 8000 hours of accelerated artificial aging, the gloss retention rate is ≥85% and the yellowing level is 0; existing similar fluorinated coatings have a gloss retention rate of only 52% and a yellowing level of 1-2; thus completely solving the problems of outdoor chalking, cracking, and yellowing.

[0020] The application process of a weather-resistant, acid and alkali-resistant fluorinated protective coating is as follows:

[0021] Base material mixing: Place the base material in the mixing equipment and use the pre-prepared electric mixer to mix the base material thoroughly. The mixing time is recommended to be 3-5 minutes. During the mixing process, ensure that the base material is completely mixed until the color and texture of the base material are completely uniform and there are no lumps or sediments.

[0022] Adding curing agent: According to the corresponding ratio, slowly pour the curing agent into the base material that is being stirred at low speed. When pouring, pour in the direction of rotation of the stirring blades to avoid the curing agent residue on the container wall.

[0023] Mixing and stirring: After adding all the hardener to the base material, continue to stir with an electric mixer. The stirring time should be controlled between 2 and 5 minutes. During the stirring process, ensure that the stirring blades are always in the lower middle part of the coating. Stir evenly at a speed of 300-500 rpm to ensure that the base material and hardener are completely and evenly mixed. Avoid stirring too vigorously during the stirring process to prevent a large amount of air from being mixed into the coating and forming too many bubbles.

[0024] Curing and standing: After stirring evenly, let the mixed coating stand at room temperature for a period of time to allow it to undergo a preliminary chemical reaction, which takes 25 minutes; Viscosity adjustment: After curing, add an appropriate amount of special thinner (not more than 5%) as needed.

[0025] Filtration and settling: After dilution, if there are impurities or air bubbles in the paint, it should be filtered using a 200-300 mesh special filter. When filtering, the filter should be completely immersed in the paint. Gently shake the filter to allow the paint to flow out naturally to remove air bubbles or small amounts of impurities generated during stirring. The filtered paint should be left to stand for 2-3 minutes before use.

[0026] Secondly, a method for preparing a weather-resistant, acid- and alkali-resistant fluorinated protective coating, comprising the following steps:

[0027] Obtain 40%-70% of the fluoropolymer by mass percentage, add it to the organic solvent, and stir in a closed mixing tank until completely dissolved and free of particles. The stirring speed is 800-1200 r / min, and the stirring time is 20-30 min. The amount of organic solvent added is to bring the total mass to 100%.

[0028] Reduce the speed to 300-500 r / min, add 1%-16% organic-inorganic hybrid UV absorber and 5%-20% compatibilizer in batches, increase the speed to 1500-2000 r / min, and emulsify and disperse at high speed for 30-60 min, with a dispersed particle size ≤10μm.

[0029] While stirring at a low speed of 400r / min, add 0.5%-10% of functional additives, adjust the viscosity of the Forte 4 viscosity cup (25℃) to 15-60s, and filter under negative pressure through a 250-mesh filter to obtain the base material;

[0030] Mix the base material and curing agent separately at a mass ratio of 4-10:1, and store them away from light.

[0031] The technical solution provided by the present invention, which discloses a weather-resistant, acid and alkali-resistant fluorinated protective coating and its preparation method, has the following technical effects:

[0032] This product utilizes a compounding process of base components and curing agents. The base components include fluoropolymers, organic-inorganic hybrid UV absorbers, functional additives, compatibilizers, and organic solvents. This achieves high UV blocking across the entire UVA and UVB bands while ensuring near-complete penetration of visible and infrared light, balancing protection with architectural transparency and decorative properties. It extends the coating's protective lifespan, eliminates defects such as film whitening and powdering, enhances the coating's resistance to UV aging, and extends the building's protective lifespan. It resolves the technical problem of the contradiction between UV blocking and high visible and infrared transmittance in existing transparent exterior wall coatings; it addresses the issues of poor compatibility, precipitation, agglomeration, and storage sedimentation between conventional UV absorbers and fluoropolymer matrices; it addresses the weak resistance of acrylic, polyurethane, and ordinary fluoropolymer coatings to strong acids and alkalis; it addresses the problems of poor long-term outdoor weather resistance, yellowing, powdering, and delamination in existing protective coatings; and it optimizes the formula and preparation process to solve the problems of batch instability, poor substrate adhesion, and high construction difficulty in fluoropolymer coatings, while improving the finished product's storage stability and compatibility with multiple substrates. Attached Figure Description

[0033] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0034] Figure 1 This is a graph showing the results of the light transmittance test.

[0035] Figure 2 Comparison view of alkali-resistant accelerated corrosion under the same working conditions;

[0036] Figure 3 This is a schematic diagram of the microstructure under a transmission electron microscope. Detailed Implementation

[0037] In order to make the technical means, inventive features, objectives and effects of the invention easy to understand, the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are some embodiments of the present invention, but not all embodiments.

