Solid electrolyte sheets and all-solid-state batteries containing them
By using hydrogenated nitrile butadiene rubber (HNBR) binder and porous support to control porosity, the problems of low ionic conductivity and lithium dendrite growth in all-solid-state batteries were solved, achieving high-rate discharge capacity and battery safety.
Patent Information
- Application Number
- CN202580026700.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-03
- Filing Date
- 2025-03-17
- Publication Date
- 2026-11-10
AI Technical Summary
In all-solid-state batteries, the high porosity of the solid electrolyte layer leads to low ionic conductivity and lithium dendrite growth, which can cause short circuits or deterioration of the battery's rate performance.
Hydrogenated nitrile butadiene rubber (HNBR) is used as a binder. Its nitrile repeating unit content, residual double bond content and Mooney viscosity are controlled. Combined with appropriate solid electrolyte particle size and porous support, the internal porosity of the solid electrolyte sheet is reduced, the ionic conductivity is improved and lithium dendrites are suppressed.
It effectively reduces the internal pores of the solid electrolyte sheet, improves ionic conductivity, suppresses battery short circuits, and enhances rate performance.
Smart Images

Figure CN123076944A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a solid electrolyte sheet and an all-solid-state battery containing the same. Background Technology
[0002] With increasing attention focused on the safety and energy density of high-capacity batteries, all-solid-state batteries have garnered significant attention as the next generation of batteries. These batteries replace the explosive liquid electrolyte with a solid electrolyte and do not use flammable solvents within the battery. Therefore, they completely eliminate the risk of fire or explosion caused by reactions such as the decomposition of traditional electrolytes, thus ensuring battery safety.
[0003] Furthermore, since lithium metal or lithium alloys can be used as the negative electrode material, the gravimetric energy density and volumetric energy density of the battery can be improved. The solid electrolyte used in the all-solid-state battery is typically an inorganic solid electrolyte, and various studies are currently underway on sulfide solid electrolytes with a silver-germanium ore structure and compositions such as Li6PS5Cl for use in the all-solid-state battery.
[0004] To realize the practical application of all-solid-state batteries, it is necessary to manufacture large-area batteries. For this purpose, the positive electrode, separator, and negative electrode must be sheet-like, just like existing lithium-ion batteries. In particular, the separator in an all-solid-state battery is composed of a solid electrolyte and a binder, and its properties (ionic conductivity, electrochemical stability, and chemical stability) vary depending on the manufacturing method and the solid electrolyte material selected.
[0005] In particular, the solid electrolyte layer used as a separator in all-solid-state batteries prevents the positive and negative electrodes from contacting each other during charging and discharging, suppresses lithium dendrites, and allows lithium ions to move smoothly at a relatively thin thickness in order to maximize the energy density of the battery.
[0006] However, the numerous pores that typically exist between multiple solid electrolyte particles within the solid electrolyte layer can reduce the ionic conductivity of the solid electrolyte layer or induce lithium dendrite growth within the battery, thereby potentially causing short circuits or deterioration of the battery's rate performance. Summary of the Invention
[0007] (a) Technical problems to be solved Therefore, one objective of the present invention is to provide a solid electrolyte sheet with reduced internal porosity and increased ionic conductivity, which, when applied to all-solid-state batteries, can suppress internal short circuits and improve rate performance.
[0008] Another objective of the present invention is to provide an all-solid-state battery comprising the aforementioned solid electrolyte sheet.
[0009] (II) Technical Solution This application claims priority to Korean Patent Application No. 10-2024-0045343, filed on April 4, 2024, the entire contents of which are incorporated herein by reference.
[0010] One embodiment of the present invention provides a solid electrolyte sheet comprising a solid electrolyte and a binder, wherein the binder comprises hydrogenated nitrile butadiene rubber (HNBR), wherein the nitrile repeating unit content of the hydrogenated nitrile butadiene rubber is 19 to 31% by weight and the residual double bond content is less than 4%, and the average particle size (D50) of the solid electrolyte is 1 to 5 μm.
[0011] The residual double bond content of the hydrogenated nitrile rubber can be less than 1.5%.
[0012] The Mooney viscosity (ML) of the hydrogenated nitrile butadiene rubber 1+4 (at 100℃) can be 50 to 95 MU.
[0013] The content of the binder can be from 0.5 to 5% by weight, based on the total weight of the solid electrolyte and the binder.
[0014] The solid electrolyte may be a sulfide solid electrolyte, a halide solid electrolyte, or a combination thereof.
[0015] The sulfide solid electrolyte can have an Argyrodite crystal structure.
[0016] The sulfide solid electrolyte can be represented by the following chemical formula 1.
[0017] [Chemical Formula 1] Li x1 P y1 S z1 D w1 M1 a1 M2 a2 In the above chemical formula 1, D is a halogen element, which is F, Cl, Br, I or a combination thereof; M1 is B, Al, Si, Ga, Ge, In, Sn or a combination thereof; M2 is O, N, As, Se, Sb, Te or a combination thereof; 4≤x1≤8, 0.5≤y1≤1.5, 3≤z1≤7, 0≤a1≤2, 0≤a2≤2.
[0018] The halide solid electrolyte can be represented by the following chemical formula 2.
[0019] [Chemical Formula 2] Li x2 M3 y2 Az2 In the above chemical formula 2, M3 is Sc, In, Zr, Lu, Er, Y, Ho or a combination thereof, A is a halogen element, which is F, Cl, Br, I or a combination thereof, and 1.5≤x2≤3.5, 0.5≤y2≤1.5, 5≤z2≤7.
