A steelmaking and continuous casting production process of 460mm section super-thick slab 9Ni steel
Through specific chemical composition design and refined process control throughout the entire process, the problems of low purity, severe central segregation, and easy surface cracking of 460mm thick 9Ni steel billets have been solved, achieving the production of high-purity, low-segregation, and surface crack-free high-quality billets, meeting the requirements for steel used in high-end LNG storage tanks.
Patent Information
- Application Number
- CN202611269251.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-20
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies make it difficult to produce 460mm thick 9Ni steel billets with high purity, low segregation, and no surface cracks, mainly due to long solidification time, easy aggregation of non-metallic inclusions, severe central segregation, and easy surface cracking.
By employing specific chemical composition design and refined process control throughout the entire process, including low impurity composition design, LF high-alkalinity high-alumina slag system to enhance inclusion adsorption, RH long-term vacuum degassing and soft blowing argon treatment, low-speed continuous casting and large reduction volume light reduction technology, combined with magnesium modification treatment and special water-cooled model, the purity of molten steel and the quality of billet are ensured.
It has achieved the production of high-purity, low-segregation and surface-crack-free high-quality cast billets, meeting the requirements for high-end LNG storage tank steel. The number of inclusions is small, and the low-magnification segregation rating is stably controlled within C1.0 grade, ensuring the toughness of the steel at ultra-low temperatures.
Smart Images

Figure CN123063671A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of iron and steel metallurgy technology, specifically to a steelmaking and continuous casting process for 460mm cross-section extra-thick slab 9Ni steel. Background Technology
[0002] 9Ni steel, as a key structural material for liquefied natural gas (LNG) storage tanks, needs to maintain excellent impact toughness in ultra-low temperature environments. With the trend towards larger equipment manufacturing, the market demand for extra-thick 9Ni steel plates is increasing. When producing thick plates using continuously cast billets, the greater the billet thickness and the higher the rolling compression ratio, the finer the grains and the better the mechanical properties of the finished steel plate. However, when the thickness of the continuously cast billet reaches the 460mm level, due to the significantly prolonged solidification time, non-metallic inclusions in the molten steel are prone to collision and aggregation during the floating process, forming large clusters. Furthermore, the central region suffers from severe central segregation and porosity defects due to large volume shrinkage. Simultaneously, the thermal stress distribution during the cooling process of extra-thick billets is complex, resulting in high sensitivity to surface and corner cracks. In existing technologies, conventional refining and continuous casting process parameters are difficult to adapt to the heat transfer and flow characteristics of a 460mm extra-thick section, leading to insufficient purity, severe internal segregation, or substandard surface quality in the produced 9Ni steel billets, thus hindering the stable manufacturing of high-quality extra-thick 9Ni steel. Summary of the Invention
[0003] To address the problems of low purity, severe central segregation, and easy surface cracking in 460mm ultra-thick 9Ni steel slabs in existing technologies, this application proposes a steelmaking and continuous casting process for 460mm ultra-thick 9Ni steel slabs, achieving synergistic improvement in high purity control of molten steel and internal and surface quality of the slab.
[0004] To achieve the above objectives, this application adopts the following technical solution: A steelmaking and continuous casting process for 460mm cross-section extra-thick 9Ni steel slabs, wherein the chemical composition of the 9Ni steel, by mass percentage, includes: C≤0.08%, Si:0.15-0.30%, Mn:0.50-0.80%, P≤0.003%, S≤0.001%, Ni:8.50-9.50%, Cr≤0.10%, Mo≤0.05%, Nb≤0.01%, V≤0.01%, Al:0.020-0.050%, with the balance being Fe; the steelmaking and continuous casting process includes: pretreatment of molten iron; converter blowing of the pretreated molten iron; and LF refining of the molten steel after converter tapping, wherein the LF refining adopts... The diffusion deoxidation process results in a final slag content of 10-18 kg / ton of steel at the end of LF refining, a binary basicity ≥6, and an Al2O3 content ≥24%. The LF-refined steel undergoes RH refining, which includes high-vacuum treatment and soft argon blowing. The high-vacuum treatment lasts ≥25 min, and after vacuum breaking, the H content in the molten steel is ≤1 ppm. The soft argon blowing treatment lasts ≥30 min. The RH-refined steel is then continuously cast at a casting speed of 0.40-0.60 m / min, with slab cross-sectional dimensions of 460 mm thickness and 1800-2270 mm width. The continuous casting includes dynamic light reduction treatment, with a reduction of ≥15 mm.