[0038] Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0039] It should be noted that the structures, proportions, sizes, etc., illustrated in the accompanying drawings of this specification are only used to complement the content disclosed in the specification for those skilled in the art to understand and read, and are not intended to limit the conditions under which the present invention can be implemented. Therefore, they have no substantial technical significance. Any modifications to the structure, changes in the proportions, or adjustments to the size, without affecting the effects and objectives that the present invention can produce, should still fall within the scope of the technical content disclosed in the present invention.

[0040] Furthermore, the terms such as "upper," "lower," "left," "right," "middle," and "one" used in this specification are merely for clarity of description and are not intended to limit the scope of the invention. Any changes or adjustments to their relative relationships, without substantially altering the technical content, should also be considered within the scope of the invention.

[0041] The "range" disclosed in this application can be defined in the form of a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints; any endpoint can be independently included or excluded, and they can be combined arbitrarily, meaning any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values ​​1 and 2 are listed, and maximum range values ​​3, 4, and 5 are also listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0" and "5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when describing a parameter as an integer ≥ 2, it is equivalent to listing integers such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, and 12 for that parameter. For instance, when describing a parameter as an integer selected from "2-10", it is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9, and 10.

[0042] In this application, the terms "multiple" or "various" are used unless otherwise specified, referring to a quantity greater than or equal to 2. For example, "one or more" means one or more types.

[0043] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0044] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments. The term "implementation" as used herein has a similar understanding.

[0045] Those skilled in the art will understand that the order in which the steps are written in the methods of various embodiments or examples does not imply a strict execution order and does not constitute any limitation on the implementation process. The detailed execution order of each step should be determined by its function and possible internal logic. Unless otherwise specified, all steps of this application may be performed sequentially or randomly, preferably sequentially. For example, if a method includes steps (a) and (b), it means that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, if a method may also include step (c), it means that step (c) can be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0046] In this application, open-ended technical features or solutions described using terms such as "containing," "including," or "comprising" do not exclude additional members beyond those listed unless otherwise specified. They can be considered as providing both closed-ended features or solutions comprised of the listed members and open-ended features or solutions that include additional members beyond the listed members. For example, if A includes a1, a2, and a3, it may also include other members or exclude additional members unless otherwise specified. This can be considered as providing both the feature or solution that "A consists of a1, a2, and a3" and the feature or solution that "A includes not only a1, a2, and a3, but also other members." In this application, unless otherwise specified, A (e.g., B) indicates that B is a non-limiting example of A, and it can be understood that A is not limited to B.

[0047] In this application, "optionally," "optionally," and "optional" mean that something is optional, that is, it means that it is selected from either "with" or "without." If there are multiple "optional" entries in a technical solution, unless otherwise specified and there are no contradictions or mutual constraints, each "optional" entry shall be independent.

[0048] One embodiment of this application provides a weather-resistant, acid and alkali-resistant fluorinated protective coating, which comprises a base component and a curing agent in a mass ratio of 4-10:1;

[0049] By mass percentage, the base material composition includes: 40%-70% fluoropolymer, 1%-16% organic-inorganic hybrid UV absorber, 0.5%-10% functional additives, 5%-20% compatibilizer, and organic solvents to make up to 100%.

[0050] The aforementioned weather-resistant and acid / alkali-resistant fluorinated protective coating comprises a fluorinated polymer composed of a fluoroolefin-vinyl ether copolymer resin, an ethylene-tetrafluoroethylene copolymer, and polyvinylidene fluoride. The fluorine content in the fluoroolefin-vinyl ether copolymer resin is ≥30%, the fluorine content in the ethylene-tetrafluoroethylene copolymer is ≥55%, and the fluorine content in the polyvinylidene fluoride is ≥50%. A ternary compound is used to improve the matrix, enhancing acid and alkali resistance and the coating's weather resistance. The fluorine-carbon bond energy is 485 kJ / mol, far exceeding the energy of ultraviolet photons and the activation energy of acid and alkali hydrolysis. Cross-linking forms a dense network structure, blocking the penetration of corrosive media. Test data shows that after immersion in 10% sulfuric acid and 10% sodium hydroxide at room temperature for 168 hours, the coating showed no blistering, peeling, or discoloration. Existing acrylic coatings blister after 72 hours, and ordinary single-component fluorinated coatings show slight whitening after 120 hours, indicating a 72% or more improvement in chemical corrosion resistance. Simultaneously, the resin itself has a light transmittance of ≥95%, preserving the appearance and texture of the base material.

[0051] The synergistic mechanism of ternary resins: FEVE contains hydroxyl groups, which can crosslink with HDI curing agent, providing the coating with crosslinking film-forming ability and substrate adhesion; ETFE improves the chemical resistance and weather resistance of the substrate; PVDF provides an extremely high CF bond ratio, strengthening the resistance to acid and alkali corrosion; after the three are compounded, they form a miscible blend system under the action of PMMA compatibilizer, taking into account crosslinking film formation, chemical corrosion resistance and transparency; after crosslinking film formation, a dense network structure is formed, blocking the penetration of acid and alkali corrosive media into the substrate; tests show that after immersion in 10% sulfuric acid and 10% sodium hydroxide at room temperature for 168 hours, the coating has no blistering, no peeling and no discoloration; compared with traditional acrylic coatings that blister and fail after 72 hours and ordinary single-component fluorine coatings that turn slightly white after 120 hours, the chemical corrosion resistance is significantly improved, while the resin matrix itself has a light transmittance of ≥95%, preserving the appearance and texture of the substrate.