[0020] The average number of pinholes in the solid electrolyte sheet can be 10 per 25cm. 2 the following.
[0021] The solid electrolyte sheet has an ionic conductivity of 0.85 mS / cm or higher at 30°C.
[0022] The solid electrolyte sheet may also include a porous support.
[0023] The porous support may comprise a polymer resin composed of polyethylene terephthalate (PET), polypropylene (PP), polyethylene (PE), polycarbonate (PC), polyvinylidene fluoride (PVDF), Teflon (PTFE), or a combination thereof.
[0024] Another embodiment of the present invention provides an all-solid-state battery comprising a positive electrode layer; a negative electrode layer; and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer and comprising the aforementioned solid electrolyte sheet.
[0025] (III) Beneficial Effects One embodiment of the present invention provides a solid electrolyte sheet that effectively reduces internal pores within the solid electrolyte sheet by incorporating a hydrogenated nitrile butadiene rubber (HNBR) binder with a controlled structure.
[0026] This improves the ionic conductivity of the solid electrolyte sheet and, when applied to all-solid-state batteries, suppresses internal short circuits caused by lithium dendrites and improves rate performance. Attached Figure Description
[0027] Figure 1 Pinhole analysis images of the solid electrolyte sheet manufactured according to Example 1.
[0028] Figure 2 Pinhole analysis images of the solid electrolyte sheet manufactured according to Example 4.
[0029] Figure 3 Pinhole analysis image of the solid electrolyte sheet manufactured according to Comparative Example 2.
[0030] Figure 4 Pinhole analysis image of the solid electrolyte sheet manufactured according to Comparative Example 9. Detailed Implementation
[0031] The terms first, second, and third are used to describe various parts, components, regions, layers, and / or segments, but are not limited thereto. These terms are used only to distinguish one part, component, region, layer, or segment from another. Therefore, without departing from the scope of the invention, the first part, component, region, layer, or segment described below may also be referred to as the second part, component, region, layer, or segment.
[0032] The technical terms used herein are for reference only in specific embodiments and are not intended to limit the invention. Unless the context clearly indicates otherwise, the singular forms used herein include the plural forms as well. The word "comprising" as used herein is used to specify a particular feature, region, integer, step, operation, element, and / or component, and does not exclude the presence or addition of other features, regions, integers, steps, operations, elements, and / or components.
[0033] When a part is described as being "above" or "on top of" another part, it can be located directly above or above the other part, or there can be other parts between the two. Conversely, when a part is described as being "directly above" another part, there are no other parts between the two.
[0034] Unless otherwise defined, all terms used herein, including technical and scientific terms, shall have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. Terms defined in common dictionaries shall be further interpreted as having meanings consistent with relevant technical literature and the content of this disclosure, and shall not be interpreted as having idealized or overly formal meanings unless otherwise defined.
[0035] In addition, unless otherwise stated, % means weight%, and 1 ppm is 0.0001 wt%.
[0036] In this specification, "the combination thereof" in the Markush form means a mixture or combination of one or more selected from the group consisting of the constituent elements listed in the Markush form, that is, including at least one selected from the group consisting of the constituent elements.
[0037] The embodiments of the present invention will now be described in detail to enable those skilled in the art to readily implement the invention. However, the present invention can be implemented in various different forms and is not limited to the embodiments described herein.
[0038] 1. Solid electrolyte tablets The solid electrolyte sheet of one embodiment of the present invention can be applied to the solid electrolyte layer in an all-solid-state battery.
[0039] More specifically, the solid electrolyte sheet of one embodiment of the present invention comprises a solid electrolyte and a binder.
[0040] At this point, the adhesive contains hydrogenated nitrile butadiene rubber (HNBR).
[0041] Nitrile butadiene rubber (NBR), traditionally used as a binder, contains double bonds in its carbon chains. These double bonds are highly reactive with sulfide solid electrolytes commonly used in solid electrolytes, and the reaction can lead to curing, potentially increasing the interfacial resistance between solid electrolyte particles. Furthermore, the volume expansion of the sulfide solid electrolyte can cause cracks in the solid electrolyte layer.
[0042] Conversely, in the adhesive of the present invention, a large number of double bonds within the carbon chain are removed during the hydrogenation of nitrile rubber (NBR). Therefore, the aforementioned problems can be prevented.
[0043] Furthermore, the inventors have confirmed that by further controlling the degree of hydrogenation of hydrogenated nitrile butadiene rubber (HNBR) (characterized by the content of residual double bonds), the content of nitrile repeating units, Mooney viscosity, etc., the internal porosity within the solid electrolyte sheet can be effectively reduced. It was also discovered that reducing the internal porosity within the solid electrolyte sheet can improve the electrical connectivity between the solid electrolyte particle interfaces, increase the ionic conductivity of the solid electrolyte sheet, and suppress short circuits when applied to all-solid-state batteries, thereby improving high-rate discharge capacity (i.e., rate performance). This completes the present invention.
[0044] To date, studies have only investigated the relationship between controlling the content of repeating nitrile units in hydrogenated nitrile rubber and inhibiting its reaction with solid electrolytes. In contrast, this invention focuses on reducing internal porosity within the solid electrolyte sheet (solid electrolyte layer) by controlling the properties of hydrogenated nitrile rubber, which will be described in detail below.
[0045] The adhesive of the present invention comprises hydrogenated nitrile butadiene rubber (HNBR), which, in addition to controlling the content of nitrile repeating units and residual double bonds, can further control Mooney viscosity.
