A method for co-processing nickel slag and steel slag to recover valuable metals
By co-processing nickel slag and steel slag, and employing high-temperature reduction and water quenching technologies, the problems of low recovery rate and high energy consumption when nickel slag is processed alone have been solved. This has enabled the efficient recovery of valuable metals and the resource utilization of solid waste, thus constructing a green circular industrial chain.
Patent Information
- Application Number
- CN202611494082.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-23
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies suffer from low recovery rates, high energy consumption, and difficulty in resource utilization of solid waste when nickel slag and steel slag are treated separately.
Nickel slag and steel slag are mixed in a certain proportion, and a reducing agent is added at high temperature for melting and reduction. Protective gas is blown in, followed by water quenching to form nickel-containing molten iron and reducing slag.
The comprehensive recovery rate of nickel, cobalt, and copper reached over 93%, and the iron recovery rate reached over 94%. The reduction slag was in a completely glassy state, realizing the full-component resource utilization of metallurgical solid waste and building a green circular industrial chain.
Smart Images

Figure CN123063602A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of non-ferrous metal metallurgy technology, and in particular to a method for the co-processing and recovery of valuable metals from nickel slag and steel slag. Background Technology
[0002] Nickel slag, produced during the smelting of nickel sulfide ore in flash furnaces or oxygen-enriched top-blown smelting systems, consists of black granules formed from high-temperature molten slag after water quenching. These granules are typically long strips or spheres and are hard in texture. Their main chemical components are FeO, SiO2, and MgO, and they are also rich in valuable metals with significant recycling value, such as iron (Fe), nickel (Ni), cobalt (Co), copper (Cu), platinum (Pt), and gold (Au). In my country, nickel slag is typically disposed of through stockpiling and left idle. Due to the long-term lack of proper utilization, the national stockpile exceeds 40 million tons. Data shows that Gansu Jinchuan Group alone discharges over 1 million tons of nickel slag annually, and the valuable metals in the slag are not recycled. Therefore, if nickel slag can be rationally utilized to maximize benefits, it will not only avoid resource waste but also protect the environment and contribute to long-term economic development.
[0003] Currently, the main domestic and international processes for recovering valuable metals from nickel slag include hydrometallurgy and pyrometallurgy. Hydrometallurgy, as the mainstream approach for recovering valuable metals from nickel slag, uses acid leaching to treat the slag. This process, involving adjusting acid concentration, steam heating, filtration, and crystallization, yields a mixture of salts such as nickel sulfate, cobalt sulfate, and copper sulfate. Then, in a reaction vessel, water is added, stirring, steam heating, and sodium carbonate is used to adjust the pH to obtain crude nickel sulfate, cobalt sulfate, and copper sulfate. Finally, after multiple purification and separation processes, the finished products of nickel sulfate, copper sulfate, and cobalt sulfate are obtained. This process achieves efficient recovery and resource utilization of valuable metals from nickel slag, with high recovery rates and wide applicability. However, it suffers from drawbacks such as a lengthy process flow, high acid consumption, high waste acid production, severe equipment corrosion, and high experimental operating costs. Pyrometallurgy remains the primary method for recovering Fe from nickel slag. The total iron content in nickel slag is typically around 40%, making it a highly valuable secondary resource. Since Fe in nickel slag usually exists in the form of ferrosilicon, traditional magnetic separation processes cannot effectively separate iron oxides. Currently, the extraction of Fe from nickel slag mainly relies on oxidation or reduction methods to dissociate the fir olivine in the slag or replace iron oxide with free oxides to meet the requirements of subsequent processes. The oxidation method involves adding modifiers such as CaO to the nickel slag, then oxidizing the iron element in the slag into magnetite phase, which precipitates out. Magnetic separation is then used to separate the magnetite from non-magnetic substances, achieving comprehensive utilization of the magnetite. However, the high smelting temperature and high proportion of CaO required for oxidation iron extraction result in high costs, making industrial application difficult. The molten reduction method treats nickel slag by adding coke or graphite powder to reduce ferrous silicate to metallic iron in a completely molten state, achieving a Fe recovery rate of over 95%. However, this method has disadvantages such as high reduction temperature, long reduction time, and large amounts of additives required. Summary of the Invention
[0004] To address the aforementioned technical problems, this invention provides a method for the co-processing and recovery of valuable metals from nickel slag and steel slag, which solves the technical problems of low recovery rate, high energy consumption, and difficulty in resource utilization of solid waste when nickel slag and steel slag are processed separately in the prior art.
