A titanium-precious metal composite setting structure, manufacturing process and jewelry

By using selective laser melting technology, prefabricated setting openings and their mechanical locking structures can be simultaneously constructed in titanium alloy jewelry. The mechanical locking connection is achieved by utilizing the local plastic deformation of precious metal inlays. This solves the problems of difficult processing of complex settings and insufficient connection stability in titanium alloy jewelry, realizes the functional zoning and structural synergy of titanium alloy and precious metal, and reduces processing difficulty and connection stability.

CN123100919APending Publication Date: 2026-11-17CHINA UNIV OF GEOSCIENCES (WUHAN)
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202611235393.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The challenges in titanium alloy jewelry include complex settings that are difficult to process, the unsuitability of titanium alloy for direct molding and setting of gemstones, and insufficient stability in the connection between precious metal settings and the titanium alloy body.

Method used

Selective laser melting is used to simultaneously construct pre-made inlay openings and their mechanical locking structures during the titanium substrate forming process. Precious metal inlays are then embedded into the pre-made inlay openings, and mechanical locking connections are formed through local plastic deformation. The precious metal inlays support and hold the gemstones in place.

Benefits of technology

It significantly reduces the processing difficulty of complex setting in titanium substrates, improves the connection stability between precious metal inlays and titanium substrates, avoids the operational difficulty of direct plastic pressing of titanium alloys, achieves functional zoning and structural synergy, reduces the amount of precious metal used, and maintains the process reliability of the gemstone setting area.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123100919A_ABST
    Figure CN123100919A_ABST
Patent Text Reader

Abstract

This invention relates to the field of assembly technology, specifically to a titanium-precious metal composite setting structure, manufacturing process, and jewelry, to solve the problems of complex settings being difficult to process in titanium alloy jewelry and the unsuitability of titanium alloys for direct plastic pressing of gemstones. Structurally, it includes a titanium base with a pre-fabricated setting, a precious metal inlay embedded within the pre-fabricated setting, and a gemstone supported and held in place by the inner setting area of ​​the precious metal inlay. This invention constructs a pre-fabricated setting and mechanical locking structure during the titanium base forming process, embeds the precious metal inlay into the pre-fabricated setting, and through local plasticity forms a stable mechanical locking connection between it and the mechanical locking structure. The precious metal inlay holds and fixes the gemstone, creating a structure where the titanium base does not directly contact the gemstone. This achieves a synergistic effect of structural support and lightweighting of the titanium base, the plastic setting function of the precious metal inlay, and the stable fixing function of the gemstone.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of gemstone assembly technology, specifically to a titanium-precious metal composite setting structure, its manufacturing process, and related jewelry. Background Technology

[0002] Titanium and titanium alloys possess characteristics such as low density, high specific strength, good corrosion resistance, good biocompatibility, and the ability to obtain a wide range of surface colors through anodizing. In recent years, they have been increasingly used in the manufacture of high-end jewelry, personalized jewelry, modular jewelry, and art crafts. Compared with traditional precious metals such as gold, karat gold, silver, and platinum, titanium alloys can achieve higher structural strength at a lower weight, making them suitable for fabricating large-volume, complex, and lightweight jewelry structures.

[0003] However, titanium alloys are also typical difficult-to-machine materials. Existing research indicates that titanium alloys exhibit low thermal conductivity, high high-temperature chemical reactivity, low elastic modulus, and high high-temperature strength during machining, easily leading to problems such as concentrated cutting heat, accelerated tool wear, work hardening, decreased surface integrity, and difficulty in controlling dimensional accuracy. For the settings in jewelry, the machining targets are usually not simple through holes or ordinary grooves, but rather complex microstructures such as steps, undercuts, dovetail grooves, annular locking grooves, micro-grooves, and positioning holes within a relatively small area. Therefore, using traditional CNC machining, micro-milling, drilling, engraving, or manual finishing methods to machine complex settings for precious metal inlays on titanium alloy bodies is not only inefficient but also suffers from high tool wear, numerous micro-structural burrs, difficulty in forming concave structures, poor dimensional consistency, and high difficulty in subsequent finishing.