[0046] First, the hydrogenated nitrile butadiene rubber (HNBR) has a nitrile repeating unit content of 19 to 31% by weight, more specifically 19 to 26% by weight. When the nitrile repeating unit content meets the above range, an appropriate amount of acrylonitrile is present in the polymer structure, thereby increasing the relative density, accelerating the curing speed, and improving the tensile strength, effectively reducing the internal porosity within the solid electrolyte sheet (or solid electrolyte layer when applied to all-solid-state batteries). This improves the ionic conductivity of the solid electrolyte sheet and, when applied to all-solid-state batteries, suppresses battery short circuits and enhances high-rate discharge capacity (i.e., rate characteristics).
[0047] The nitrile repeating unit content is expressed as a percentage by weight (%) based on the total weight of the hydrogenated nitrile butadiene rubber polymer. Furthermore, the nitrile repeating unit content can be measured and calculated using Fourier transform infrared spectroscopy and the Dumas method, specifically according to ISO 24698-1.
[0048] Furthermore, the residual double bond content of the hydrogenated nitrile butadiene rubber (HNBR) is less than 4%, and more specifically, it can be less than 1.5% or less than 1.0%.
[0049] "Residual double bond content" refers to the amount of double bonds remaining in the carbon chain of hydrogenated nitrile butadiene rubber (HNBR). The residual double bond content is expressed as a percentage (%), which is the percentage of the number of repeating units in HNBR whose double bonds have not been removed, divided by the sum of the CC and C=C repeating units in HNBR. In other words, the residual double bond content can be expressed by the following equation (1).
[0050] [Relation 1] Residual Double Bonding Content (%) = [C=C] / ([C=C] + [CC]) 100 The "residual double bond content" can be measured using infrared spectroscopy.
[0051] Specifically, as the degree of hydrogenation of nitrile rubber increases, the amount of residual double bonds within the carbon chain can be reduced. When the residual double bond content meets the aforementioned range, the amount of unsaturated double bonds in the NBR polymer bonding structure can be reduced, improving the bonding strength between polymers. That is, as the bonding strength between polymers binding solid electrolyte particles increases, the internal porosity within the solid electrolyte sheet (or solid electrolyte layer when applied to all-solid-state batteries) can be effectively reduced. This improves the ionic conductivity of the solid electrolyte sheet and, when applied to all-solid-state batteries, suppresses battery short circuits, enhancing high-rate discharge capacity (i.e., rate performance).
[0052] Furthermore, the Mooney viscosity (ML) of the hydrogenated nitrile butadiene rubber (HNBR) 1+4 (at 100℃) can be 50 to 95 MU, more specifically, it can be 60 to 90 MU.
[0053] Mooney viscosity (ML) 1+4 "(100℃)" can be obtained by measuring the hydrogenated nitrile butadiene rubber polymer at 100℃ according to ISO 289 / ASTM D 1646.
[0054] The Mooney viscosity of hydrogenated nitrile butadiene rubber (NBR) is related to the polymer molecular weight; as the polymer molecular weight increases, the Mooney viscosity can also increase. If the Mooney viscosity of NBR is too low, the bonding strength between polymers weakens, potentially reducing the internal porosity within the solid electrolyte sheet. Conversely, if the Mooney viscosity is too high, the bonding strength between polymers becomes too strong, causing agglomeration of solid electrolyte particles, which may also reduce the internal porosity within the solid electrolyte sheet. Therefore, when the Mooney viscosity of NBR meets the above-mentioned range, it can effectively reduce the internal porosity within the solid electrolyte sheet (or solid electrolyte layer in all-solid-state batteries). This improves the ionic conductivity of the solid electrolyte sheet and, when applied to all-solid-state batteries, can suppress battery short circuits and improve high-rate discharge capacity (i.e., rate performance).
[0055] The composition of the hydrogenated nitrile butadiene rubber (HNBR) of the present invention will be described in more detail below.
[0056] The hydrogenated nitrile butadiene rubber (HNBR) of the present invention may contain repeating units of nitrile monomers, repeating units of aliphatic conjugated diene monomers, and other repeating units.
[0057] [Repeating unit containing nitrile monomers] Nitrile-containing monomers capable of forming repeating units can include α,β-ene unsaturated nitrile monomers. Specifically, there are no particular limitations on α,β-ene unsaturated nitrile monomers, as long as they are α,β-ene unsaturated compounds with a nitrile group. Examples include acrylonitrile; α-haloacrylonitrile such as α-chloroacrylonitrile and α-bromoacrylonitrile; and α-alkylacrylonitrile such as methacrylonitrile and α-ethylacrylonitrile. Among these, acrylonitrile and methacrylonitrile are preferred from the perspective of further improving the output characteristics and high-temperature cycling characteristics of all-solid-state secondary batteries, and acrylonitrile is more preferred. On the other hand, a single nitrile-containing monomer can be used, or two or more can be combined in any proportion.
[0058] [Aliphatic conjugated diene monomer repeating unit] There are no particular limitations on the aliphatic conjugated diene monomers capable of forming repeating units; examples include 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), and 2,3-dimethyl-1,3-butadiene. Among these, 1,3-butadiene is preferred from the perspective of ensuring sufficient flexibility of the solid electrolyte layer while further improving the output characteristics and high-temperature cycling characteristics of the all-solid-state secondary battery. Furthermore, aliphatic conjugated diene monomers can be used alone or in combination of two or more in any proportion.