[0005] To achieve the above objectives, the technical solution of the present invention is as follows: A method for co-processing nickel slag and steel slag to recover valuable metals includes the following steps: Step 1: Grind the nickel slag into powder and mix it with steel slag in a ratio of 1-2:1 to obtain a mixture. Step 2: Add a reducing agent to the mixture and melt and reduce it at a temperature of 1200-1500℃ for 1-4 hours. During the melting and reduction process, a protective gas is blown in. The protective gas is preheated high-purity Ar gas. Step 3: Water quench the molten and reduced material, including nickel-iron molten metal, reducing slag, and flue gas.
[0006] Further, the nickel slag described in step 1 comprises the following components by mass percentage: Fe: 30%-40%, O: 35%-40%, Si: 15-20%, Mg: 5%-10%, Ca: 1%-5%, Ni < 1%, Al < 1%, Cu < 1%, and the remainder being impurity elements.
[0007] Furthermore, the steel slag includes one or more of converter steel slag, electric furnace slag, and refining slag.
[0008] Furthermore, the Al2O3 content in the reducing slag accounts for 1-5% of the total mass of CaO, MgO, Al2O3, and SiO2 in the steel slag; the mass ratio of MgO / Al2O3 in the reducing slag is 0.4-0.6; and the binary basicity R in the reducing slag is... 2 =CaO / SiO2 ratio is 1 to 2.0.
[0009] Furthermore, the Ar gas in step 2 is introduced in a dispersed blowing manner at a flow rate of 300-400 ml / min.
[0010] Furthermore, the reducing agent mentioned in step 2 is one or more of carbon powder and coke powder.
[0011] Furthermore, the carbon-oxygen ratio of the reducing agent mentioned in step 2 refers to the ratio of the mass of carbon added to the reducing agent to the mass of carbon required for the metal oxide in the theoretical reduction mixture, and its value is 1.0-1.5.
[0012] Furthermore, the preheating temperature of the Ar gas is 150°C.
[0013] Compared with existing technologies, the beneficial effects of this invention are as follows: This invention breaks through the technical limitations of traditional single slag treatment and innovatively constructs a nickel slag-steel slag co-processing system: nickel slag provides abundant valuable metal elements (Fe, Ni, Co, Cu), while steel slag contributes sufficient FeO and CaO components, forming a thermodynamic complementary mechanism during the smelting process. The comprehensive recovery rate of nickel, cobalt, and copper in the obtained nickel-containing molten iron can reach over 93% (with nickel recovery reaching over 99%), and the iron recovery rate reaches over 94%. The reducing slag is in a completely glassy state (amorphous phase content >95%), achieving continuity in the preparation process. The nickel-containing molten iron can be used as molten iron for steelmaking, and the reducing slag can be used to develop and produce products such as slag powder, foam ceramics, and aerated concrete blocks. This technology realizes the resource utilization of all components of metallurgical solid waste, constructing a green circular industrial chain of "treating waste with waste and turning waste into treasure," which has significant economic benefits and environmental value. Attached Figure Description
[0014] Figure 1 This is a process flow diagram of the present invention; Detailed Implementation
[0015] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments. It should be understood that these descriptions are merely exemplary and not intended to limit the scope of the invention. Furthermore, descriptions of well-known structures and technologies are omitted in the following description to avoid unnecessarily obscuring the concepts of the invention.
[0016] The nickel slag comprises the following components by mass percentage: Fe: 36.57%, O: 35.32%, Si: 15.25%, Mg: 7.61%, Ca: 3.04%, Ni: 0.391%, Al: 0.911%, Cu: 0.16%, with the remainder being impurity elements.