[0004] Traditional gem-setting techniques typically rely on the localized plastic deformation of precious metal materials to secure the gemstone. Techniques such as prong setting, bezel setting, pave setting, channel setting, and micro-pave setting usually require the prongs, bezels, or beading prongs to undergo controlled plastic deformation under external force, thus stably holding the gemstone's girdle or edge. Precious metals such as gold, karat gold, silver, and platinum have good ductility and adjustability, making them suitable for these setting operations. In contrast, titanium alloys have higher hardness and more pronounced elastic recovery. Furthermore, their small local structures are prone to insufficient deformation, localized cracking, concentrated stress on the gemstone, and difficulties in later repairs during bending, beading, or repeated adjustments. Therefore, directly forming small prongs or beading structures on the titanium alloy body to directly hold the gemstone makes it difficult to simultaneously achieve setting stability, ease of processing, and ease of repair.

[0005] Selective laser melting (SLM) is an important method in metal powder bed fusion additive manufacturing, capable of directly fabricating complex metal components based on 3D models and layer-by-layer forming principles. Existing additive manufacturing research indicates that metal additive manufacturing is particularly suitable for fabricating complex geometries that are difficult to achieve with traditional subtractive processing, and can achieve near-net-shape forming of various metal materials such as titanium alloys, stainless steel, aluminum alloys, and nickel-based alloys. In the jewelry manufacturing field, direct metal laser sintering or selective laser melting technologies have been used in the forming research of gold, silver, titanium, and stainless steel rings, demonstrating the feasibility of metal powder bed fusion technology in jewelry manufacturing. However, current research and applications focus more on the integrated forming of the jewelry body, complex shapes, or direct printing of precious metals. For the complex structure problem of "how to reliably support precious metal inlays on a complex titanium alloy body, and further complete the gemstone setting with precious metal inlays," there is still a lack of targeted structural design and fabrication methods.

[0006] Among existing patent technologies, CN111202320A discloses a method for seamless titanium inlay; CN104259459A discloses a method for preparing titanium alloy handicrafts using selective laser melting technology; CN103653576A discloses a shape memory alloy gemstone holder with slotted gemstones; and CN101991251A discloses a dovetail micro-inlay process. These solutions respectively involve titanium gemstone inlay, additive manufacturing of titanium alloy handicrafts, fixing gemstones in alloy gemstone holders, and traditional jewelry dovetail micro-inlay. However, these solutions do not adequately address the following issues: First, how to utilize selective laser melting technology to simultaneously construct complex mechanical locking settings for mounting precious metal inlays during the titanium alloy body forming process; second, how to avoid subsequent machining of difficult-to-machine structures such as micro-undercuts, dovetail grooves, and annular locking grooves on the titanium alloy body; third, how to enable the titanium alloy body to bear the structural support and complex shaping functions, while the malleable precious metal inlays bear the gemstone holding function; and fourth, how to improve the pull-out resistance, rotation resistance, and loosening resistance between the precious metal inlays and the titanium alloy body.

[0007] Therefore, in response to the problems of complex settings in titanium alloy jewelry, the unsuitability of titanium alloy for direct plastic pressing of gemstones, and the insufficient stability of the connection between precious metal inlays and the titanium alloy body, it is necessary to propose a titanium alloy-precious metal composite setting structure and its preparation method. Summary of the Invention

[0008] Based on the above description, the present invention provides a titanium-precious metal composite setting structure, manufacturing process and jewelry, to solve the problems of complex setting difficulties in titanium alloy jewelry, the unsuitability of titanium alloy for direct plastic pressing of gemstones, and insufficient connection stability between precious metal inlays and the titanium alloy body.

[0009] The technical solution of the present invention to solve the above-mentioned technical problems is as follows: In a first aspect, the present invention provides a titanium-noble metal composite inlay structure, comprising: A titanium substrate has a pre-fabricated inlay opening, the inner wall of which is provided with a mechanical locking structure. The pre-fabricated inlay opening and the mechanical locking structure are integrally formed with the titanium substrate by selective laser melting process. A precious metal inlay is set in the pre-made setting opening, having an outer connecting area facing the titanium substrate and an inner setting area facing the gemstone; the outer connecting area forms a mechanical locking connection with the mechanical locking structure through local plastic deformation to restrict the axial pull-out, circumferential rotation and radial loosening of the precious metal inlay relative to the titanium substrate; The gemstone is supported and held in place by the inner setting area of ​​the precious metal inlay, and the titanium base does not directly contact or press the gemstone.