[0052] The organic-inorganic hybrid UV absorber is a compound of fluorinated triazine organic UV absorber and fluorinated coupling agent modified nano-inorganic powder in a mass ratio of 1:1-4. The fluorinated coupling agent modified nano-inorganic powder is selected from one or more of 20-50nm modified rutile titanium dioxide and modified zinc oxide. The fluorinated hybrid UV absorption system is improved to balance light transmission and UV protection. The particle size is smaller than half the wavelength of visible light, effectively preventing light scattering. The coating haze is ≤1.2%. The visible light transmittance is ≥91%, and the infrared transmittance is ≥83%, which is almost complete. Inorganic reflection, organic conversion, and free radical capture result in a full-band UV blocking rate of ≥95%. Compared with existing transparent fluorine coatings, the UV blocking ability is improved by 27%, and the light transmittance is improved by 11%, completely solving the optical contradiction.

[0053] The functional additives are one or more of the following: polymeric block dispersants, polyether siloxane wetting agents, polyester leveling agents, silicone defoamers, and hindered amine light stabilizers;

[0054] The compatibilizer is polymethyl methacrylate (PMMA). PMMA acts as a compatible transition phase, reducing the interfacial tension between the FEVE-ETFE-PVDF ternary fluoropolymers and improving the interfacial bonding between the hybrid UV absorber and the fluorinated matrix. With the addition of functional additives, the coating shows no stratification or precipitation after 3 months of storage at room temperature; after 2 years of long-term outdoor use, there is no additive precipitation or surface whitening; the UV protection performance degradation rate of the coating is reduced from 41% in the existing technology to 6%, without compromising the coating's hardness or adhesion.

[0055] The functional additives and compatibilizers are combined to solve the defects of additive precipitation and agglomeration, eliminate the interfacial tension between additives and resins, and there is no stratification or precipitation after 3 months of storage; there is no surface precipitation or whitening after 2 years of outdoor use; compared with the existing ordinary UV additive system, the coating protection attenuation rate is reduced from 41% to 6%, which significantly extends the service life; at the same time, it does not negatively affect the coating hardness and adhesion.

[0056] The organic solvent is a mixture of butyl acetate, methyl ethyl ketone, and S100 aromatic hydrocarbons in a mass ratio of 3:2:2. The compound solvent has good solubility for all three fluorinated resins, ensuring that the resin is completely dissolved without any colloids, while also taking into account the evaporation rate, so that the film formed during construction is less likely to have pinholes or orange peel defects.

[0057] The curing agent is an aliphatic HDI trimer curing agent.

[0058] The aforementioned weather-resistant, acid and alkali-resistant fluorinated protective coating has a 38% higher crosslinking density and a multi-substrate adhesion ≥5.2MPa; after 8000 hours of accelerated artificial aging, the gloss retention rate is ≥85% and the yellowing level is 0; existing similar fluorinated coatings have a gloss retention rate of only 52% and a yellowing level of 1-2; thus completely solving the problems of outdoor chalking, cracking, and yellowing.

[0059] The application process of a weather-resistant, acid and alkali-resistant fluorinated protective coating is as follows:

[0060] Base material mixing: Place the base material in the mixing equipment and use the pre-prepared electric mixer to mix the base material thoroughly. The mixing time is recommended to be 3-5 minutes. During the mixing process, ensure that the base material is completely mixed until the color and texture of the base material are completely uniform and there are no lumps or sediments.

[0061] Adding curing agent: According to the corresponding ratio, slowly pour the curing agent into the base material that is being stirred at low speed. When pouring, pour in the direction of rotation of the stirring blades to avoid the curing agent residue on the container wall.

[0062] Mixing and stirring: After adding all the hardener to the base material, continue to stir with an electric mixer. The stirring time should be controlled between 2 and 5 minutes. During the stirring process, ensure that the stirring blades are always in the lower middle part of the coating. Stir evenly at a speed of 300-500 rpm to ensure that the base material and hardener are completely and evenly mixed. Avoid stirring too vigorously during the stirring process to prevent a large amount of air from being mixed into the coating and forming too many bubbles.

[0063] Curing and standing: After stirring evenly, let the mixed coating stand at room temperature for a period of time to allow it to undergo a preliminary chemical reaction, which takes 25 minutes; Viscosity adjustment: After curing, add an appropriate amount of special thinner (not more than 5%) as needed.

[0064] Filtration and settling: After dilution, if there are impurities or air bubbles in the paint, it should be filtered using a 200-300 mesh special filter. When filtering, the filter should be completely immersed in the paint. Gently shake the filter to allow the paint to flow out naturally to remove air bubbles or small amounts of impurities generated during stirring. The filtered paint should be left to stand for 2-3 minutes before use.