[0005] The above scheme combines a specific low-impurity composition design with refined process control throughout the entire process. It utilizes a high-alkalinity, high-alumina slag system to enhance inclusion adsorption, and combines long-term vacuum degassing and soft blowing to promote the flotation and removal of inclusions. Furthermore, it matches low-speed continuous casting and large-reduction light-reduction technology for the 460mm extra-thick cross section to effectively compensate for solidification shrinkage, thereby obtaining a high-purity, low-segregation, and surface-crack-free high-quality billet.
[0006] As an alternative implementation, only aluminum wire is added for deoxidation during the LF refining process, and a lightweight insulating material is used to cover the surface of the steel slag after the LF refining is completed.
[0007] This alternative implementation avoids the risk of severe turbulence and secondary oxidation of the molten steel during the wire feeding process by limiting the addition of the deoxidizer to aluminum wire rather than aluminum wire. At the same time, after refining, covering with lightweight insulation material isolates the air from contact with the steel slag, preventing nitrogen absorption and secondary oxidation caused by the exposure of the molten steel, and further ensuring the purity of the molten steel.
[0008] As an optional implementation, the RH refining process also includes a magnesium modification treatment, which modifies the Al2O3 inclusions in the molten steel into magnesium aluminum spinel inclusions, and controls the Ca content in the molten steel to prevent the precipitation of CaS inclusions during the solidification process.
[0009] This alternative implementation utilizes magnesium to modify high-melting-point, easily agglomerated Al2O3 inclusions into fine, dispersed magnesium-aluminum spinel inclusions, reducing their tendency to collide and aggregate in molten steel; at the same time, it strictly controls the calcium content to avoid the precipitation of harmful CaS-type inclusions due to solute enrichment at the end of solidification, thereby improving the internal cleanliness of the billet from the source.
[0010] As an optional implementation, the secondary cooling zone of the continuous casting is cooled using a dedicated water-cooled model to ensure that the slab is free of surface cracks and corner cracks.
[0011] This optional implementation addresses the characteristics of slow heat transfer and uneven billet growth in the 460mm extra-thick cross section. By using a dedicated water-cooling model to precisely control the specific water volume and temperature field distribution of each cooling section, the surface temperature of the billet avoids the high-temperature brittle zone, reducing the thermal stress gradient and thus effectively suppressing the generation of surface longitudinal cracks, transverse cracks, and corner cracks.
[0012] As an optional implementation, the 9Ni steel contains P≤0.003%, S≤0.001%, N≤25ppm, and the number of inclusions is <10 / mm², and the low-magnification segregation rating of the 9Ni steel slab is ≤C1.0.
[0013] This alternative implementation specifies the key quality indicators of the final product. The extremely low content of harmful elements and the areal density of inclusions ensure the toughness reserve of the steel at ultra-low temperatures, while the low magnification segregation rating below C1.0 ensures the density and compositional uniformity of the core structure of the extra-thick slab, meeting the stringent requirements for steel used in high-end LNG storage tanks.
[0014] As an optional implementation, after pretreatment of the molten iron, the S content in the molten iron is ≤0.002%; the oxygen content of the steel produced by the converter blowing is ≤500ppm, and the P content, S content, and N content of the steel produced are ≤0.003%, ≤0.008%, and ≤15ppm.