[0010] Based on the above technical solution, the present invention can be further improved as follows.

[0011] Furthermore, the mechanical locking structure includes one or more combinations of the following structures: An undercut groove, dovetail groove, or annular groove is provided on the inner wall of the prefabricated inlay opening; A stepped support surface is provided at the bottom of the prefabricated inlay opening; Anti-rotation plane, anti-rotation boss, locking hole or positioning hole provided on the side wall or bottom of the prefabricated inlay opening; Micro-tooth structure or porous rough interface is provided on the inner surface of the prefabricated inlay.

[0012] Furthermore, the outer connecting area of ​​the precious metal inlay is provided with a connecting structure adapted to the mechanical locking structure. The connecting structure includes one or more of the following: flange, folded edge, riveted part, flared part, undercut part, positioning part, meshing part, or roughened surface.

[0013] Furthermore, the connecting structure in the outer connecting area undergoes local plastic deformation through at least one of pressing, riveting, flaring, flanging, rolling, or interference fit, thereby forming the mechanical locking connection with the mechanical locking structure.

[0014] Furthermore, the inner setting area includes a gemstone support portion and a gemstone clamping portion; the gemstone clamping portion is one or a combination of prongs, bezels, edging, prongs, track walls, or micro-prongs, which fixes the gemstone through its own plastic deformation.

[0015] Secondly, the present invention provides a method for constructing a titanium-noble metal composite inlay structure, comprising the following steps: S1. Establish a three-dimensional model of the titanium substrate, and pre-set the pre-fabricated inlay and mechanical locking structure in the model; S2. Generate selected area laser melting forming data based on the three-dimensional model, using titanium or titanium alloy powder; S3. Selective laser melting process is used to melt powder layer by layer to prepare an integrated titanium matrix and prefabricated inlay. When forming the prefabricated inlay and its mechanical locking structure area, contour scanning or local fine scanning strategy is adopted, and the laser power and / or powder layer thickness are lower than those of the main load-bearing area. S4. Prepare a precious metal inlay that matches the pre-made inlay opening; S5. Place the precious metal inlay into the prefabricated inlay opening, and cause local plastic deformation of the outer connecting area by pressing, riveting, flaring, flanging or rolling, so as to form a mechanical locking connection with the mechanical locking structure. S6. Place the gemstone on the precious metal setting and fix it in place by plastically deforming the inner setting area of ​​the precious metal setting.

[0016] Based on the above technical solution, the present invention can be further improved as follows.

[0017] Furthermore, the post-processing includes one or more of the following: powder removal, support removal, heat treatment, sandblasting, polishing, anodizing, or PVD coating.

[0018] Furthermore, in step S3, when forming the main load-bearing area of ​​the titanium substrate, the volumetric energy density Ev of selective laser melting is controlled at 30-100 J / mm³; when forming the prefabricated inlay and mechanical locking structure area, the volumetric energy density Ev is controlled at 35-80 J / mm³. The volumetric energy density Ev = P / (v·h·t), where P is the laser power, v is the scanning speed, h is the scanning interval, and t is the powder layer thickness.

[0019] Furthermore, the inner setting area of ​​the precious metal inlay is provided with prongs, bezels, or track walls. In step S6, the gemstone is fixed by pressing, bending, or rolling the prongs, bezels, or track walls.

[0020] Thirdly, the present invention provides a piece of jewelry comprising the aforementioned titanium-precious metal composite setting structure.

[0021] Compared with the prior art, the technical solution of this application has the following beneficial technical effects: I. This invention significantly reduces the processing difficulty of complex inlay settings on titanium substrates, improving the manufacturing feasibility and dimensional consistency of micro-complex inlay structures. While titanium and titanium alloys possess advantages such as low density, high specific strength, good corrosion resistance, and rich surface decorative effects, they also suffer from problems during machining, including low thermal conductivity, concentrated cutting heat, high tool wear, and significant elastic recovery. For jewelry inlay structures, prefabricated inlay settings require intricate and complex features such as undercut grooves, dovetail grooves, annular grooves, stepped support surfaces, locking holes, positioning holes, micro-tooth structures, and anti-rotation structures. If these are formed after the titanium substrate is formed, the processing difficulty is high, and consistency is difficult to guarantee. This invention utilizes selective laser melting to simultaneously and integrally form prefabricated inlay settings and mechanical locking structures during the titanium substrate forming process. This allows the aforementioned complex structures to be directly obtained during the forming stage, thereby reducing or avoiding subsequent complex micro-subtractive machining.

