A flexible perovskite solar cell based on a decoupled self-assembly molecular-perovskite co-deposition strategy and its fabrication method.
By employing a self-assembled molecule-perovskite co-deposition strategy with decoupling agents doped on a flexible conductive substrate, the problem of uniform anchoring and crystallization of self-assembled molecules and perovskite precursors on the flexible substrate is solved, enabling the fabrication of efficient and stable flexible perovskite solar cells and modules, suitable for large-area applications and industrial production.
Patent Information
- Application Number
- CN202611127087.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-28
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies struggle to achieve uniform anchoring and efficient crystallization of self-assembled molecules and perovskite precursors on flexible conductive substrates, leading to performance degradation in large-area flexible modules and becoming a bottleneck restricting the commercialization of flexible perovskite modules.
By employing a decoupled self-assembled molecule-perovskite co-deposition strategy, and controlling interfacial interactions through doping with bifunctional decoupling agents, a self-assembled monolayer/perovskite layer was prepared, achieving uniform anchoring of self-assembled molecules and efficient crystallization of perovskite.
It has enabled the fabrication of efficient and stable flexible perovskite solar cells and modules, which are suitable for large-area applications, improve device performance and stability, and are suitable for industrial production.
Smart Images

Figure CN123076100A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photovoltaic materials technology, specifically relating to a flexible perovskite solar cell based on a decoupled self-assembly molecule-perovskite co-deposition strategy and its preparation method. Background Technology
[0002] Flexible perovskite solar cells possess advantages such as being lightweight, flexible, low-cost, and capable of large-area fabrication, making them promising for applications in curved photovoltaic buildings, automotive photovoltaics, aerospace, and wearable electronic devices. Currently, the photoelectric conversion efficiency (PCE) of small-area flexible devices has exceeded 26%, but efficiency and stability decrease sharply as the device area is increased, becoming a core bottleneck restricting the commercialization of flexible perovskite modules.
[0003] The fundamental reason for the performance degradation of large-area flexible components lies in the interface defects of flexible conductive substrates: flexible substrates are mostly deposited with low-temperature ITO, which has low crystallinity and surface hydroxyl groups are easy to desorb quickly in polar solvents; at the same time, the phosphonic acid groups in the self-assembled molecules have strong interactions with the perovskite precursor, which leads to delayed anchoring and uneven distribution of self-assembled molecules, thereby disrupting the perovskite crystallization process and generating a large number of defects and grain boundary pores.
[0004] While traditional self-assembled molecule-perovskite co-deposition processes have solved the film wettability problem, they cannot overcome the dynamic competition between hydroxyl desorption and molecular anchoring on flexible substrates, making it difficult to achieve large-area uniform film formation. Therefore, there is an urgent need to develop an efficient decoupling strategy to precisely control the interaction between self-assembled molecules and perovskite precursors, achieve uniform interface modification and high-quality perovskite crystallization, and break through the performance bottleneck of large-area flexible components. Summary of the Invention
[0005] Technical problem solved: To address the above-mentioned technical problems, this invention provides a flexible perovskite solar cell based on a decoupled self-assembled molecule-perovskite co-deposition strategy and its preparation method. By regulating the interfacial interaction through a bifunctional decoupling agent, uniform anchoring of self-assembled molecules and efficient crystallization of perovskite are achieved, resulting in a high-efficiency, stable, and scalable flexible perovskite solar cell and module.
[0006] Technical solution: In a first aspect, the present invention provides a flexible perovskite solar cell based on a decoupled self-assembled molecule-perovskite co-deposition strategy, comprising a flexible conductive substrate, a self-assembled monolayer / perovskite layer, an electron transport layer and a cathode, wherein the self-assembled monolayer / perovskite layer is prepared by co-deposition of a self-assembled molecule-perovskite precursor solution doped with a decoupling agent.
[0007] Preferably, the chemical structural formula of the self-assembled molecule is: , Wherein, R is a neutral substituent, a weak electron-donating substituent, or a weak electron-withdrawing substituent.
[0008] Furthermore, the chemical structural formula of R is as follows: .