[0015] This alternative implementation strengthens impurity control in the front-end process, reduces the load on subsequent LF and RH refining, and lays the foundation for high-purity smelting of extra-thick slabs; in particular, controlling the nitrogen content of the converter steel to below 15ppm can effectively prevent the formation of nitride inclusions and ensure the low nitrogen level of the final molten steel. Beneficial effects
[0016] 1. This application optimizes the chemical composition design of 9Ni steel, controlling harmful elements such as P, S, and N to extremely low levels. Combined with the LF high-basicity high-Al2O3 slag diffusion deoxidation process, the strong adsorption capacity of high-basicity slag for xCaO·yAl2O3 inclusions is utilized. With the addition of long-term high vacuum and soft argon blowing treatment by RH, the inclusions are fully floated and removed, resulting in a significant improvement in the purity of molten steel. The number of inclusions in the tundish sample can be controlled to <10 inclusions / mm².
[0017] 2. This application introduces magnesium modification treatment in the RH refining stage, which transforms the easily agglomerated Al2O3 inclusions in the molten steel into fine and dispersed magnesium-aluminum spinel inclusions, reducing the probability of inclusion collision growth; at the same time, by controlling the Ca content in the molten steel, the precipitation of CaS inclusions during solidification is avoided, which improves the internal cleanliness of the billet from a microscopic level and provides microstructural protection for the low-temperature toughness of extra-thick slabs.
[0018] 3. This application addresses the solidification characteristics of an extra-thick 460mm section by employing a low casting speed of 0.40-0.60m / min in conjunction with a dedicated secondary cooling water-cooling model to precisely control the surface temperature field of the billet, avoiding surface and corner cracks caused by thermal stress concentration. Simultaneously, it utilizes a dynamic and precise light reduction technique with a reduction of ≥15mm to effectively compensate for the solidification shrinkage of the billet core, eliminate central porosity and segregation, and stably control the low-magnification segregation rating of the billet within C1.0 grade, achieving synergistic optimization of the internal and surface quality of the extra-thick 9Ni steel billet. Attached Figure Description
[0019] Figure 1 This is a ternary phase diagram of inclusions during RH bag lifting according to an embodiment of this application; Figure 2 This is a ternary phase diagram of inclusions in the continuous casting ladles according to an embodiment of this application; Figure 3 This is a low-magnification photograph of a 460mm cross-section of a 9Ni steel billet according to an embodiment of this application. Detailed Implementation
[0020] To make the objectives, technical solutions, and advantages of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Example 1
[0021] This embodiment provides a steelmaking and continuous casting process for 460mm cross-section extra-thick 9Ni steel slabs. This process addresses the technical challenges of long solidification time, easy inclusion aggregation, and severe central segregation in extra-thick sections. Through refined control throughout the entire process, it achieves a synergistic improvement in high purity and internal quality. In this embodiment, the chemical composition of the 9Ni steel, by mass percentage, includes: C≤0.08%, Si:0.15-0.30%, Mn:0.50-0.80%, P≤0.003%, S≤0.001%, Ni:8.50-9.50%, Cr≤0.10%, Mo≤0.05%, Nb≤0.01%, V≤0.01%, Al:0.020-0.050%, with the balance being Fe. Specifically, keeping C at an extremely low level is to avoid carbide precipitation that could impair low-temperature toughness; Ni, as the core alloying element, has a content range of 8.50-9.50%, which ensures that the steel still has a stable austenitic structure and excellent toughness at -196℃; strictly controlling the upper limits of P, S and Al content aims to reduce grain boundary segregation and the formation of brittle inclusions, laying the compositional foundation for obtaining high-purity molten steel.
[0022] The specific steps for implementing this steelmaking and continuous casting production process are as follows: Step S100 involves pretreating the molten iron. In this embodiment, after pretreatment, the sulfur content in the molten iron is controlled to ≤0.002%. Specifically, a mechanical stirring method combined with a high-efficiency desulfurizing agent is used for deep desulfurization treatment, reducing the sulfur content of the molten iron entering the furnace to an extremely low level. This front-end control measure significantly reduces the desulfurization burden on the subsequent LF refining furnace, shortens the LF treatment cycle, and thus reduces the risk of temperature drop and nitrogen absorption in the molten steel during refining, providing a source guarantee for the production of ultra-low sulfur 9Ni steel.