[0065] The transmittance of the weather-resistant, acid- and alkali-resistant fluorinated protective coating of this invention was tested against that of existing coatings. Figure 1 As shown, L1 is the coating of this solution, L2 is the existing fluorine coating, and L3 is the acrylic coating. The horizontal axis of the optical curve represents the wavelength of light (200nm-2500nm), and the vertical axis represents the light transmittance (0%-100%). Notes: In the ultraviolet band (270-400nm), the transmittance of this solution is ≤4.2%; in the visible light band (450-780nm) and near-infrared band (780-2500nm), the transmittance of this solution is ≥83%. Existing coatings suffer from severe visible light scattering and significant attenuation of short-wavelength transmission. This solution has a relative advantage in selective light transmission.

[0066] Figure 2For comparison under the same working conditions and accelerated corrosion resistance, the test medium was a 10wt% sodium hydroxide aqueous solution at room temperature, and the immersion time was 168h; 2-1 is the coating sample of this scheme, 2-2 is the ordinary PVDF fluoropolymer coating sample, and 2-3 is the acrylic coating sample; the substrate was uniformly 6063 architectural aluminum alloy sheet; the test results were as follows: the coating of sample 2-1 was smooth without blistering, discoloration, or interface peeling; the coating of sample 2-2 showed whitening at the edge of the sheet and slight interface peeling; the coating of sample 2-3 showed overall swelling, dense blistering, and local peeling; the coating of this scheme has a strong alkali resistance mechanism.

[0067] Figure 3 This is a schematic diagram of the microstructure under a transmission electron microscope, with a uniform scale bar of 50 nm; Figure 3 a represents the dispersion morphology of the fluorine-modified nano-UV absorber of the present invention, with a particle size of 25-40 nm, uniform dispersion, and no agglomeration defects; Figure 3 b represents the morphology of unmodified nano-titanium dioxide powder in the prior art, with particles agglomerated and clumped, and a particle size of 120-300nm; the additive compatibility improvement mechanism provided by this solution clarifies the microscopic principle of eliminating coating whitening and storage sedimentation, and supports the creativity of the formulation.

[0068] Another embodiment of this application provides a method for preparing a weather-resistant, acid and alkali-resistant fluorinated protective coating, comprising the following steps:

[0069] Obtain 40%-70% of the fluoropolymer by mass percentage, add it to the organic solvent, and stir in a closed mixing tank until completely dissolved and free of particles. The stirring speed is 800-1200 r / min, and the stirring time is 20-30 min. The amount of organic solvent added is to bring the total mass to 100%.

[0070] Reduce the speed to 300-500 r / min, add 1%-16% organic-inorganic hybrid UV absorber and 5%-20% compatibilizer in batches, increase the speed to 1500-2000 r / min, and emulsify and disperse at high speed for 30-60 min, with a dispersed particle size ≤10μm.

[0071] While stirring at a low speed of 400r / min, add 0.5%-10% of functional additives, adjust the viscosity of the Forte 4 viscosity cup (25℃) to 15-60s, and filter under negative pressure through a 250-mesh filter to obtain the base material;

[0072] Mix the base material and curing agent separately at a mass ratio of 4-10:1, and store them away from light.

[0073] Example 1:

[0074] 40% of the fluoropolymer was obtained by mass percentage and added to 23.5% organic solvent. The mixture was stirred in a sealed stirring tank until completely dissolved and free of particles. The stirring speed was 800 r / min and the stirring time was 20 min. The amount of organic solvent added was to bring the total mass to 100%. The fluoropolymer was composed of 20% fluoroolefin-vinyl ether copolymer resin, 10% ethylene-tetrafluoroethylene copolymer, and 10% polyvinylidene fluoride. The fluoroolefin-vinyl ether copolymer resin was LUMIFLON® LF-910LM, the ethylene-tetrafluoroethylene copolymer was Fluon® ETFEC-88AXM, and the polyvinylidene fluoride was Kynar500. The organic solvent was a mixture of butyl acetate, methyl ethyl ketone, and S100 aromatics in a mass ratio of 3:2:2.

[0075] Reduce the speed to 300 r / min, add 16% organic-inorganic hybrid UV absorber and 20% compatibilizer in batches, increase the speed to 1500 r / min, and emulsify and disperse at high speed for 30 min, with a dispersed particle size ≤10 μm; the organic-inorganic hybrid UV absorber is a compound of fluorinated triazine organic UV absorber and fluorinated coupling agent modified nano-inorganic powder in a mass ratio of 1:1, and the fluorinated coupling agent modified nano-inorganic powder is selected from one or more of 20 nm modified rutile titanium dioxide and modified zinc oxide; the compatibilizer is polymethyl methacrylate;

[0076] While stirring at a low speed of 400 r / min, add 0.5% functional additives, adjust the viscosity to 15-60 s using a Ford cup (25℃), and filter under negative pressure through a 250 mesh screen to obtain the base material; the functional additives are 0.1% polymer block dispersant, 0.1% polyether siloxane wetting agent, 0.1% polyester leveling agent, 0.1% silicone defoamer, and 0.1% hindered amine light stabilizer;

[0077] Mix the base material and curing agent separately in a 4:1 ratio and store them away from light; the curing agent is an aliphatic HDI trimer curing agent.