[0009] Preferably, the chemical structural formula of the decoupling agent is: , In this context, R1 is an organic ammonium ion, and R2 is a substituent with strong coordinating ability.
[0010] Furthermore, the chemical structural formula of R1 is as follows: ; The chemical structural formula of R2 is as follows: .
[0011] Furthermore, the decoupling agent is 3,5-bis(methanesulfonyl)aniline iodide (BSAI), 3,5-bis(methylthio)aniline iodide (BTAI), 3,5-bis(methanesulfonyl)benzaldehyde imine iodide (BSMAI) or 3,5-bis(methylthio)benzaldehyde imine iodide (BTMAI).
[0012] Preferably, the flexible conductive substrate is PET / ITO, and the electron transport layer is C. 60 / BCP composite layer, wherein the cathode is a copper electrode.
[0013] In a second aspect, the present invention provides a method for preparing the flexible perovskite solar cell described in the first aspect, comprising the following steps: S1. Prepare a self-assembled molecule-perovskite precursor solution doped with decoupling agent; S2. Spin-coat the precursor solution onto a flexible conductive substrate, adding the antisolvent chlorobenzene during the spin-coating process, and then heat-treating to obtain a self-assembled monolayer / perovskite layer. S3. An electron transport layer and a cathode are sequentially fabricated on the perovskite layer to obtain a flexible perovskite solar cell.
[0014] Preferably, the doping concentration of the decoupling agent in the precursor solution is 1.0–3.5 mmol / L; the heat treatment conditions are 110–130°C for 20–40 minutes.
[0015] Preferably, the precursor solution is Cs. 0.05 FA 0.95The PbI3 system uses DMF / DMSO in a volume ratio of 4:1, with PbI2 concentrations of 1.7–1.9 mmol / mL, MACl concentrations of 0.15–0.17 mmol / mL, CsI concentrations of 0.05–0.1 mmol / mL, FAI concentrations of 1.45–1.6 mmol / mL, and self-assembled molecules concentrations of 1.0–3.5 mmol / L.
[0016] Thirdly, the present invention provides a decoupling agent modified perovskite thin film, which is prepared by the following method: a self-assembled molecule-perovskite precursor solution doped with the decoupling agent described in the first aspect is spin-coated onto a flexible conductive substrate, and after adding the antisolvent chlorobenzene, it is heat-treated at 110-130°C for 20-40 minutes to obtain a self-assembled monolayer / perovskite layer thin film, namely, a decoupling agent modified perovskite thin film.
[0017] Fourthly, the present invention provides the application of the decoupling agent modified perovskite thin film described in the third aspect in the preparation of flexible perovskite solar cells or flexible perovskite modules of different areas.
[0018] The decoupling agent of this invention precisely decouples the binding of self-assembled molecules to perovskite precursors through strong two-site interactions: it releases the bound self-assembled molecules, allowing them to quickly anchor on the flexible ITO surface and form a uniform and dense monolayer; it suppresses the disturbance of perovskite crystallization by residual self-assembled molecules, induces uniform grain growth, and reduces defect density; it requires no additional interface layer or post-processing, the process is simple and scalable, and it is suitable for the fabrication of large-area flexible components.