[0017] A method for co-processing nickel slag and steel slag to recover valuable metals includes the following steps: Step 1: Grind 100g of nickel slag into powder and mix it with 50g of converter steel slag to obtain a mixture; the Al2O3 content in the steel slag accounts for 2.5% of the total mass of CaO, MgO, Al2O3, and SiO2 in the steel slag; the MgO / Al2O3 mass ratio in the steel slag is 0.45; the binary basicity R2 = CaO / SiO2 in the steel slag is 1.8; Step 2: Add 12g of carbon powder (reducing agent) to the mixture and melt and reduce it at 1300℃ for 1 hour. During the melting and reduction process, the protective gas is blown in by a dispersed blowing method. The protective gas is preheated high-purity Ar gas with a preheating temperature of 150℃ and a blowing flow rate of 300ml / min. Step 3: Water quench the molten and reduced material, including nickel-iron molten metal, reducing slag, and flue gas.
[0018] The recycled materials include reduction slag, nickel-containing molten iron, and flue gas. The main components of the nickel-containing molten iron are shown in Table 3, and the main components of the reduction slag are shown in Table 4. The nickel-containing molten iron can be used to prepare stainless steel and corrosion-resistant steel. The reduction slag can be used directly in building materials, as well as in the production of microcrystalline glass or foam ceramics.
[0019] In the entire process of Example 1, the yields of nickel, cobalt, copper, and iron in the nickel slag were 99.4%, 95.6%, 97.3%, and 96.2%, respectively.
[0020] Example 2 Step 1: Grind 100g of nickel slag into powder and mix it with 60g of converter steel slag to obtain a mixture; the Al2O3 content in the steel slag accounts for 2.8% of the total mass of CaO, MgO, Al2O3, and SiO2 in the steel slag; the MgO / Al2O3 mass ratio in the steel slag is 0.5; the binary basicity R in the steel slag is... 2 =CaO / SiO2 is 1.7; Step 2: Add 14g of carbon powder to the mixture and melt and reduce it at 1350℃ for 1.5h. During the melting and reduction process, the protective gas is blown in by a dispersion blowing method. The protective gas is preheated high-purity Ar gas with a preheating temperature of 150℃ and a blowing flow rate of 350ml / min. Step 3: Water quench the molten and reduced material, including nickel-iron molten metal, reducing slag, and flue gas.
[0021] The recycled materials include reduction slag, nickel-containing molten iron, and flue gas. The main components of the nickel-containing molten iron are shown in Table 3, and the main components of the reduction slag are shown in Table 4. The nickel-containing molten iron can be used to prepare stainless steel and corrosion-resistant steel. The reduction slag can be used directly in building materials, as well as in the production of microcrystalline glass or foam ceramics.
[0022] In the entire process of Example 2, the yields of nickel, cobalt, copper, and iron in the nickel slag were 98.1%, 94.5%, 95.7%, and 95.2%, respectively.
[0023] Example 3 Step 1: Grind 100g of nickel slag into powder and mix it with 70g of converter steel slag to obtain a mixture; the Al2O3 content in the steel slag accounts for 3.0% of the total mass of CaO, MgO, Al2O3, and SiO2 in the steel slag; the MgO / Al2O3 mass ratio in the steel slag is 0.55; the binary basicity R in the steel slag is... 2 =CaO / SiO2 = 1.6; Step 2: Add 15g of carbon powder to the mixture and melt and reduce it at 1400℃ for 2 hours. During the melting and reduction process, the protective gas is blown in by a dispersion blowing method. The protective gas is preheated high-purity Ar gas with a preheating temperature of 150℃ and a blowing flow rate of 400ml / min. Step 3: Water quench the molten and reduced material, including nickel-iron molten metal, reducing slag, and flue gas.
[0024] The recycled materials include reduction slag, nickel-containing molten iron, and flue gas. The main components of the nickel-containing molten iron are shown in Table 3, and the main components of the reduction slag are shown in Table 4. The nickel-containing molten iron can be used to prepare stainless steel and corrosion-resistant steel. The reduction slag can be used directly in building materials, as well as in the production of microcrystalline glass or foam ceramics.