[0078] Example 2:

[0079] 55% of the fluoropolymer was obtained by mass percentage and added to 19% of the organic solvent. The mixture was stirred in a sealed stirring tank until completely dissolved and free of particles. The stirring speed was 1000 r / min and the stirring time was 25 min. The amount of organic solvent added was to bring the total mass to 100%. The fluoropolymer was composed of 35% fluoroolefin-vinyl ether copolymer resin, 10% ethylene-tetrafluoroethylene copolymer, and 10% polyvinylidene fluoride. The fluoroolefin-vinyl ether copolymer resin used was LUMIFLON® LF-910LM, the ethylene-tetrafluoroethylene copolymer used was Fluon® ETFEC-88AXM, and the polyvinylidene fluoride used was Kynar500. The organic solvent was a mixture of butyl acetate, methyl ethyl ketone, and S100 aromatics in a mass ratio of 3:2:2.

[0080] Reduce the speed to 400 r / min, add 8.5% organic-inorganic hybrid UV absorber and 12.5% ​​compatibilizer in batches, increase the speed to 1750 r / min, and emulsify and disperse at high speed for 45 min, with a dispersed particle size ≤10 μm; the organic-inorganic hybrid UV absorber is a compound of fluorinated triazine organic UV absorber and fluorinated coupling agent modified nano-inorganic powder in a mass ratio of 1:2, the fluorinated coupling agent modified nano-inorganic powder is selected from one or more of 20-50 nm modified rutile titanium dioxide and modified zinc oxide; the compatibilizer is polymethyl methacrylate;

[0081] While stirring at a low speed of 400 r / min, add 5% functional additives, adjust the viscosity of the Forte 4 viscosity cup (25℃) to 15-60s, filter under negative pressure through a 250 mesh filter to obtain the base material; the functional additives are 1% polymer block dispersant, 1% polyether siloxane wetting agent, 1% polyester leveling agent, 1% silicone defoamer, and 1% hindered amine light stabilizer;

[0082] Mix the base material and curing agent separately in a 7:1 ratio and store them away from light; the curing agent is an aliphatic HDI trimer curing agent.

[0083] Example 3:

[0084] 70% of the fluoropolymer was obtained by mass percentage and added to 14% organic solvent. The mixture was stirred in a sealed stirring tank until completely dissolved and free of particles. The stirring speed was 1200 r / min and the stirring time was 30 min. The amount of organic solvent added was to bring the total mass to 100%. The fluoropolymer was composed of 30% fluoroolefin-vinyl ether copolymer resin, 20% ethylene-tetrafluoroethylene copolymer, and 20% polyvinylidene fluoride. The fluoroolefin-vinyl ether copolymer resin used was LUMIFLON® LF-910LM, the ethylene-tetrafluoroethylene copolymer used was Fluon® ETFEC-88AXM, and the polyvinylidene fluoride used was Kynar500. The organic solvent was a mixture of butyl acetate, methyl ethyl ketone, and S100 aromatics in a mass ratio of 3:2:2.

[0085] Reduce the speed to 500 r / min, add 1% organic-inorganic hybrid UV absorber and 5% compatibilizer in batches, increase the speed to 2000 r / min, and emulsify and disperse at high speed for 60 min, with a dispersed particle size ≤10 μm; the organic-inorganic hybrid UV absorber is a compound of fluorinated triazine organic UV absorber and fluorinated coupling agent modified nano-inorganic powder in a mass ratio of 1:4, the fluorinated coupling agent modified nano-inorganic powder is selected from one or more of 20-50 nm modified rutile titanium dioxide and modified zinc oxide; the compatibilizer is polymethyl methacrylate;

[0086] While stirring at a low speed of 400 r / min, add 10% functional additives, adjust the viscosity to 15-60s using a Ford-4 viscosity cup (25℃), and filter under negative pressure through a 250-mesh filter to obtain the base material; the functional additives are 2% polymer block dispersant, 2% polyether siloxane wetting agent, 2% polyester leveling agent, 2% silicone defoamer, and 2% hindered amine light stabilizer;

[0087] Mix the base material and curing agent separately at a ratio of 10:1 and store them away from light; the curing agent is an aliphatic HDI trimer curing agent.

[0088] Experimental example:

[0089] 70% of the fluoropolymer was obtained by mass percentage and added to 14% organic solvent. The mixture was stirred in a closed stirring tank until completely dissolved and free of particles. The stirring speed was 1200 r / min and the stirring time was 30 min. The amount of organic solvent added was to bring the total mass to 100%. The fluoropolymer was composed of 30% fluoroolefin-vinyl ether copolymer and 40% ethylene-tetrafluoroethylene copolymer. The fluoroolefin-vinyl ether copolymer was LUMIFLON® LF-910LM and the ethylene-tetrafluoroethylene copolymer was Fluon® ETFEC-88AXM. The organic solvent was a mixture of butyl acetate, methyl ethyl ketone, and S100 aromatics in a mass ratio of 3:2:2.