[0022] Second, it effectively improves the connection stability between precious metal inlays and the titanium substrate. After the precious metal inlay is embedded in the pre-fabricated setting in the titanium substrate, its outer connection area undergoes localized plastic deformation through pressing, riveting, flaring, flanging, rolling, or interference fit. This allows the precious metal material to enter the undercut groove, dovetail groove, annular groove, locking hole, positioning hole, micro-toothed structure, or porous rough interface, forming a mechanical locking connection. This simultaneously restricts the axial pull-out, radial loosening, and circumferential rotation of the precious metal inlay relative to the titanium substrate, improving the structural reliability of the jewelry under long-term wear, impact, friction, and temperature change conditions. This connection does not rely on adhesives and does not require dissimilar metal welding between titanium and precious metals, avoiding problems such as welding heat effects, surface oxidation, and color changes.

[0023] Third, it avoids the operational difficulties and structural risks associated with directly setting gemstones in titanium substrates. Traditional gemstone setting techniques such as prong setting, bezel setting, pave setting, channel setting, and micro-pave setting rely on the controlled plastic deformation of metal prongs, bezels, or pegs under external force. However, titanium alloys have high hardness and significant elastic recovery, making them unsuitable for directly undertaking the function of delicate plastic setting. This invention transfers the gemstone fixing function to a malleable precious metal setting component. Precious metals with good ductility and adjustability, such as gold, karat gold, and platinum, complete the gemstone support and clamping, thereby reducing the technical difficulty of directly setting gemstones in titanium materials and improving the controllability, reliability, and ease of later maintenance of the gemstone fixing structure.

[0024] Fourth, it enables functional zoning and structural synergy among the titanium base, precious metal settings, and gemstones. The titanium base primarily undertakes functions such as complex design, lightweight load-bearing, structural support, and surface decoration; the precious metal settings primarily undertake functions such as mechanical locking with the titanium base, gemstone support, and gemstone plastic clamping; the gemstones, as the objects to be fixed, are set and secured by the precious metal settings. Through the above functional zoning, the advantages of titanium material—lightweight, high strength, complex forming, and surface coloring—are simultaneously utilized within the same jewelry structure, along with the technological advantages of precious metal materials—easy setting, easy repair, and easy maintenance.

[0025] Fifth, it can reduce the amount of precious metals used while maintaining the reliability of the gemstone setting process. Precious metal settings are only placed in key local areas where gemstone support, clamping, and mechanical locking are required, and their volume is preferably smaller than that of the titanium substrate. Thus, while reducing the amount of precious metals used, the malleability and adjustability of precious metals in gemstone setting are still retained, giving the jewelry products both a lightweight structure and good material economy.

[0026] VI. It can optimize the process sequence between titanium substrate post-processing, precious metal setting assembly, and gemstone protection. The titanium substrate can undergo post-processing steps such as powder removal, support removal, heat treatment, sandblasting, polishing, anodizing, or PVD coating before precious metal settings and gemstone assembly. This avoids premature exposure of gemstones or precious metal settings to high temperatures, sandblasting impacts, electrolytes, coating environments, or mechanical polishing processes, thereby reducing the risk of gemstone damage, precious metal part deformation, and decreased assembly accuracy.

[0027] VII. It possesses excellent product applicability and structural scalability. The titanium substrate can be made of pure titanium or titanium alloy, and can be applied to various jewelry forms such as rings, pendants, earrings, brooches, bracelets, necklaces, and watchmaking modules. The titanium substrate itself can be solid, hollow, lattice-shaped, thin-walled, or curved. Precious metal settings can be adapted to various gemstone setting methods such as prong setting, bezel setting, pave setting, channel setting, micro-pave setting, and channel setting. Therefore, this invention is suitable for the manufacture of high-end jewelry, personalized jewelry, lightweight jewelry, and modular jewelry. Attached Figure Description

[0028] Figure 1 This is a cross-sectional view of the titanium-precious metal composite inlay structure assembly provided in an embodiment of the present invention; Figure 2 These are schematic diagrams of various embodiments of the mechanical locking structure; Figure 3 This is a schematic diagram of the preparation method of the present invention; Figure 4 This is an assembly diagram of the structure in Example 1; Figure 5 This is an assembly diagram of the structure in Example 2.