[0023] Step S200 involves converter blowing of the pretreated molten iron. In this embodiment, the oxygen content of the steel tapped from the converter is ≤500ppm, and the P content is ≤0.003%, S ≤0.008%, and N ≤15ppm. Specifically, a double-slag method or a slag-retaining method is used to enhance the converter's dephosphorization capacity, and low-oxygen tapping is achieved through optimized endpoint control technology. Low-oxygen tapping not only reduces the amount of subsequent deoxidizer added and lowers the base for the formation of inclusions in deoxidation products, but also controls the nitrogen content below 15ppm, effectively preventing the formation of nitride inclusions and ensuring that the molten steel entering the refining process has a high initial cleanliness.
[0024] Step S300 involves LF refining of the molten steel after tapping from the converter. LF refining employs a diffusion deoxidation process, with the final slag content being 10-18 kg / ton of steel, a binary basicity ≥6, and an Al2O3 content ≥24%. Specifically, a reducing slag system with high basicity and high alumina content is constructed by precisely adding lime and pre-melted slag. A binary basicity ≥6 provides strong desulfurization thermodynamic conditions, while an Al2O3 content ≥24% effectively lowers the slag melting point and improves the slag fluidity, enabling it to fully adsorb and dissolve easily agglomerated inclusions such as xCaO·yAl2O3 in the molten steel. Simultaneously, controlling the final slag amount within the range of 10-18 kg / ton of steel ensures a sufficient slag-metal reaction interface while avoiding the heating difficulties and arc instability problems caused by excessively thick slag layers.
[0025] Step S400 involves RH refining of the LF-refined steel. RH refining includes high-vacuum treatment and soft argon blowing. The high-vacuum treatment time is ≥25 min, and the H content in the molten steel after vacuum breaking is ≤1 ppm. The soft argon blowing time is ≥30 min. Specifically, considering the large volume and long floating distance of the 460mm extra-thick slab steel, the high-vacuum treatment time is extended to more than 25 minutes. This utilizes the CO bubbles generated by the carbon-oxygen reaction for deep dehydrogenation and promotes the collision and growth of small inclusions. After vacuum breaking, at least 30 minutes of weak stirring and soft argon blowing are performed to keep the molten steel in a quasi-static state, providing sufficient kinetic conditions for the floating and removal of modified fine inclusions. Ultimately, the hydrogen content is stably controlled below 1 ppm, eliminating the potential for white spot defects.
[0026] Step S500 involves continuous casting of the RH-refined molten steel at a casting speed of 0.40-0.60 m / min. The slab cross-section dimensions are 460 mm thick and 1800-2270 mm wide. The continuous casting includes dynamic light reduction treatment, with a reduction of ≥15 mm. Specifically, a low casting speed of 0.40-0.60 m / min is used to accommodate the slow solidification characteristics of the extra-thick cross-section, ensuring that the liquid core length matches the equipment's cooling capacity. Based on this, dynamic precision light reduction of ≥15 mm is implemented, accurately aligning the reduction position with the pasty area at the end of solidification. Mechanical extrusion compensates for the volume shrinkage of the solidified molten steel, forcing the solute-rich mother liquor to flow in the opposite direction, thereby effectively eliminating central porosity and segregation. This process combination is a key means to solve the internal quality problems of 460 mm extra-thick 9Ni steel slabs, ensuring that the central density of the slab meets the requirements of high-end applications.
[0027] Example 2 This embodiment, based on Embodiment 1, further specifies the deoxidation method and anti-oxidation measures in the LF refining stage. As an optional implementation, only aluminum wire is added for deoxidation during LF refining, and a lightweight insulating material is used to cover the surface of the steel slag after LF refining.