[0019] Beneficial effects: 1) This invention grows a self-assembled monolayer / perovskite layer on a flexible conductive substrate by doping a decoupling agent in a self-assembled molecule-perovskite precursor solution, and prepares a high-efficiency and stable flexible perovskite solar cell based on this film. 2) This invention, through the ingenious design of functional groups of decoupling agents, regulates the interaction with different components (FAI / PbI2) in perovskite materials, inhibits the binding of self-assembled molecules with perovskite components, thereby releasing self-assembled molecules, and thus achieving uniform distribution of self-assembled molecules and ordered crystallization of perovskite, and finally preparing high-quality self-assembled monolayer / perovskite layer on flexible conductive substrate. 3) The method for preparing self-assembled monolayers / perovskite layers in this invention is also applicable to the preparation of large-area self-assembled monolayers / perovskite layers, thereby obtaining efficient large-area flexible perovskite components, and achieving demonstrative applications in portable chargers and remote-controlled drones; 4) The preparation method of the present invention is simple, does not introduce an additional interface layer or post-processing process, and the product has excellent performance and is suitable for industrial production. Attached Figure Description
[0020] Figure 1 It is 3,5-bis(methanesulfonyl)aniline iodide (BSAI) 1 H NMR spectrum; Figure 2 SEM images of flexible perovskite films before and after doping with decoupling agent; Figure 3 The time-of-flight secondary ion mass spectra of flexible perovskite films before and after doping with the decoupling agent; Figure 4 AFM-IR images of flexible self-assembled monolayer films before and after doping with decoupling agent; Figure 5 Current-voltage curve of flexible perovskite solar cell (effective area 0.0628 cm²) 2 ); Figure 6 This is a voltage-light intensity dependence curve for flexible perovskite solar cells. Figure 7 The figures show the current-voltage curves of flexible perovskite solar cells based on different doping amounts of decoupling agents. Figure 8 The steady-state fluorescence intensity distribution of flexible perovskite films with different areas is shown in the figure. Figure 9 30×35 cm 2 Schematic diagram of perovskite thin film and UV absorption curves of flexible perovskite thin film before and after doping with decoupling agent; Figure 10 Current-voltage curves for flexible perovskite modules (areas 14.55, 80, and 750 cm²). 2 ); Figure 11 For different self-assembled molecules 14.55 cm 2 Current-voltage curve of flexible perovskite module; Figure 12 The graph shows the operational stability of the flexible perovskite module. Figure 13 This is a graph showing the bending stability of a flexible perovskite component. Figure 14 Real-time power output diagram of a portable charger; Figure 15 This is a graph showing the real-time power output of a remotely controlled drone. Detailed Implementation
[0021] The present invention will be described in detail below with reference to specific embodiments: A method for fabricating flexible perovskite solar cells based on a decoupled self-assembly molecule-perovskite co-deposition strategy includes the following steps: (1) First, prepare a self-assembled molecule-perovskite precursor solution doped with a decoupling agent (Cs).0.05 FA 0.95 PbI3, solvent DMF / DMSO); (2) Spin-coat the prepared self-assembled molecule-perovskite precursor solution onto a clean PET / ITO substrate, add the anti-solvent chlorobenzene, and anneal to obtain a self-assembled monolayer / perovskite layer film with a thickness of 500-700 nm. (4) The electron transport layer is C 60 The / BCP composite electron transport layer was deposited using a vacuum evaporation machine, with thicknesses of 25 nm and 5 nm, respectively. (5) The electrode is a copper electrode, which is deposited by vacuum evaporation machine with a thickness of 100 nm.
[0022] The preparation method of the decoupling agent is as follows: 1) The synthesis reaction formula for the decoupling agent 3,5-bis(methanesulfonyl)aniline iodide (BSAI) is as follows: , 3,5-Di(methanesulfonyl)aniline was added to a reaction flask, and ethanol was added and stirred until completely dissolved. Under an argon atmosphere, hydroiodic acid was slowly added and stirred continuously at room temperature for 6 h. After the reaction was completed, the product was filtered under reduced pressure to obtain a light yellow solid crude product. The crude product was purified by recrystallization from diethyl ether and dried under vacuum to obtain a white solid product BSAI.
[0023] 2) The synthesis reaction formula for the decoupling agent 3,5-di(methylthio)aniline iodide (BTAI) is as follows: , 3,5-Di(methylthio)aniline was added to a reaction flask, and ethanol was added and stirred until completely dissolved. Under an argon atmosphere, hydroiodic acid was slowly added and stirred continuously at room temperature for 6 h. After the reaction was completed, the product was filtered under reduced pressure to obtain a light yellow solid crude product. The crude product was purified by recrystallization from diethyl ether and dried under vacuum to obtain a white solid product BTAI.