[0059] [Other repeating units] There are no particular restrictions on other repeating units as long as they are derived from repeating units of monomers that can copolymerize with the aforementioned nitrile-containing monomers and aliphatic conjugated diene monomers. For example, olefinic unsaturated carboxylic acid ester monomer units can be listed.
[0060] The olefinic unsaturated carboxylic acid ester monomers capable of forming olefinic unsaturated carboxylic acid ester monomer units can be, for example, monomers composed of esters of olefinic unsaturated monocarboxylic acids or monomers composed of diesters of olefinic unsaturated dicarboxylic acids.
[0061] Here, monomers composed of esters of olefinically unsaturated monocarboxylic acids can be exemplified by (meth)acrylate monomers. On the other hand, in this invention, "(meth)propylene" refers to propylene and / or methpropylene.
[0062] In addition, (meth)acrylate monomers can include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, tert-butyl acrylate, isobutyl acrylate, n-pentyl acrylate, isopentyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, decyl acrylate, lauryl acrylate, n-tetradecyl acrylate, stearyl acrylate, and other alkyl acrylates; methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, isopentyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, nonyl methacrylate, decyl methacrylate, lauryl methacrylate, n-tetradecyl methacrylate, stearyl methacrylate, glycidyl methacrylate, and other alkyl methacrylates.
[0063] In addition, monomers composed of diesters of olefinic unsaturated dicarboxylic acids can include dialkyl maleate esters such as diethyl maleate and dibutyl maleate; dialkyl fumarate esters such as diethyl fumarate and dibutyl fumarate; and dialkyl itaconic acid esters such as diethyl itaconic acid esters and dibutyl itaconic acid esters.
[0064] From the perspective of further improving the output characteristics and high-temperature cycling characteristics of all-solid-state secondary batteries, methyl acrylate, ethyl acrylate, methyl methacrylate, n-butyl acrylate, and dibutyl itaconic acid are preferred. On the other hand, olefinic unsaturated carboxylic acid ester monomers can be used alone, or two or more can be combined in any proportion.
[0065] [Manufacturing method of hydrogenated nitrile butadiene rubber] There are no particular limitations on the manufacturing method of hydrogenated nitrile butadiene rubber. For example, hydrogenated nitrile butadiene rubber can be manufactured by polymerizing a monomer composition containing the above-mentioned monomers in an aqueous solvent. On the other hand, the content ratio of each monomer in the monomer composition can be determined according to the content ratio of the desired monomer units (repeating units) in the polymer.
[0066] On the other hand, there are no particular restrictions on the polymerization method; any method from solution polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc., can be used. Furthermore, the polymerization reaction can be any type of reaction, such as ionic polymerization, free radical polymerization, living free radical polymerization, various condensation polymerizations, addition polymerization, etc. Additionally, known emulsifiers or polymerization initiators can be used during polymerization as needed.
[0067] Furthermore, the average particle size (D50) of the solid electrolyte of the present invention is 1 to 5 μm, more specifically, it can be 1.5 to 4.5 μm or 2 to 4 μm. If the average particle size (D50) of the solid electrolyte is too small, there may be problems with reduced ionic conductivity and high-rate discharge capacity. If the average particle size (D50) of the solid electrolyte is too large, the surface quality of the solid electrolyte sheet is uneven, and pores are generated between the solid electrolyte particles, which may lead to battery short circuits. Moreover, when the average particle size (D50) of the solid electrolyte meets the above-mentioned range, it has good compatibility with the HNBR binder of the present invention, and can effectively reduce the internal pores within the solid electrolyte sheet (or solid electrolyte layer when applied to all-solid-state batteries).
[0068] In this specification, the average particle size (D50) can be defined as the particle size corresponding to 50% of the cumulative volume on the particle size distribution curve. The average particle size (D50) can be measured, for example, using a laser diffraction method.
[0069] On the other hand, based on the total weight of the solid electrolyte and the binder, the binder content of the present invention can be 0.5 to 5% by weight, more specifically, 0.5 to 3% by weight. If the binder content is too low, the solid electrolyte particles cannot be sufficiently bonded (combined), and the effect of reducing the internal porosity of the solid electrolyte sheet may be weakened. If the binder content is too high, the solid electrolyte particles will aggregate too strongly, which may actually increase the internal porosity of the solid electrolyte sheet.
[0070] The solid electrolyte may be a sulfide solid electrolyte, a halide solid electrolyte, or a combination thereof.
[0071] For example, the sulfide solid electrolyte can be selected from Li2S-P2S5, Li2S-P2S5-LiX (where X is a halogen element), Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-ZmSn (where m and n are positive numbers, and Z is one of Ge, Zn, or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q (Where p and q are positive numbers, and M is one of P, Si, Ge, B, Al, Ga, and In), Li3PS4, Li7P3S 11 Li 7-x PS6-x Cl x (where 0≤x≤2), Li 7-x PS 6-x Br x (where 0 ≤ x ≤ 2) and Li 7-x PS 6-x I x One or more of the following (where 0 ≤ x ≤ 2).
[0072] For example, the sulfide solid electrolyte can be prepared by treating starting materials such as Li₂S and P₂S₅ using methods such as melt quenching or mechanical milling. Furthermore, heat treatment can be performed after such treatment. The solid electrolyte can be amorphous, crystalline, or a mixture thereof. Additionally, the solid electrolyte can be, for example, a material containing at least sulfur (S), phosphorus (P), and lithium (Li) as constituent elements in the aforementioned sulfide solid electrolyte material. For example, the solid electrolyte can be a material containing Li₂S-P₂S₅.