[0090] Reduce the speed to 500 r / min, add 1% organic-inorganic hybrid UV absorber and 5% compatibilizer in batches, increase the speed to 2000 r / min, and emulsify and disperse at high speed for 60 min, with a dispersed particle size ≤10 μm; the organic-inorganic hybrid UV absorber is a compound of fluorinated triazine organic UV absorber and fluorinated coupling agent modified nano-inorganic powder in a mass ratio of 1:4, the fluorinated coupling agent modified nano-inorganic powder is selected from one or more of 20-50 nm modified rutile titanium dioxide and modified zinc oxide; the compatibilizer is polymethyl methacrylate;

[0091] While stirring at a low speed of 400 r / min, add 10% functional additives, adjust the viscosity to 15-60s using a Ford-4 viscosity cup (25℃), and filter under negative pressure through a 250-mesh filter to obtain the base material; the functional additives are 2% polymer block dispersant, 2% polyether siloxane wetting agent, 2% polyester leveling agent, 2% silicone defoamer, and 2% hindered amine light stabilizer;

[0092] Mix the base material and curing agent separately at a ratio of 10:1 and store them away from light; the curing agent is an aliphatic HDI trimer curing agent.

[0093] Comparative Example 1:

[0094] By weight percentage: 40% fluoropolymer (20% LUMIFLON® LF-910LM, 10% Fluon® ETFEC-88AXM, 10% Kynar500), 23.5% organic solvent (butyl acetate: methyl ethyl ketone: S100 = 3:2:2), 20% compatibilizer PMMA, 16% common benzotriazole UV absorber (Tinuvin 327), and 0.5% functional additives; the functional additives are 0.1% polymeric block dispersant, 0.1% polyether siloxane wetting agent, 0.1% polyester leveling agent, 0.1% silicone defoamer, and 0.1% hindered amine light stabilizer.

[0095] Variable description: "Fluorotriazine organic UV absorber modified with fluorine coupling agent nano-TiO2 / ZnO" is replaced with an equal amount of ordinary organic UV absorber, and no nano-inorganic powder is introduced, in order to verify the effect of organic-inorganic hybrid UV absorber on weather resistance.

[0096] Comparative Example 2:

[0097] By weight percentage: 40% fluoropolymer (20% LUMIFLON® LF-910LM, 10% Fluon® ETFEC-88AXM, 10% Kynar500), 43.5% organic solvent (to make up), 16% organic-inorganic hybrid UV absorber, 0.5% functional additives, no PMMA added; the functional additives are 0.1% polymer block dispersant, 0.1% polyether siloxane wetting agent, 0.1% polyester leveling agent, 0.1% silicone defoamer, and 0.1% hindered amine light stabilizer.

[0098] Variable description: The compatibilizer is removed and the organic solvent is replenished accordingly. This is used to verify the effect of PMMA compatibilizer on the compatibility of multiphase fluorinated resin and the overall performance of the coating film.

[0099] The coatings obtained by using the base material and curing agent obtained in Examples 1-3 were tested together with the coatings of Experimental Examples and Comparative Examples 1-2 under the following board preparation and testing conditions. The test contents and testing methods are shown in Table 1.

[0100] Panel preparation conditions: tinplate (120mm×50mm×0.3mm) and sandblasted steel plate (150mm×70mm×1mm), air spraying, dry film thickness (35±5)μm, tested after curing at 25℃ / 50%RH for 7 days.

[0101] The experimental data results are as follows: basic physical and mechanical properties are shown in Table 2; resistance to media is shown in Table 3; weathering and aging performance, xenon lamp aging for 2000h is shown in Table 4, QUV (UVB-313) aging for 1500h is shown in Table 5; and pollution resistance performance is shown in Table 6.

[0102] Serial Number Testing items Test methods / standards Key Indicators 1 Paint film appearance GB / T 1729 Smooth, free of pinholes and shrinkage cavities 2 Adhesion GB / T 9286 Cross-cut test (1 mm) Levels 0-5 3 Pencil hardness GB / T 6739 H~3H 4 Impact resistance GB / T 1732 (50 cm·kg) No cracks, no peeling 5 flexibility GB / T 1731 (shaft diameter 1 mm) No cracks 6 Water resistance GB / T 1733 (40℃ deionized water, 500 h) No bubbling, no rust, adhesion ≤ Grade 1 7 Acid resistance <![CDATA[GB / T 9274(5% H2SO4,25℃,500 h)]]> No bubbling, no discoloration, no peeling 8 Alkali resistance GB / T 9274 (5% NaOH, 25℃, 500 h) No bubbling, no discoloration, no peeling 9 Salt spray resistance GB / T 1771 (Neutral Salt Spray, 1000 h) Erosion at the scribed area ≤2 mm, no blistering 10 Resistant to artificial climate aging GB / T 1865 (Xenon lamp, 2000 h) Gloss retention, color change ΔE, chalking grade 11 QUV accelerated aging resistance GB / T 14522 (UVB-313, 1500 h) Gloss retention rate, chalking grade 12 Stain resistance GB / T 9780 (Fly ash / graphite method, 5 cycles) The rate of decrease in reflectance is ≤15%. 13 Contact angle Seat drop method (water / hexadecane) Water contact angle ≥105° 14 60° gloss GB / T 9754 initial luster