[0028] Specifically, in the LF refining process of step S300, the addition of deoxidizer is strictly limited to the addition of aluminum wire, rather than the conventional aluminum wire feeding process. The physical mechanism of this operational difference is as follows: aluminum wire feeding usually requires inserting the aluminum wire at high speed into the deep part of the molten steel through a wire feeding gun. This process will generate a strong mechanical stirring effect on the molten steel, which can easily lead to violent fluctuations at the steel-slag interface and even slag entrapment, thus increasing the number of large inclusions in the steel. In contrast, by directly adding aluminum wire, the aluminum wire gradually melts at the steel-slag interface and diffuses into the molten steel, resulting in a more stable and gentle deoxidation reaction. This avoids the risk of secondary pollution caused by external disturbances and is particularly suitable for smelting 9Ni steel, which requires extremely high purity.
[0029] In terms of slag system control, this embodiment achieves a binary basicity of ≥6 and an Al2O3 content of ≥24% in the final LF steel slag through precise addition of lime and pre-melted slag. These two parameters exhibit a significant synergistic effect: a binary basicity of ≥6 provides a strong reducing atmosphere and sufficient free CaO, creating favorable thermodynamic conditions for deep desulfurization; while an Al2O3 content of ≥24% effectively lowers the melting point of the high-basicity slag system, improves the fluidity of the slag liquid, and enables it to fully dissolve and adsorb easily agglomerated inclusions such as xCaO·yAl2O3 in the molten steel. If the Al2O3 content is too low, the high-basicity slag will become viscous, not only worsening the desulfurization kinetics but also losing its adsorption capacity for calcium aluminate inclusions; conversely, insufficient basicity prevents ultra-low sulfur control even with good fluidity. Therefore, both are indispensable, forming the core barrier for inclusion adsorption in the LF process.
[0030] Immediately after LF refining, the surface of the steel slag is covered with a lightweight insulating material. For example, carbonized rice husks can be used as a covering agent, as they have low bulk density and low thermal conductivity, forming a dense heat-insulating and air-barrier layer on the steel slag surface. This measure serves two purposes: firstly, it isolates the air from direct contact with the high-temperature steel slag, preventing atmospheric oxygen and nitrogen from penetrating into the molten steel and avoiding secondary oxidation and nitrogen accumulation; secondly, it reduces radiative heat loss from the molten steel, maintaining a stable LF outlet temperature and providing a good thermodynamic basis for subsequent RH vacuum treatment.
[0031] Example 3 This embodiment, based on Embodiment 1, further defines the control of inclusion morphology and the deep purification process during the RH refining stage. As an optional implementation, the RH refining also includes magnesium modification treatment, which modifies the Al2O3 inclusions in the molten steel into magnesium aluminum spinel inclusions, and controls the Ca content in the molten steel to prevent the precipitation of CaS inclusions during solidification.
[0032] Specifically, in the RH refining process of step S400, in addition to performing basic high-vacuum degassing and soft argon blowing operations, a magnesium modification process is introduced. This process involves adding a magnesium source, such as a magnesium-iron alloy or a nickel-magnesium alloy, to the molten steel. Utilizing the extremely strong deoxidizing ability and affinity of magnesium, the originally high-melting-point, easily agglomerated solid Al2O3 inclusions in the molten steel are transformed in situ into MgO·Al2O3 spinel-like inclusions. Figure 1 This is a ternary phase diagram of inclusions during RH bag lifting according to an embodiment of this application. Figure 2 This is a ternary phase diagram of inclusions in ladles during continuous casting, according to an embodiment of this application. (Combined with...) Figure 1 and Figure 2 As can be seen, after magnesium modification, the composition of inclusions significantly shifts from the pure Al2O3 region to the MgO-Al2O3 spinel phase region or the low-melting-point composite oxide region. This morphological transformation has key technical value: compared to the irregular and easily collide-grown Al2O3 clusters, Mg-Al spinel inclusions are spherical or near-spherical, small in size and dispersed, and their tendency to collide and aggregate in molten steel is greatly reduced, making it more difficult to form large inclusions that are detrimental to low-temperature toughness. It should be understood that although the figure shows a specific compositional evolution trend, in actual production, as long as the main body of the inclusions transforms into the Mg-Al spinel type and remains in a dispersed state, the modification objective of this application is considered to have been achieved.