[0024] 3) The synthetic reaction formula for the decoupling agent 3,5-bis(methanesulfonyl)benzaldehyde imine iodide (BSMAI) is as follows: , 3,5-Di(methanesulfonyl)benzaldehyde imine was added to a reaction flask, and ethanol was added and stirred until completely dissolved. Under an argon atmosphere, hydroiodic acid was slowly added and stirred continuously at room temperature for 6 h. After the reaction was completed, the product was filtered under reduced pressure to obtain a light yellow solid crude product. The crude product was purified by recrystallization from diethyl ether and dried under vacuum to obtain a white solid product BSMAI.
[0025] 4) The synthesis reaction formula for the decoupling agent 3,5-bis(methylthio)benzaldehyde imine iodide (BTMAI) is as follows: , 3,5-Di(methylthio)benzaldehyde imine was added to a reaction flask, and ethanol was added and stirred until completely dissolved. Under an argon atmosphere, hydroiodic acid was slowly added and stirred continuously at room temperature for 6 h. After the reaction was completed, the product was filtered under reduced pressure to obtain a light yellow solid crude product. The crude product was purified by recrystallization from diethyl ether and dried under vacuum to obtain a white solid product BTMAI.
[0026] Device photoelectric performance testing: Newport xenon lamps were used to simulate AM 1.5G standard sunlight with a light intensity of 100 mW / cm². 2 Current-voltage data were acquired using a Keithley 2400 digital source meter; light intensity calibration was performed using a standard silicon solar cell with a KG-5 filter; the effective area of the device was calibrated using a precise aperture, and the test area included 0.0628 cm². 2 14.55 cm 2 80 cm 2 and 750 cm 2 Steady-state photoelectric conversion efficiency is measured by V max The stable photocurrent density was calculated under bias voltage. Example 1
[0027] The preparation method of the decoupling agent 3,5-bis(methanesulfonyl)aniline iodide (BSAI) is as follows: 3,5-Di(methanesulfonyl)aniline (2.493 g, 10.00 mmol) was added to a three-necked flask, and 20 mL of ethanol was added and stirred until completely dissolved. Under an argon atmosphere, hydroiodic acid (1.39 g, 10.05 mmol) was slowly added, and the mixture was stirred continuously at room temperature for 6 h. After the reaction was completed, the product was filtered under reduced pressure to obtain a pale yellow solid crude product. The crude product was recrystallized from diethyl ether and dried under vacuum to obtain a white solid BSAI with a yield of 2.111 g, or 56%.
[0028] 3,5-Di(methanesulfonyl)aniline iodide 1 H NMR image as follows Figure 1 As shown: ¹H NMR (400 MHz, DMSO) δ: 7.44 (s, 1H), 7.38 (s, 3H), 7.34 (s, 2H), 3.22 (s, 6H). Example 2
[0029] Thin film preparation with doped decoupling agents: (1) Prepare a precursor solution doped with 1.5 mmol / L BSAI (obtained from Example 1): The solvent is DMF / DMSO (volume ratio 4:1), and the concentrations of each component are: PbI2 1.76 mmol / mL, MACl 0.16 mmol / mL, CsI 0.08 mmol / mL, FAI 1.52 mmol / mL, and self-assembled molecule Me-4PACz 1.5 mmol / L; (2) Spin-coating film on the cleaned PET / ITO substrate: 4000 rpm, 45 s, add anti-solvent chlorobenzene 10 s before the end of spin coating; (3) Anneal at 120℃ for 30 min to obtain a flexible self-assembled monolayer / perovskite layer film doped with decoupling agent.
[0030] Preparation of comparative thin films without decoupling agents: Except for the absence of the decoupling agent BSAI, the precursor ratio, spin coating parameters, and annealing conditions are completely consistent with the thin film preparation with the above-mentioned doped decoupling agent, and an undoped control thin film is prepared.
[0031] like Figure 2 As shown, the top and bottom grains of the BSAI-doped perovskite film exhibit a uniform and dense morphology, with a significant reduction in intergranular pores; the undoped film, on the other hand, has uneven grain size and dense pores. These results demonstrate that the decoupling agent effectively eliminates the disturbance effect of self-assembled molecules on perovskite crystallization, significantly improving the film's crystallinity quality. Example 3
[0032] Self-assembled monolayers / perovskite layers were prepared using the doped / undoped precursor systems of Example 2, respectively. The doping decoupling agent was BTMAI at a concentration of 1.5 mmol / L, and time-of-flight secondary ion mass spectrometry was performed.