[0103] Table 1

[0104] Testing items Example 1 Example 2 3rd Embodiment Experimental Example Comparative Example 1 Comparative Example 2 Paint film appearance Smooth Smooth Smooth Smooth Smooth There are shrinkage cavities Adhesion (Grade) 0 0 0 0 1 2 Pencil hardness H 2H 2H 2H H HB Impact resistance (cm·kg) 50 passed 50 passed 50 passed 50 passed 50 passed 30 passed Flexibility (mm) 1 1 1 1 1 3 60° initial gloss 82 85 88 86 80 72 Water contact angle (°) 112 115 118 116 104 98

[0105] Table 2

[0106] Testing items Example 1 Example 2 3rd Embodiment Experimental Example Comparative Example 1 Comparative Example 2 Water resistance (500 h) No abnormalities No abnormalities No abnormalities No abnormalities Slight bubbling Bubbling and peeling <![CDATA[Resistant to 5% H2SO4 (500 h)]]> No abnormalities No abnormalities No abnormalities No abnormalities Slight discoloration foaming Resistant to 5% NaOH (500 h) No abnormalities No abnormalities No abnormalities No abnormalities Slight loss of light Bubbling and peeling Resistance to neutral salt spray (1000 h) Erosion depth 0.8 mm Erosion depth 0.5 mm Erosion depth 0.3 mm Erosion depth 0.4 mm Erosion depth 2.5 mm Erosion 5 mm, blistering

[0107] Table 3

[0108] Testing items Example 1 Example 2 3rd Embodiment Experimental Example Comparative Example 1 Comparative Example 2 Gloss retention rate (%) 92 95 96 95 68 45 Color change ΔE 1.2 0.8 0.6 0.7 3.8 6.2 Powdering grade 0 0 0 0 1 2 Adhesion after aging (grade) 0 0 0 0 1 3

[0109] Table 4

[0110] Testing items Example 1 Example 2 3rd Embodiment Experimental Example Comparative Example 1 Comparative Example 2 Gloss retention rate (%) 88 91 93 92 55 30 Powdering grade 0 0 0 0 1 3 Cracking none none none none none Obvious cracks

[0111] Table 5

[0112] Testing items Example 1 Example 2 3rd Embodiment Experimental Example Comparative Example 1 Comparative Example 2 Reflectance coefficient reduction rate (%) 8.5 7.2 6.0 6.5 16.8 22.5

[0113] Table 6

[0114] Based on the above experimental data, the following conclusions can be drawn:

[0115] The weather-resistant and acid-alkali-resistant fluorinated protective coatings prepared in Examples 1-3 exhibited a gloss retention rate ≥92%, discoloration ΔE ≤1.2, and chalking grade 0 after 2000 hours of xenon lamp aging; a gloss retention rate ≥88% after 1500 hours of QUV aging; no abnormalities after 500 hours of 5% H2SO4 / 5% NaOH aging; ≤0.8mm of scratch penetration after 1000 hours of neutral salt spray aging; and a pollution resistance reflection coefficient reduction rate ≤8.5%. All indicators were significantly better than the two comparative examples, achieving a synergistic improvement in ultra-weather resistance, acid and alkali resistance, and pollution resistance.

[0116] Compared with Example 1, when the organic-inorganic hybrid UV absorber was replaced with an equal amount of ordinary benzotriazole organic UV absorber, the gloss retention rate after 2000 hours under a xenon lamp was only 68%, a decrease of 24 percentage points compared with Example 1. The discoloration ΔE increased to 3.8, and the chalking reached level 1. The gloss retention rate after 1500 hours under QUV was only 55%. This shows that ordinary organic UV absorbers are prone to migration and photodegradation, and have insufficient long-term weather resistance. The organic-inorganic hybrid system of the fluorinated triazine organic absorber (absorption conversion) and the fluorinated coupling agent modified nano-TiO2 / ZnO (scattering shielding) in this scheme achieves full-band protection against 280-400nm UV light through the synergistic effect of the two. The surface modification of the fluorinated coupling agent makes the nanoparticles uniformly dispersed in the fluorinated matrix, which is the fundamental reason for the leap in weather resistance.

[0117] Compared to Example 2, after removing the PMMA compatibilizer, the following issues were observed: film pinholes, adhesion reduced to grade 2, impact resistance only 30cm, and flexibility reduced to 3mm; gloss retention after 2000h xenon lamp exposure was only 45%, chalking grade 2, and adhesion reduced to grade 3 after aging; significant cracks appeared after 1500h QUV testing; and acid, alkali, and salt spray resistance deteriorated severely. This demonstrates that there is thermodynamic incompatibility between ETFE / PVDF and FEVE resin. PMMA, as a compatibilizer, effectively reduces interfacial tension, enabling the multiphase fluorinated resin to form a uniform and stable coating film, and is a necessary component to ensure mechanical properties, media resistance, and weather resistance.