[0073] From the perspective of better achieving ionic conductivity, the sulfide solid electrolyte can have an Argyrodite crystal structure.
[0074] Sulfide solid electrolytes with a germanium argyrite crystal structure may contain elements such as Li, P, S, and halogens, and may further contain other doping elements as needed. By further incorporating other doping elements into the germanium argyrite crystal structure, the water stability of the solid electrolyte can be improved, or electrochemical properties such as battery capacity can be better achieved.
[0075] For example, the sulfide solid electrolyte can be represented by the following chemical formula 1.
[0076] [Chemical Formula 1] Li x1 P y1 S z1 D w1 M1 a1 M2 a2 In the above chemical formula 1, D is a halogen element, which is F, Cl, Br, I or a combination thereof; M1 is B, Al, Si, Ga, Ge, In, Sn or a combination thereof; M2 is O, N, As, Se, Sb, Te or a combination thereof; 4≤x1≤8, 0.5≤y1≤1.5, 3≤z1≤7, 0≤a1≤2, 0≤a2≤2.
[0077] Furthermore, the halide solid electrolyte can be represented by the following chemical formula 2.
[0078] [Chemical Formula 2] Lix2 M3 y2 A z2 In the above chemical formula 2, M3 is Sc, In, Zr, Lu, Er, Y, Ho or a combination thereof, A is a halogen element, which is F, Cl, Br, I or a combination thereof, and 1.5≤x2≤3.5, 0.5≤y2≤1.5, 5≤z2≤7.
[0079] On the other hand, the solid electrolyte sheet of the present invention effectively reduces internal porosity due to the above-described structure, and its average number of pinholes can be 10 per 25 cm. 2 More specifically, it can be 5 per 25cm. 2 Below or 2.5 pieces / 25cm 2 The following describes how LEDs (light-emitting diodes) can be placed on the back of the solid electrolyte sheet, spaced at 5×5cm intervals. 2 Count the number of light spots emitted through pinholes in the solid electrolyte sheet per unit area, and calculate the number of any 10 5×5cm pinholes within the solid electrolyte sheet. 2 The average number of pinholes per unit area is used to measure the average number of pinholes on a solid electrolyte sheet.
[0080] Furthermore, the solid electrolyte sheet of the present invention improves ionic conductivity by reducing internal pores, and its ionic conductivity at 30°C can be 0.85 mS / cm or higher, more specifically, 1.05 mS / cm or higher.
[0081] The solid electrolyte sheet may further include a porous support. By further including a porous support in the solid electrolyte sheet, its mechanical rigidity can be significantly improved, enabling it to function as a self-supporting membrane.
[0082] For example, the porous support may comprise a polymer resin composed of polyethylene terephthalate (PET), polypropylene (PP), polyethylene (PE), polycarbonate (PC), polyvinylidene fluoride (PVDF), Teflon (PTFE), or a combination thereof, but is not necessarily limited thereto.
[0083] 2. Manufacturing method of solid electrolyte sheets The solid electrolyte sheet of the present invention can be manufactured according to the following manufacturing method, which will be described below.
[0084] First, a solid electrolyte composition is formed.
[0085] The solid electrolyte composition may contain a solvent together with the solid electrolyte and binder of the present invention described above. The solid electrolyte and binder have been described in detail above, therefore related descriptions are omitted.
[0086] For example, the solvent may be xylene, toluene, isobutyl isobutyrate or a combination thereof, but is not necessarily limited to these, as long as it is a solvent used in the art.
[0087] The solid electrolyte composition may also contain a dispersant capable of improving the dispersibility of the solid components within the solid electrolyte composition, and may further contain other additives as needed.
[0088] Next, the solid electrolyte composition is coated onto a substrate or porous support.
[0089] The substrate is not particularly limited as long as it has chemical stability relative to the solid electrolyte composition. For example, the substrate can be PET (polyethylene terephthalate), PEN (polyethylene naphthalate), PES (polyethersulfone), PC (polycarbonate), PP (polypropylene), or a combination thereof, but is not necessarily limited to these.
[0090] For example, the porous support may comprise a polymer resin composed of polyethylene terephthalate (PET), polypropylene (PP), polyethylene (PE), polycarbonate (PC), polyvinylidene fluoride (PVDF), Teflon (PTFE), or a combination thereof, but is not necessarily limited thereto.
[0091] The coating is not particularly limited as long as it is done using methods commonly used in the art; for example, it can be done by casting a slurry.
[0092] Next, the solid electrolyte composition coated on the substrate or porous support is dried to remove the solvent in the solid electrolyte composition, thereby forming a solid electrolyte sheet.
[0093] For example, the drying can be carried out at a temperature of about 20 to 60°C.
[0094] 3. All-solid-state batteries Another embodiment of the present invention provides an all-solid-state battery comprising a positive electrode layer; a negative electrode layer; and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer and comprising the aforementioned solid electrolyte sheet.
[0095] More specifically, the positive electrode layer may include a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector.
[0096] For example, the positive electrode active material layer may comprise a positive electrode active material and a solid electrolyte. The solid electrolyte comprised in the positive electrode active material layer may be the same as or different from the solid electrolyte comprised in the solid electrolyte sheet.
[0097] A cathode active material is a material capable of reversibly absorbing and desorbing lithium ions. Examples of cathode active materials include lithium transition metal oxides such as lithium cobalt oxide (LCO), lithium nickel oxide, lithium nickel cobalt oxide, lithium nickel aluminum cobalt oxide (NCA), lithium nickel manganese cobalt oxide (NCM), lithium manganate, and lithium iron phosphate; nickel sulfide, copper sulfide, lithium sulfide, iron oxide, and vanadium oxide; but these are not necessarily limited to these materials; any material used as a cathode active material in this field is acceptable. Cathode active materials can be used alone or in mixtures of two or more.