[0033] The results are as follows Figure 3 As shown, BTMAI doping exhibits strong and uniform PO2 at the ITO / perovskite interface. - The characteristic fragment signal (attributed to self-assembled molecules) indicates that the molecules are uniformly and densely anchored at the interface; the weak signal of the undoped group and its disordered distribution within the perovskite film indicate that most molecules remain inside the perovskite film, resulting in uneven anchoring at the interface. The results demonstrate that the decoupling agent can accelerate the anchoring dynamics of self-assembled molecules, significantly reduce molecule residue inside the perovskite, and thus achieve uniform distribution and anchoring of self-assembled molecules at the ITO / perovskite interface. Example 4
[0034] Self-assembled monolayers / perovskite layers were prepared using the doped / undoped precursor systems of Example 2, respectively. The perovskite layer was then removed by washing with DMF solvent to obtain self-assembled monolayer films anchored only on the PET / ITO surface.
[0035] The results are as follows Figure 4 As shown, the self-assembled monolayer doped with BSAI exhibits a strong and uniform characteristic infrared signal, indicating that the molecules are uniformly and densely anchored on the flexible substrate surface; the undoped group shows a weak and unevenly distributed signal, indicating obvious interface defects. The results demonstrate that the decoupling agent effectively solves the key problems of delayed anchoring and uneven distribution of self-assembled molecules on flexible conductive substrates. Example 5
[0036] Fabrication of doped devices: (1) Flexible perovskite films doped with BSAI were prepared using the method of Example 2; (2) Vacuum evaporation at 25 nm C 60 + 5 nm BCP electron transport layer; (3) Vacuum evaporation of a 100 nm copper electrode yielded an effective area of 0.0628 cm². 2 Flexible devices.
[0037] Fabrication of undoped contrast devices: Except for the absence of a decoupling agent, the rest of the process is completely consistent with the fabrication of the doped devices described above.
[0038] The current-voltage curve of a flexible perovskite solar cell is shown in the figure below. Figure 5 As shown in Table 1 below: Table 1 Photovoltaic performance parameters of flexible perovskite solar cells
[0039] Depend on Figure 5 As shown in Table 1, after doping with the decoupling agent, the open-circuit voltage and fill factor of the device are significantly improved, and the photoelectric conversion efficiency reaches 26.94%; the efficiency of the undoped device is only 24.47%. This proves that the decoupling agent effectively suppresses nonradiative recombination, reduces interface transport losses, and significantly improves the performance of small-area flexible devices. Example 6
[0040] The device was fabricated using the decoupling agent BSMAI at a concentration of 1.5 mmol / L according to the process in Example 5, and the voltage-light intensity dependence was tested under different light intensities.
[0041] V OC The curve relating to light intensity ( Figure 6 )show, V OCProportional to the logarithm of light intensity, the slopes of the undoped and doped BSMAI flexible devices are 1.82kT / q and 1.07kT / q, respectively, where k is the Boltzmann constant, T is the temperature, and q is the elementary charge. The decrease in slope indicates that trap-assisted recombination in the decoupling agent-doped perovskite thin film is effectively suppressed, promoting… V OC This enhances and improves the performance of flexible devices. Example 7
[0042] BSAI doping concentrations were set to 0, 1, 1.5, 2.5, and 3.5 mmol / L. Devices were fabricated and their performance was tested according to the process in Example 5. The results are shown in Table 2. Figure 7 As shown.