[0118] The total amount of fluoropolymer increased from 40% to 70% (Examples 1 to 3), the water contact angle increased from 112° to 118°, the salt spray corrosion resistance decreased from 0.8 mm to 0.3 mm, the pollution resistance decrease rate decreased from 8.5% to 6.0%, and the xenon lamp gloss retention rate increased from 92% to 96%, showing a positive correlation trend. The experimental example (a binary compound of FEVE and ETFE, without PVDF) had performance close to that of a ternary compound, indicating that ETFE is the main source of contribution to acid and alkali resistance, and PVDF further enhances weather resistance and hydrophobicity.

[0119] Considering both performance and cost, the second embodiment (containing 55% fluoropolymer, including 35% FEVE, 10% ETFE, and 10% PVDF; 8.5% hybrid UV absorber, organic:inorganic = 1:2; 12.5% ​​PMMA; 5% additives; base material:curing agent = 7:1) is the optimal implementation method: gloss retention rate of 95% after 2000 hours under xenon lamp, ΔE = 0.8, salt spray corrosion diffusion of 0.5mm, and pollution resistance reduction rate of 7.2%. It achieves the best balance between high weather resistance and acid and alkali resistance and raw material cost, and is recommended as the preferred formulation for industrialization.

[0120] According to the present invention, a weather-resistant and acid-alkali-resistant fluorinated protective coating and its preparation method are provided. The coating is prepared by using a fluorinated olefin-vinyl ether copolymer resin, ethylene-tetrafluoroethylene copolymer, and polyvinylidene fluoride compounded with a fluorinated polymer matrix, and adding fluorinated organic-inorganic hybrid ultraviolet absorbers, compatibilizers, and functional additives. The coating achieves a comprehensive effect of high transparency, full-band ultraviolet blocking, acid and alkali corrosion resistance, ultra-long weather resistance, and stable storage without precipitation, thereby solving the defects caused by the prior art.

[0121] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.

Claims

1. A weather-resistant, acid and alkali-resistant fluorinated protective coating, characterized in that, It contains a base material component and a curing agent in a mass ratio of 4-10:1; By mass percentage, the base material composition comprises: 40%-70% fluoropolymer, 1%-16% organic-inorganic hybrid UV absorber, 0.5%-10% functional additives, 5%-20% compatibilizer, and organic solvents to bring the total to 100%.

2. The weather-resistant, acid and alkali-resistant fluorinated protective coating according to claim 1, characterized in that, The fluoropolymer is a compound of fluoroolefin-vinyl ether copolymer resin, ethylene-tetrafluoroethylene copolymer, and polyvinylidene fluoride.

3. The weather-resistant, acid and alkali-resistant fluorinated protective coating according to claim 2, characterized in that, The fluorine content in the fluoroolefin-vinyl ether copolymer resin is ≥30%, the fluorine content in the ethylene-tetrafluoroethylene copolymer is ≥55%, and the fluorine content in the polyvinylidene fluoride is ≥50%.

4. The weather-resistant, acid and alkali-resistant fluorinated protective coating according to claim 1, characterized in that, The organic-inorganic hybrid ultraviolet absorber is a mixture of fluorinated triazine organic ultraviolet absorber and fluorinated coupling agent modified nano-inorganic powder in a mass ratio of 1:1-4.

5. The weather-resistant, acid and alkali-resistant fluorinated protective coating according to claim 4, characterized in that, The fluorine coupling agent modified nano-inorganic powder is selected from one or more of the following: modified rutile titanium dioxide and modified zinc oxide with a wavelength of 20-50 nm.

6. The weather-resistant, acid and alkali-resistant fluorinated protective coating according to claim 1, characterized in that, The functional additives are one or more of the following: polymeric block dispersants, polyether siloxane wetting agents, polyester leveling agents, organosilicon defoamers, and hindered amine light stabilizers.

7. The weather-resistant, acid and alkali-resistant fluorinated protective coating according to claim 1, characterized in that, The compatibilizer is polymethyl methacrylate.

8. The weather-resistant, acid and alkali-resistant fluorinated protective coating according to claim 1, characterized in that, The organic solvent is a mixture of butyl acetate, methyl ethyl ketone, and S100 aromatic hydrocarbons in a mass ratio of 3:2:

2.

9. The weather-resistant, acid and alkali-resistant fluorinated protective coating according to claim 1, characterized in that, The curing agent is an aliphatic HDI trimer curing agent.

10. A method for preparing a weather-resistant, acid and alkali-resistant fluorinated protective coating, characterized in that, Includes the following steps: Obtain 40%-70% of the fluoropolymer by mass percentage, add it to an organic solvent, and stir until completely dissolved without any granules. Add 1%-16% of organic-inorganic hybrid UV absorber and 5%-20% of compatibilizer in batches, and emulsify and disperse by high-speed stirring, with a particle size ≤10μm. While stirring at low speed, add 0.5%-10% of functional additives, adjust the viscosity of the Forte 4 viscosity cup (25℃) to 15-60s, filter under negative pressure through a 250-mesh filter to obtain the base material; The base material and curing agent are packaged separately according to a mass ratio of 4-10:1.