[0025] In the entire process of Example 3, the yields of nickel, cobalt, copper, and iron in the nickel slag were 97.5%, 93.0%, 94.5%, and 94.8%, respectively.
[0026] Taking toner as a reducing agent as an example, the chemical reaction equations involved in the process of this invention include: (1) C(s)+FeO(l)=Fe(l)+CO(g); (2) C(s)+Cu2O(l)=2Cu(l)+CO(g); (3) C(s)+NiO(l)=Ni(l)+CO(g); (4) C(s)+CoO(l)=Co(l)+CO(g); (5) 2FeO·SiO2(l)+CaO(s)=2CaO·SiO2(l)+FeO(l); In the process of co-reduction smelting of nickel slag and steel slag, nickel cobalt oxides in nickel slag will be partially reduced to nickel cobalt elements by the reducing agent, i.e., reactions (2), (3), and (4); iron oxides will be reduced to low-valence iron oxides or iron elements by the reducing agent, i.e., reaction (1); while ferrous oxide in the ferroolitic phase of nickel slag reacts with calcium oxide in steel slag to form slag (5) to generate Ca2SiO4, and the generated ferrous oxide participates in reaction (1) to achieve iron enrichment.
[0027] The main chemical compositions of the raw materials used in the experiment, the nickel-containing molten iron produced, and the reducing slag are shown in the table below: As can be seen from Table 3, the obtained reduced molten iron is based on iron and is enriched with nickel and a small amount of cobalt and copper. It can be used as a mother liquor for nickel-based alloy preparation and realize the recovery of valuable metals. Table 4 shows the composition analysis of the reduction slag. The smelting reduction slag in this study is a calcium magnesium silicate slag system with low content of residual iron, sulfur, phosphorus and alkali metals. It is stable in phase and can be directly used as cement admixture or roadbed filler to realize the resource utilization of all components of solid waste.
[0028] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for co-processing nickel slag and steel slag to recover valuable metals, characterized in that... Includes the following steps: Step 1: Grind the nickel slag into powder and mix it with steel slag in a ratio of 1-2:1 to obtain a mixture. Step 2: Add a reducing agent to the mixture and melt and reduce it at a temperature of 1200-1500℃ for 1-4 hours. During the melting and reduction process, a protective gas is blown in. The protective gas is preheated high-purity Ar gas. Step 3: Water quench the molten and reduced material, including nickel-iron molten metal, reducing slag, and flue gas.
2. The method for co-processing and recovering valuable metals from nickel slag and steel slag according to claim 1, characterized in that, The nickel slag described in step 1 comprises the following components by mass percentage: Fe: 30%-40%, O: 35%-40%, Si: 15-20%, Mg: 5%-10%, Ca: 1%-5%, Ni < 1%, Al < 1%, Cu < 1%, and the remainder being impurity elements.
3. The method for co-processing and recovering valuable metals from nickel slag and steel slag according to claim 1, characterized in that, The steel slag includes one or more of converter steel slag, electric furnace slag, and refining slag.
4. The method for co-processing and recovering valuable metals from nickel slag and steel slag according to claim 1, characterized in that, The Al2O3 content in the reducing slag accounts for 1-5% of the total mass of CaO, MgO, Al2O3, and SiO2 in the steel slag; the mass ratio of MgO / Al2O3 in the reducing slag is 0.4-0.6; the binary basicity R in the reducing slag... 2 =CaO / SiO2 is 1 to 2.
0.
5. The method for co-processing and recovering valuable metals from nickel slag and steel slag according to claim 1, characterized in that, The Ar gas in step 2 is introduced by a dispersed blowing method, with a flow rate of 300-400 ml / min.
6. The method for co-processing and recovering valuable metals from nickel slag and steel slag according to claim 1, characterized in that: The reducing agent mentioned in step 2 is one or more of carbon powder and coke powder.
7. The method for co-processing and recovering valuable metals from nickel slag and steel slag according to claim 1, characterized in that: The carbon-to-oxygen ratio of the reducing agent in step 2 is 1.0-1.
5.
8. The method for co-processing and recovering valuable metals from nickel slag and steel slag according to claim 5, characterized in that: The preheating temperature of the Ar gas is 150°C.