[0043] Table 2 Comparison of photovoltaic performance parameters of flexible perovskite solar cells with different doping amounts
[0044] The results show that doping concentrations in the range of 1.0–3.5 mmol / L can improve device performance; 1.5 mmol / L is the optimal doping concentration. V OC FF and PCE reach their maximum values. Example 8
[0045] Large-area film deposition process (1) The precursor solvent was changed to DMF / 2-Me / NMP (volume ratio 5:14:1), and the component concentrations were: PbI2 1.3 mmol / mL, MACl 0.42 mmol / mL, CsI 0.06 mmol / mL, FAI 1.14 mmol / mL, Me-4PACz 1.5 mmol / L, BSAI 1.5 mmol / L; (2) Slit coating is used: substrate / coating head spacing is 0.15 mm, coating speed is 8 mm / s, liquid injection speed is 0.1 mL / min, nitrogen air knife pressure is 0.3 MPa and speed is 12 mm / s; (3) Prepare 5×5 cm 2 10×10 cm 2 and 30×35 cm 2 Large-area films are annealed at 120°C for 30 minutes.
[0046] Steady-state fluorescence intensity distribution of flexible perovskite films of different areas is shown in the figure. Figure 8 As shown, after doping with the decoupling agent, films of different areas all exhibited stronger and more uniform steady-state fluorescence signals, indicating that the film quality is significantly less dependent on the substrate area, and large-area, high-quality film deposition can be achieved. Example 9
[0047] Decoupling agent BTAI in 30×35 cm 2 Applications in large-area thin films 30×35 cm slit coatings were prepared according to the slit coating process in Example 8. 2 Large-area flexible perovskite thin films, containing Me-4PACz 1.5 mmol / L and BTAI 1.5 mmol / L. (Example: ...) Figure 9 As shown, the prepared film was divided into nine regions according to the coating direction, and ultraviolet absorption tests were performed to obtain the ultraviolet absorption curves of the perovskite film in the nine regions. After doping with the decoupling agent BTAI, the nine regions of the perovskite film exhibited a more uniform absorption intensity, indicating that the uniformity of the film was significantly improved. Example 10
[0048] A large-area thin film was prepared according to the slit coating process in Example 8, and C was deposited by vapor deposition. 60 BCP and copper electrodes were used to obtain flexible components of different areas, and their performance is shown in Table 3. Figure 10 As shown.
[0049] Table 3 Photovoltaic performance of flexible perovskite modules with different areas
[0050] From Table 3 and Figure 10 It can be seen that the efficiency of undoped components decreases sharply with increasing area; the efficiency of doped components decreases significantly at 750 cm². 2 Even with an ultra-large area, the efficiency remains high at 20.56%, and the efficiency loss is significantly reduced, proving that the strategy of this invention can achieve efficient and stable fabrication of large-area flexible components. Example 11
[0051] Three different self-assembled molecules, MeO-2PACz, 4PADCB, and DMAcPA, were selected, and the BSAI doping concentration was fixed at 1.5 mmol / L to prepare 14.55 cm⁻¹ molecule. 2 Flexible components, performance is shown in Table 4 and Figure 11 As shown.
[0052] Table 4 Performance of different self-assembled molecular components
[0053] The results demonstrate that the decoupling strategy of this invention has good adaptability to various phosphonic acid self-assembly molecules, can significantly improve the efficiency of devices in different systems, and has excellent versatility. Example 12
[0054] The 14.55 cm prepared in Example 10 2 The components are treated as objects, and their operational stability and mechanical bending stability are tested.
[0055] Operating stability (ISOS-L-3, 1 sun, 85℃, maximum power point): The efficiency retention rate of the undoped module after 1044 h was only 42.1%; the retention rate of the doped module reached 92.5%. Figure 12 ); Bending stability (bending radius 10 mm): Undoped components retained 75.5% after 10,000 bends; doped components retained 92.1%. Figure 13 ).
[0056] The results show that the decoupling agent reduces self-assembled molecular residues, enhances interfacial bonding strength, and significantly improves device operational stability and mechanical reliability. Example 13
[0057] Using 750 cm 2 Large-area flexible components are being validated in practical applications.
[0058] Portable charger: Output power is 20.5W in sunny weather and 12.1W in cloudy evenings, providing stable power to personal electronic devices such as mobile phones and tablets. Figure 14 ); Remote-controlled drone: After integrating flexible components, the overall weight only increases by 8%, the flight time is extended from 8 minutes to 19 minutes, and the flight distance is increased from 4 km to 9.5 km, without affecting flight control and balance. Figure 15 ).