[0098] The lithium transition metal oxide is, for example, a compound represented by any of the following chemical formulas: Li a A 1-b B b D2 (where 0.90≤a≤1, 0≤b≤0.5); Li a E 1-b B b O 2-c D c (In the formula, 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05); LiE 2-b B b O 4-c D c (In the formula, 0≤b≤0.5, 0≤c≤0.05); Li a Ni 1-b-c Co b B c D α (In the formula, 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, 0<α≤2); Li a Ni 1-b-c Co b B c O 2-α F α (In the formula, 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, 0<α<2); Li a Ni 1-b-c Co b B c O 2-α F2 (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, 0<α<2); Li a Ni 1-b-c Mn b B c Dα (In the formula, 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, 0<α≤2); Li a Ni 1-b-c Mn b B c O 2-α F α (In the formula, 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, 0<α<2); Li a Ni 1-b-c Mn b B c O 2-α F2 (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, 0<α<2); Li a Ni b E c G d O2 (where 0.90≤a≤1, 0≤b≤0.9, 0≤c≤0.5, 0.001≤d≤0.1); Li a Ni b Co c Mn d G e O2 (where 0.90≤a≤1, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, 0.001≤e≤0.1); Li a NiG b O2 (where 0.90≤a≤1, 0.001≤b≤0.1); Li a CoG b O2 (where 0.90≤a≤1, 0.001≤b≤0.1); Li a MnG b O2 (where 0.90≤a≤1, 0.001≤b≤0.1); Li a Mn2G b O4 (in the formula, 0.90≤a≤1, 0.001≤b≤0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3 (0≤f≤2); Li (3-f)Fe2(PO4)3 (0≤f≤2); LiFePO4. In these compounds, A is Ni, Co, Mn, or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof. Compounds with an additional coating can also be used on the surface of these compounds, and mixtures of the above compounds with the additional coating compound can be used. The coating applied to the surface of these compounds may include, for example, oxides, hydroxides, hydroxy oxides, carbonate oxides, or hydroxycarbonates of the coating element. The compound constituting such a coating may be amorphous or crystalline. The coating contains Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or mixtures thereof. The coating formation method is selected within a range that does not adversely affect the properties of the positive electrode active material. For example, the coating method may be spraying, dipping, etc. Specific coating methods are readily understood by those skilled in the art, therefore detailed descriptions are omitted.
[0099] For example, the positive electrode active material layer can contain a solid electrolyte. The solid electrolyte contained in the positive electrode layer can be the same as or different from the solid electrolyte contained in the solid electrolyte layer.
[0100] For example, the positive electrode active material layer may include a binder. Binders may be, for example, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, etc., but are not limited to these; any material used as a binder in the art is acceptable.
[0101] For example, the positive electrode active material layer may contain a conductive material. Conductive materials include, but are not limited to, graphite, carbon black, acetylene black, Ketjen black, carbon fiber, metal powder, etc., as well as any material used as a conductive material in the art.
[0102] For example, in addition to the above-mentioned positive electrode active material, solid electrolyte, binder and conductive material, the positive electrode active material layer may also contain additives such as filler, coating agent, dispersant, ion conduction aid.
[0103] The positive electrode active material layer may include fillers, coatings, dispersants, ion conduction aids, etc., which can be made of known materials commonly used in all-solid-state secondary battery electrodes.
[0104] The positive electrode current collector can be, for example, a plate or foil made of indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or their alloys. The thickness of the positive electrode current collector can be, for example, 1 to 100 μm, 1 to 50 μm, 5 to 25 μm, or 10 to 20 μm.
[0105] More specifically, the negative electrode layer may include a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector.
[0106] For example, the negative electrode active material layer may include a negative electrode active material and a binder.
[0107] For example, the negative electrode active material may include carbon-based negative electrode active materials, metal / metal-like negative electrode active materials, or combinations thereof.
[0108] The carbon-based negative electrode active material can be amorphous carbon. Examples of amorphous carbon include carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), and graphene, but it is not necessarily limited to these; any material classified as amorphous carbon in this field is acceptable. Amorphous carbon is carbon that is non-crystalline or has extremely low crystallinity, distinguishing it from crystalline carbon or graphitic carbon.
[0109] The metal / metal-like anode active material comprises one or more of the group consisting of lithium (Li), gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn), but is not necessarily limited thereto. Any material in the art that can form an alloy or compound with lithium is acceptable as a metal anode active material or a metal-like anode active material.
[0110] The binder included in the negative electrode active material layer may be, for example, styrene-butadiene rubber (SBR), polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyethylene, PVDF / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, etc., but is not necessarily limited to these; any material used as a binder in this field may be used. The binder may consist of a single binder or multiple different binders.
[0111] By including a binder in the negative electrode active material layer, the negative electrode active material layer can be stabilized on the negative electrode current collector. Furthermore, even though the volume and / or relative position of the negative electrode active material layer changes during charging and discharging, cracking of the negative electrode active material layer can be suppressed.
[0112] The negative electrode active material layer may also contain additives used in existing all-solid-state batteries, such as fillers, coatings, dispersants, ion conduction aids, etc.