[0029] The attached diagram lists the components represented by each number as follows: 1. Titanium base; 2. Prefabricated setting; 3. Mechanical locking structure; 4. Precious metal setting; 5. Outer connecting area; 6. Inner setting area; 7. Gemstone support; 8. Gemstone clamping part; 9. Gemstone; 10. Inverted groove; 11. Dovetail groove; 12. Annular groove; 13. Locking hole or positioning hole; 14. Micro-toothed or rough interface; 15. Anti-rotation structure; 16. Plastic deformation zone; 17. Prongs; 18. Press-in direction arrow; 19. Edging; 20. Support cup or support groove. Detailed Implementation

[0030] To facilitate understanding of this application, a more complete description will be provided below with reference to the accompanying drawings, which illustrate embodiments of the present application. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided so that the disclosure of this application will be thorough and complete.

[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application.

[0032] It should be noted that when one element is considered to be "connected" to another element, it can be directly connected to the other element or connected to the other element through an intermediary element. In the following embodiments, "connection" should be understood as "electrical connection," "communication connection," etc., if the connected circuits, modules, units, etc., have the transmission of electrical signals or data between them.

[0033] The core concept of this invention lies in the following: During the titanium substrate forming process, a pre-fabricated setting opening and its internal mechanical locking structure are simultaneously and integrally constructed using selective laser melting technology. A malleable precious metal setting is then embedded into this pre-fabricated setting opening, and through localized plastic deformation, it forms a stable mechanical locking connection with the mechanical locking structure. Finally, the precious metal setting supports and holds the gemstone in place. Thus, within the same jewelry structure, the structural support and lightweighting functions of the titanium substrate, the malleable setting function of the precious metal setting, and the stable fixing function of the gemstone are synergistically achieved.

[0034] The titanium-noble metal composite inlay structure provided by this invention, such as Figure 1As shown, the invention mainly includes a titanium substrate 1, a precious metal inlay 4, and a gemstone 9. The titanium substrate 1 has a pre-fabricated inlay opening 2, and the inner wall of the pre-fabricated inlay opening 2 has a mechanical locking structure 3. The pre-fabricated inlay opening 2 and the mechanical locking structure 3 are integrally formed simultaneously with the titanium substrate 1 using selective laser melting, rather than being obtained through a secondary subtractive processing step after the titanium substrate is formed. The precious metal inlay 4 is embedded in the pre-fabricated inlay opening 2, and it has an outer connecting area 5 facing the titanium substrate 1 and an inner inlay area 6 facing the gemstone 9. The outer connecting area 5 forms a mechanical locking connection with the mechanical locking structure 3 through localized plastic deformation, thereby restricting the axial pull-out, circumferential rotation, and radial loosening of the precious metal inlay 4 relative to the titanium substrate 1. The gemstone 9 is supported and clamped by the inner inlay area 6 of the precious metal inlay 4, and the titanium substrate 1 does not directly contact or press against the gemstone 9. The technical solution of the present invention will be described in detail below with reference to the accompanying drawings and specific embodiments.

[0035] The mechanical locking structure 3 is key to achieving a reliable connection between the titanium substrate and the precious metal insert in this invention. For example... Figure 2 As shown, the mechanical locking structure 3 includes one or more combinations of the following structures: a buckle groove 10, a dovetail groove 11, or an annular groove 12 provided on the inner wall of the prefabricated inlay 2; a stepped support surface provided on the bottom of the prefabricated inlay 2; an anti-rotation plane, an anti-rotation boss, a locking hole, or a positioning hole 13 provided on the side wall or bottom of the prefabricated inlay 2; and a micro-toothed structure 14 or a porous rough interface provided on the inner surface of the prefabricated inlay 2. Correspondingly, the outer connecting area 5 of the precious metal inlay 4 is provided with a connecting structure adapted to the above-mentioned mechanical locking structure, including one or more of the following: a flange, a flared portion, a riveted portion, a flared portion, a buckle, a positioning portion, a toothed portion, or a roughened surface. It undergoes local plastic deformation through at least one of the following methods: pressing, riveting, flaring, flanging, rolling, or interference fit, thereby forming a mechanical locking connection with the mechanical locking structure. It should be noted that the connection between the precious metal inlay 4 and the titanium substrate 1 does not rely on adhesives as the primary fixing method, nor does it require dissimilar metal welding between the titanium and the precious metal, thus avoiding problems such as welding heat effects, surface oxidation, color changes, or heat damage to the gemstone. The specific forms and working principles of each mechanical locking structure are described below. Those skilled in the art will understand that these structures can be used individually or in various combinations to enhance the locking effect.