[0033] While implementing magnesium modification, this embodiment places particular emphasis on strict control of the Ca content in the molten steel. This is because 9Ni steel has extremely high requirements for low-temperature toughness. If the residual Ca content in the molten steel is too high, CaS-like inclusions are easily precipitated at the grain boundaries due to solute enrichment at the end of solidification. CaS inclusions are not only brittle themselves, but also become the core for crack initiation, severely impairing the impact performance of the steel at -196℃. Therefore, in this embodiment, by accurately calculating the amount of magnesium source added and optimizing the oxidizing properties of the slag system, the Ca content in the molten steel is controlled at an extremely low level, for example, below 10 ppm, or dynamically adjusted through an online detection feedback mechanism, ensuring that the risk of CaS precipitation is completely avoided while achieving inclusion modification. This combination strategy of "magnesium modification + low Ca control" is the core innovation of this application, which distinguishes it from conventional 9Ni steel calcium treatment processes, and effectively solves the contradiction between the internal cleanliness and low-temperature toughness of extra-thick slabs.
[0034] To address the challenges of inclusion flotation caused by the large volume of molten steel and long solidification time in 460mm extra-thick slabs, this embodiment specifically matches the time window for RH refining. The high-vacuum treatment time is set to ≥25 min, and the soft-blown argon treatment time is set to ≥30 min. This process window is not arbitrarily determined but is based on the kinetic requirements of smelting extra-thick slabs: compared to conventional thin slabs, the 460mm cross-section corresponds to a larger volume of molten steel per furnace, a longer steel circulation path, and a significantly increased settling time required for the removal of small inclusions. Extending the high-vacuum time to over 25 minutes allows for the full utilization of CO bubbles generated by the carbon-oxygen reaction to carry hydrogen and small inclusions out; while the weak stirring soft-blown argon treatment for at least 30 minutes after vacuum breaking provides sufficient quasi-static flotation conditions for the modified fine spinel inclusions, avoiding re-entry or secondary oxidation of inclusions due to excessive stirring.
[0035] Example 4 This embodiment, based on Embodiment 1, further defines the adaptation process and final product quality verification for the 460mm extra-thick cross-section in the continuous casting stage. As an optional implementation, the casting speed is 0.40-0.60 m / min, and the slab cross-section dimensions are 460mm thick and 1800-2270mm wide. Specifically, compared to a conventional slab, the 460mm extra-thick cross-section has a significantly increased heat transfer distance from the center to the surface, resulting in a quadratic extension of the solidification time. Using a conventional casting speed could easily lead to an excessively long liquid core exceeding the equipment's support range, or bulging deformation due to an excessively thin shell. This embodiment strictly controls the casting speed within the low-speed range of 0.40-0.60 m / min to ensure that the residence time of the slab in the crystallizer and secondary cooling zone is sufficient to form a uniform shell of sufficient thickness, while simultaneously ensuring that the solidification end position stably falls within the effective operating area of the dynamic light-pressure equipment, creating the necessary preconditions for subsequent elimination of center segregation. It should be understood that this pulling speed range is an optimal window derived from thermal balance calculations based on a combination of 460mm thickness and 1800-2270mm width, ensuring both production safety and production efficiency.