[0113] The all-solid-state battery may further include a second negative electrode active material layer disposed between the negative electrode current collector and the negative electrode active material layer during charging. The second negative electrode active material layer may be a layer precipitated between the negative electrode current collectors during charging, or a layer further disposed on the negative electrode active material layer during electrode assembly. The second negative electrode active material layer may be a metal layer containing lithium or a lithium alloy. The lithium alloy may be, for example, Li-Al alloy, Li-Sn alloy, Li-In alloy, Li-Ag alloy, Li-Au alloy, Li-Zn alloy, Li-Ge alloy, Li-Si alloy, etc., but is not limited to these; any material used as a lithium alloy in the art is acceptable. The second negative electrode active material layer may be composed of one of these alloys and / or lithium, or may be composed of multiple alloys and / or lithium.
[0114] The negative electrode current collector can be made of a material that does not react with lithium, i.e., it neither forms an alloy nor a compound. Examples of materials that can be used as electrode current collectors in this field include copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), and nickel (Ni), but are not necessarily limited to these; any material suitable for use as an electrode current collector in this field is acceptable. The negative electrode current collector can be composed of one of the aforementioned metals, or an alloy or coating material of two or more metals. The negative electrode current collector can be in the form of a plate or a foil.
[0115] The embodiments of the present invention will be described in more detail below through examples. However, the following examples are merely preferred embodiments of the present invention, and the present invention is not limited to the following examples.
[0116] Example 1 (1) Preparation of 3μm Li6PS5Cl Argyrodite solid electrolyte Li6PS5Cl was synthesized via a dry process. Specifically, Li2S, P2S5, and LiCl were weighed according to the composition, mixed at 300 rpm for 8 hours using a planetary mill, then pressed into tablets at 300 MPa and heat-treated at 550 °C under an argon (Ar) atmosphere to synthesize the Li6PS5Cl silver germanium ore solid electrolyte. Subsequently, the synthesized solid electrolyte was ball-milled to achieve an average particle size (D50) of 3 μm.
[0117] (2) Manufacturing of solid electrolyte sheets The prepared solid electrolyte was mixed with xylene solvent containing 2 wt% HNBR binder to form a solid electrolyte composition (slurry). At this point, based on the total weight of the solid electrolyte and HNBR binder, the content of HNBR binder was 2 wt%. Furthermore, the HNBR binder had a nitrile repeating unit content of 21 wt%, a residual double bond content of 0.9%, and a Mooney viscosity (ML). 1+4 The value at 100℃ is 39 MU.
[0118] Subsequently, the solid electrolyte composition (slurry) is coated onto a PET (polyethylene terephthalate) substrate using a doctor blade coating method.
[0119] Subsequently, the coated solid electrolyte composition (slurry) is dried at 50°C and then peeled off from the PET substrate to obtain a solid electrolyte sheet.
[0120] (3) Manufacturing of all-solid-state batteries The prepared solid electrolyte sheet was punched into 0.785 cm pieces. 2 The area was filled into a powder-pressed battery, and then a composite electrode was loaded onto it. A positive electrode slurry was prepared by mixing positive electrode active material (NCM811), solid electrolyte (Li6PS5Cl), and conductive material (denka black) in a weight ratio of 70:29:1, and loaded at a loading of 20.0 mg onto a 0.785 cm² substrate. 2 On the surface area, a composite electrode was fabricated and densified at 300 MPa. Subsequently, an In-Li counter electrode was used as the negative electrode, bonded at 50 MPa, and the cell was secured under the same pressure.
[0121] Other embodiments and comparative examples Except for the preparation by changing the content of nitrile repeating units, residual double bond content and Mooney viscosity of HNBR binder as shown in Table 1, solid electrolyte sheets and all-solid-state batteries were manufactured in the same manner as in Example 1.
[0122] Table 1 below summarizes the physical properties of the HNBR binder used in the examples and comparative examples, the evaluation results of the physical properties of the solid electrolyte sheet obtained according to Experimental Example 1 described below, and the evaluation results of the rate characteristics of the all-solid-state battery obtained according to Experimental Example 2.
[0123] Table 1 Experimental Example 1: Evaluation of the physical properties of solid electrolyte sheets (1) Ionic conductivity For the solid electrolyte sheet manufactured according to the examples and comparative examples, SUS was used as the working electrode, the battery was secured with a pressure of 70 MPa, and a voltage of 10 mV was applied at 30°C to measure the impedance.
[0124] (2) Average number of pinholes and pinhole image analysis LEDs (light-emitting diodes) are placed on the back of the solid electrolyte sheet at intervals of 5×5cm. 2 Count the number of light spots emitted through pinholes in the solid electrolyte sheet per unit area, and calculate the number of any 10 5×5cm pinholes within the solid electrolyte sheet. 2 The average number of pinholes per unit area is used to measure the average number of pinholes in the solid electrolyte sheet manufactured according to the examples and comparative examples.
[0125] Furthermore, the pinholes inside the solid electrolyte sheets manufactured according to Examples 1 and 4 and Comparative Examples 2 and 9 were observed using LED backlighting, and the images were sequentially displayed on [the images are shown in the original text]. Figures 1 to 4 .
[0126] Experimental Example 2: Evaluation of the Rate Characteristics of All-Solid-State Batteries After manufacturing the all-solid-state battery, it was aged at room temperature for 2 hours, followed by initial cycling. Capacity evaluation was based on a baseline capacity of 180 mAh / g, with charge / discharge conditions of CC / CV 2.5 to 4.20 V and a 1 / 20 C cutoff. The first cycle was performed under 0.1 C charge / 0.1 C discharge conditions. The discharge capacity obtained in the second cycle at 1.5 C was then calculated as a percentage of the discharge capacity from the first cycle to evaluate rate performance.