[0036] The undercut groove 10 can be provided on the inner wall of the prefabricated inlay opening 2, and its opening direction is opposite to the insertion direction of the precious metal inlay 4 or forms a partial reverse limiting. As a specific embodiment, the groove depth of the undercut groove 10 can be 0.05-0.50mm, and the width can be 0.05-0.80mm. The annular groove 12 is a preferred form of the undercut groove 10, which extends continuously or intermittently along the circumferential direction of the inner wall of the prefabricated inlay opening 2 to form an annular locking space. When the outer connecting area 5 of the precious metal inlay 4 (e.g., its flange, flared portion, or turned-up portion) undergoes plastic deformation under riveting, rolling, or flaring action and fills the undercut groove 10 or the annular groove 12, the main limiting structure that restricts axial pull-out can be formed.

[0037] The dovetail groove 11 is a variant of the undercut groove, with its cross-sectional width gradually increasing from the groove opening to the bottom, forming a mechanically interlocking space that is wider inside and narrower outside. In one embodiment, the groove wall inclination angle of the dovetail groove 11 can be 5°-45°. Compared to ordinary rectangular cross-section grooves, the dovetail groove 11 can provide stronger lateral interlocking force because the plastically deformable material filled in it will generate a wedge-tightening effect under pull-out force, thereby simultaneously improving pull-out resistance and loosening resistance. The dovetail groove 11 can be provided along a partial sidewall of the inlay opening, or it can be provided continuously or intermittently along the circumference of the inlay opening.

[0038] The stepped support surface is located at the bottom or inner wall of the prefabricated setting 2 to support the bottom surface, outer flange, or annular support of the precious metal setting 4. Its main function is to provide a precise axial assembly positioning reference for the precious metal setting 4 and to bear and transfer the downward load on the gemstone and setting. The stepped support surface is usually used in combination with undercut grooves, annular grooves, etc., to provide axial support and axial pull-out prevention functions, respectively.

[0039] The anti-rotation structure 15 is used to restrict the circumferential rotation of the precious metal setting 4 within the pre-fabricated setting opening 2. Its specific implementation includes, but is not limited to, non-circular contours (such as ellipses or polygons) provided on the sidewalls of the pre-fabricated setting opening 2, anti-rotation planes, anti-rotation bosses, or anti-rotation grooves. Correspondingly, the outer connecting area 5 of the precious metal setting 4 is provided with matching non-circular outer walls, planes, grooves, or bosses. This structure is particularly important for applications requiring directional gemstone setting (such as marquise-cut, pear-shaped gemstones, or array-style track settings).

[0040] Locking holes or positioning holes 13 can be provided on the side wall, bottom, or stepped support surface of the prefabricated inlay 2, and their shape can be round, elliptical, square, elongated, blind, or through. During the assembly and plastic deformation of the precious metal inlay 4, part of the material of its outer connecting area 5 is squeezed or pressed into the locking holes or positioning holes 13, forming a discrete point-like riveting structure, thereby providing additional resistance to pull-out and rotation, as well as precise circumferential positioning reference.

[0041] The micro-tooth structure 14 is disposed on the inner wall, bottom, or opening edge of the prefabricated inlay 2, and its form includes circumferential teeth, longitudinal teeth, cross teeth, oblique teeth, dot matrix teeth, or irregular teeth. As a preferred embodiment, the tooth height is 0.01-0.20 mm and the tooth pitch is 0.02-0.30 mm. When the precious metal inlay 4 is assembled by pressing or rolling, the material of its outer connecting area 5 (especially the softer precious metal) will locally undergo plastic flow and embed into the depression of the micro-tooth structure 14, thereby multiplying the frictional resistance and mechanical interlocking force of the connecting interface without significantly changing the macroscopic structural dimensions.