[0059] This invention achieves uniform distribution of self-assembled molecules through a decoupling agent, solving the problem of uneven molecular anchoring on flexible substrates and reducing interface defect density by more than 90%. The perovskite grains are dense, uniform, and pore-free, with significantly improved crystallinity, suitable for substrates ranging from 0.06 to 750 cm⁻¹. 2 Full-area film deposition; efficiency of small-area devices exceeds 26%, and efficiency degradation rate of large-area components is <5%, with excellent working stability and bending stability; low-temperature process, no extra steps, compatible with roll-to-roll large-area preparation, and can be applied to scenarios such as portable chargers and drone power supply.
[0060] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A flexible perovskite solar cell based on a decoupled self-assembly molecular-perovskite co-deposition strategy, characterized in that, It includes a flexible conductive substrate, a self-assembled monolayer / perovskite layer, an electron transport layer, and a cathode. The self-assembled monolayer / perovskite layer is prepared by co-deposition of a self-assembled molecule-perovskite precursor solution doped with a decoupling agent.
2. The flexible perovskite solar cell based on the decoupled self-assembly molecular-perovskite co-deposition strategy according to claim 1, characterized in that, The chemical structural formula of the self-assembled molecule is: , Wherein, R is a neutral substituent, a weak electron-donating substituent, or a weak electron-withdrawing substituent.
3. The flexible perovskite solar cell based on the decoupled self-assembly molecular-perovskite co-deposition strategy according to claim 2, characterized in that, The chemical structural formula of R is as follows: 。 4. The flexible perovskite solar cell based on the decoupled self-assembly molecular-perovskite co-deposition strategy according to claim 1, characterized in that, The chemical structural formula of the decoupling agent is: , In this context, R1 is an organic ammonium ion, and R2 is a substituent with strong coordinating ability.
5. The flexible perovskite solar cell based on the decoupled self-assembly molecular-perovskite co-deposition strategy according to claim 4, characterized in that, The chemical structural formula of R1 is as follows: ; The chemical structural formula of R2 is as follows: 。 6. A method for fabricating a flexible perovskite solar cell based on a decoupled self-assembly molecular-perovskite co-deposition strategy as described in claim 1, characterized in that, Includes the following steps: S1. Prepare a self-assembled molecule-perovskite precursor solution doped with decoupling agent; S2. Spin-coat the precursor solution onto a flexible conductive substrate, adding the antisolvent chlorobenzene during the spin-coating process, and then heat-treating to obtain a self-assembled monolayer / perovskite layer. S3. An electron transport layer and a cathode are sequentially fabricated on the perovskite layer to obtain a flexible perovskite solar cell.
7. The preparation method according to claim 6, characterized in that: The doping concentration of the decoupling agent in the precursor solution is 1.0–3.5 mmol / L; the heat treatment conditions are 110–130℃ for 20–40 minutes.
8. The preparation method according to claim 6, characterized in that: The precursor solution is Cs 0.05 FA 0.95 The PbI3 system uses DMF / DMSO in a volume ratio of 4:1, with PbI2 concentrations of 1.7–1.9 mmol / mL, MACl concentrations of 0.15–0.17 mmol / mL, CsI concentrations of 0.05–0.1 mmol / mL, FAI concentrations of 1.45–1.6 mmol / mL, and self-assembled molecules concentrations of 1.0–3.5 mmol / L.
9. A decoupling agent modified perovskite thin film, characterized in that, The preparation method of the decoupling agent modified perovskite film is as follows: spin-coat a self-assembled molecule-perovskite precursor solution of the doped decoupling agent as described in claim 1 onto a flexible conductive substrate, add the antisolvent chlorobenzene, and then heat-treat at 110-130°C for 20-40 minutes to obtain a self-assembled monolayer / perovskite layer film, i.e., a decoupling agent modified perovskite film.
10. The application of the decoupling agent modified perovskite film according to claim 9 in the preparation of flexible perovskite solar cells or flexible perovskite modules of different areas.