[0127] Reference Figures 1 to 4 It can be confirmed that, even by visual observation, the internal pores of the solid electrolyte sheet in the embodiment are significantly reduced compared to the solid electrolyte sheet in the comparative example.
[0128] More specifically, referring to Table 1, it can be confirmed that in Examples 1 to 5, where the content of nitrile repeating units in the HNBR binder, the content of residual double bonds, the average particle size (D50) of the solid electrolyte, and other physical properties were appropriately controlled, the average number of pinholes in the solid electrolyte sheets was significantly less than in the comparative examples. Therefore, it can be confirmed that the solid electrolyte sheets possess excellent ionic conductivity and excellent rate performance.
[0129] Conversely, it can be confirmed that in Comparative Examples 1 to 9, where the content of nitrile repeating units or residual double bonds in the HNBR binder deviates from the scope of the present invention, the average number of pinholes in the solid electrolyte sheet is greater than in the Examples. Therefore, it can be confirmed that the ionic conductivity of the solid electrolyte sheet is generally degraded compared to the Examples, and a battery short circuit occurs during high-rate discharge.
[0130] On the other hand, comparing Examples 1 and 5 with Examples 2 to 4 confirms that in Examples 2 to 4, where the Mooney viscosity and residual double bond content of the HNBR binder are further and more appropriately controlled within the scope of the present invention, the average number of pinholes in the solid electrolyte sheet is less than in Examples 1 and 5. Therefore, it can be confirmed that the ionic conductivity of the solid electrolyte sheet and the high-rate discharge capacity characteristics of the all-solid-state battery are better achieved.
[0131] The preferred embodiments of the present invention have been described above, but the present invention is not limited thereto. Various modifications can be made within the scope of the claims, the detailed description of the invention and the drawings, and these modifications are of course also within the scope of the present invention.
[0132] Therefore, the essential scope of protection of this invention is defined by the appended claims and their equivalents.
Claims
1. A solid electrolyte sheet comprising a solid electrolyte and a binder, The adhesive contains hydrogenated nitrile butadiene rubber (HNBR). The hydrogenated nitrile butadiene rubber has a nitrile repeating unit content of 19 to 31% by weight and a residual double bond content of less than 4%. The average particle size (D50) of the solid electrolyte is 1 to 5 μm.
2. The solid electrolyte sheet according to claim 1, wherein, in, The residual double bond content of the hydrogenated nitrile rubber is less than 1.5%.
3. The solid electrolyte sheet according to claim 1, wherein, in, The Mooney viscosity (ML) of the hydrogenated nitrile butadiene rubber 1+4 (at 100℃) is 50 to 95 MU.
4. The solid electrolyte sheet according to claim 1, wherein, in, The content of the binder is 0.5 to 5% by weight, based on the total weight of the solid electrolyte and the binder.
5. The solid electrolyte sheet according to claim 1, wherein, in, The solid electrolyte is a sulfide solid electrolyte, a halide solid electrolyte, or a combination thereof.
6. The solid electrolyte sheet according to claim 5, wherein, in, The sulfide solid electrolyte has a silver-germanium ore crystal structure.
7. The solid electrolyte sheet according to claim 5, wherein, in, The sulfide solid electrolyte is represented by the following chemical formula 1: [Chemical Formula 1] The x1 P y1 S z1 D w1 M1 a1 M2 a2 In the above chemical formula 1, D is a halogen element, which is F, Cl, Br, I or a combination thereof; M1 is B, Al, Si, Ga, Ge, In, Sn or a combination thereof; M2 is O, N, As, Se, Sb, Te or a combination thereof; 4≤x1≤8, 0.5≤y1≤1.5, 3≤z1≤7, 0≤a1≤2, 0≤a2≤2.
8. The solid electrolyte sheet according to claim 5, wherein, in, The halide solid electrolyte is represented by the following chemical formula 2: [Chemical Formula 2] Li x2 M3 y2 A z2 In the above chemical formula 2, M3 is Sc, In, Zr, Lu, Er, Y, Ho or a combination thereof, A is a halogen element, which is F, Cl, Br, I or a combination thereof, and 1.5≤x2≤3.5, 0.5≤y2≤1.5, 5≤z2≤7.
9. The solid electrolyte sheet according to claim 1, wherein, in, The solid electrolyte sheet has an average of 10 pinholes per 25cm. 2 the following.
10. The solid electrolyte sheet according to claim 1, wherein, in, The solid electrolyte sheet has an ionic conductivity of ≥0.85 mS / cm at 30°C.
11. The solid electrolyte sheet according to claim 1, wherein, in, The solid electrolyte sheet also includes a porous support.
12. The solid electrolyte sheet according to claim 11, wherein, in, The porous support comprises a polymer resin consisting of polyethylene terephthalate (PET), polypropylene (PP), polyethylene (PE), polycarbonate (PC), polyvinylidene fluoride (PVDF), Teflon (PTFE), or a combination thereof.
13. The solid electrolyte sheet according to claim 1, wherein, in, The solid electrolyte sheet serves as a solid electrolyte layer when applied to all-solid-state batteries.
14. An all-solid-state battery comprising a positive electrode layer; a negative electrode layer; and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer and comprising the solid electrolyte sheet of claim 1.
Citation Information
Patent Citations
Cogeneration systems and methods for generating heating and electricity
KR1020240045343A