[0036] As an optional implementation, the secondary cooling zone of continuous casting employs a dedicated water-cooling model to ensure that the slab is free of surface and corner cracks. Specifically, 9Ni steel is a crack-sensitive steel, and the large temperature difference between the surface and core of the extra-thick slab during cooling leads to concentrated thermal stress, which easily induces cracks. The dedicated water-cooling model used in this application is not a simple constant water volume control, but a dynamic water distribution strategy based on real-time temperature field feedback of the slab. For example, a weak cooling mode is used in the early stage of secondary cooling to reduce the cooling intensity and decrease the thermal gradient on the slab surface; in the later stage of secondary cooling, the water volume ratio of each circuit is dynamically adjusted according to the casting speed to ensure that the slab surface temperature always avoids the high-temperature brittle zone of 700℃-900℃ before entering the straightening zone. This refined temperature field management effectively suppresses surface longitudinal cracks, transverse cracks, and corner cracks caused by the superposition of phase transformation stress and thermal stress, providing a reliable guarantee for the surface quality of extra-thick slabs.
[0037] As an optional implementation, continuous casting includes dynamic light reduction treatment, with a reduction of ≥15mm. Specifically, for a 460mm extra-thick slab, the volume voids caused by central solidification shrinkage are the root cause of central segregation and porosity. Conventional light reduction (e.g., 5-10mm) is insufficient to penetrate the thick slab shell and effectively compress the core mushy region. This embodiment sets a large reduction of ≥15mm, precisely aligning the reduction roller gap with the mushy region at the end of solidification, using mechanical force to forcibly compact the solidifying dendritic framework, extruding the solute-rich mother liquor, and promoting the densification of the equiaxed crystal region. Figure 3 This is a low-magnification microstructure photograph of a 460mm cross-section of a 9Ni steel billet according to an embodiment of this application. Figure 3 As shown, the central region of the cross-section of the slab produced by this process has a dense microstructure with no obvious shrinkage cavities or porosity bands, and the low-magnification segregation rating is consistently controlled within C1.0. This visual evidence directly confirms the effect of a large reduction of ≥15mm on improving the internal quality of extra-thick slabs.
[0038] As an optional implementation, the 9Ni steel contains P ≤ 0.003%, S ≤ 0.001%, N ≤ 25ppm, and inclusions < 10 per mm², with a low-magnification segregation rating of ≤ C1.0 for the 9Ni steel slab. The P, S, and N contents reflect the comprehensive purification capabilities of the hot metal pretreatment, converter, and refining processes; the low-magnification segregation rating of ≤ C1.0 verifies the accuracy of the matching between the continuous casting light reduction and the casting speed. Through the aforementioned closed-loop control of "composition-process-quality," this embodiment successfully achieved the synergistic manufacturing of a 460mm thick 9Ni steel slab with high purity, high density, and a defect-free surface.
[0039] Example 5 To further verify the necessity and critical effect of the key technical parameters of this application, a set of comparative examples was set up in this embodiment. In this comparative example, except that the binary basicity of the steel slag at the end of the LF refining stage was adjusted to 4.5, all other production process conditions were completely consistent with those of Examples 1 to 4. Specifically, the chemical composition of 9Ni steel, the sulfur content after hot metal pretreatment, the oxygen and nitrogen content of the steel tapped from the converter, the amount of slag and Al2O3 content at the end of LF refining, the high vacuum time and soft argon blowing time of RH refining, and the casting speed, cross-sectional dimensions and dynamic light reduction in the continuous casting stage were all strictly controlled within the range described in Example 1. Only the binary basicity of the steel slag at the end of LF refining was reduced from ≥6 to 4.5 to examine the impact of this parameter deviating from the range defined in this application on the final product quality.
[0040] Testing revealed a significant deterioration in the purity and internal quality of the 460mm cross-section 9Ni steel slab produced in this comparative example. Specifically, the number of inclusions in the cross-sectional sample of the slab reached 18 per mm², far exceeding the <10 per mm² level achievable in the embodiments of this application. Furthermore, low-magnification microstructure examination of the slab showed a center segregation rating of C2.0, failing to meet the quality requirement of ≤C1.0. This negative result directly demonstrates that when the binary basicity of the LF slag system is below 6, even with other process parameters under optimal control, it is impossible to produce qualified high-purity extra-thick slabs.
[0041] The root cause of the aforementioned quality defects lies in the imbalance of thermodynamic and kinetic conditions of the slag system. Specifically, binary basicity is a key indicator determining the slag's desulfurization capacity and inclusion adsorption capacity. When the binary basicity drops to 4.5, the activity of free CaO in the slag decreases significantly, leading to a sharp decline in the slag's ability to dissolve and adsorb easily agglomerated inclusions such as xCaO·yAl2O3 in the molten steel. A large number of unadsorbed inclusions remain in the molten steel and eventually remain inside the billet. In addition, lower basicity also leads to an increase in the melting point and viscosity of slag systems with high Al2O3 content, hindering the mass transfer process at the slag-metal reaction interface and further weakening the purification efficiency of the refining process. For 460mm extra-thick slabs, due to the long solidification time, residual inclusions have more time to collide, grow, and accumulate in the central region, thus exacerbating central segregation and porosity defects. Therefore, the limitation of the binary basicity of steel slag at the LF refining endpoint to ≥6 in this application is not a conventional choice or arbitrary designation in the field, but a necessary technical means determined based on the smelting characteristics of extra-thick slabs. It plays an irreplaceable role in achieving deep purification of molten steel and internal quality control of cast billets.
[0042] The above description is merely a specific implementation of this application, but the scope of protection of this application is not limited thereto.
Claims
1. A steelmaking and continuous casting process for 460mm cross-section extra-thick 9Ni steel slabs, characterized in that, The chemical composition of the 9Ni steel, by mass percentage, includes: C≤0.08%, Si:0.15-0.30%, Mn:0.50-0.80%, P≤0.003%, S≤0.001%, Ni:8.50-9.50%, Cr≤0.10%, Mo≤0.05%, Nb≤0.01%, V≤0.01%, Al:0.020-0.050%, with the balance being Fe; The steelmaking and continuous casting production process includes: Pretreatment of molten iron; The pretreated molten iron is then smelted in a converter. The molten steel after tapping from the converter is subjected to LF refining. The LF refining adopts a diffusion deoxidation process. The final slag content of the LF refining is 10-18 kg / ton of steel, the binary basicity is ≥6, and the Al2O3 content is ≥24%. The molten steel after LF refining is subjected to RH refining, which includes high vacuum treatment and soft argon blowing treatment. The high vacuum treatment time is ≥25min, and the H content in the molten steel after vacuum breaking is ≤1ppm. The soft argon blowing treatment time is ≥30min. The molten steel refined by RH is continuously cast at a casting speed of 0.40-0.60 m / min. The slab cross-sectional dimensions are 460 mm thick and 1800-2270 mm wide. The continuous casting includes dynamic light reduction treatment, and the reduction amount of the dynamic light reduction treatment is ≥15 mm.
2. The production process according to claim 1, characterized in that, In the LF refining process, only aluminum wire is added for deoxidation, and after the LF refining is completed, a lightweight insulation material is used to cover the surface of the steel slag.
3. The production process according to claim 1, characterized in that, The RH refining process also includes magnesium modification treatment, which modifies the Al2O3 inclusions in the molten steel into magnesium aluminum spinel inclusions, and controls the Ca content in the molten steel to prevent the precipitation of CaS inclusions during solidification.
4. The production process according to claim 1, characterized in that, The secondary cooling zone of the continuous casting uses a special water-cooled model for cooling to ensure that the slab is free of surface cracks and corner cracks.
5. The production process according to claim 1, characterized in that, The 9Ni steel contains P≤0.003%, S≤0.001%, N≤25ppm, and inclusions<10 per mm². The low-magnification segregation rating of the 9Ni steel slab is ≤C1.
0.
6. The production process according to claim 1, characterized in that, After pretreatment, the sulfur content in the molten iron is ≤0.002%. The oxygen content of the steel produced by the converter blowing process is ≤500ppm, and the P content, S content, and N content of the steel produced are ≤0.003%, ≤0.008%, and ≤15ppm.