[0042] A porous, roughened interface is essentially a microscale mechanical locking structure. It can be achieved directly through selective laser melting (SLM) to obtain high surface roughness (e.g., a surface not subsequently polished), or through specialized surface treatments such as sandblasting or laser etching. The porous, roughened interface primarily increases the contact area and friction, making it particularly suitable as an auxiliary locking mechanism in conjunction with the aforementioned macroscopic locking structures. Preferably, the porous, roughened interface is located in a non-visible assembly area of ​​the setting to avoid affecting the appearance of the jewelry.

[0043] In a preferred embodiment, a stepped support surface (for axial positioning and support), an annular undercut groove (for axial pull-out prevention), and an anti-rotation plane (for circumferential anti-rotation) can be simultaneously provided within the prefabricated setting opening 2, thereby achieving complete mechanical locking in multiple directions. In another preferred embodiment, a dovetail groove, a locking hole, and a micro-toothed structure can be simultaneously provided within the prefabricated setting opening 2, wherein the dovetail groove provides lateral engagement, the locking hole provides point-like riveting, and the micro-toothed structure improves contact resistance and local engagement capability. Those skilled in the art can make any feasible combination of the above-mentioned mechanical locking structures according to the structural requirements of specific jewelry, and all such combinations are within the protection scope of this invention.

[0044] Example 1 This embodiment provides a titanium-precious metal composite setting ring structure, the overall structure and assembly relationship are as follows: Figure 4 As shown.

[0045] The composite setting structure of this embodiment includes a TA2 pure titanium ring body (i.e., titanium base 1), an 18K gold prong setting (i.e., precious metal setting 4), and a round brilliant-cut diamond (i.e., gemstone 9). The titanium base 1 is the main body of the ring band and setting, made of TA2 pure titanium and integrally formed using selective laser melting. TA2 pure titanium has characteristics such as low density, high specific strength, good corrosion resistance, excellent biocompatibility, and the ability to obtain rich surface colors through anodizing, making it suitable as the main structural material for rings and other jewelry worn close to the body for extended periods. The top of the setting of the titanium base 1 has a pre-fabricated circular setting opening 2 for accommodating the precious metal setting. This pre-fabricated setting opening 2 is pre-established during the three-dimensional model design stage of the titanium base and integrally formed synchronously with the titanium base during the selective laser melting process, rather than being obtained through secondary processing such as CNC machining or manual grooving after the titanium base is formed.

[0046] The inner wall of the prefabricated setting slot 2 is provided with a mechanical locking structure 3. In this embodiment, the mechanical locking structure 3 includes an annular groove 12 (i.e., an annular undercut groove) provided in the lower middle part of the inner wall of the prefabricated setting slot 2, and a stepped support surface provided at the bottom of the prefabricated setting slot 2. The annular groove 12 has a depth of 0.15 mm and a width of 0.30 mm, and extends continuously along the circumference of the inner wall of the prefabricated setting slot 2. Its opening direction is opposite to the pull-out direction of the precious metal inlay, forming a reverse limit. The stepped support surface is used to determine the assembly depth of the precious metal inlay 4 in the prefabricated setting slot 2, and to bear the load transmitted downward by the gemstone and the precious metal inlay. The stepped support surface and the annular groove 12 are used together to provide axial support and axial anti-pull-out functions, respectively.

[0047] The precious metal setting 4 is an 18K gold ring-shaped prong setting, manufactured using a combination of lost-wax casting and CNC precision finishing. 18K gold (75% gold content) possesses excellent ductility, malleability, and workability, making it suitable for subsequent plastic deformation operations and gem setting. The precious metal setting 4 includes an outer connecting area 5 facing the titanium substrate and an inner setting area 6 facing the gemstone. The outer connecting area 5 has an annular flange that mates with the annular groove 12. The outer diameter of this annular flange is slightly larger than the inner diameter of the pre-made setting opening 2, forming an interference fit of 0.02mm to ensure initial radial clamping force after pressing in. The inner setting area 6 is provided with a gemstone support 7 and a gemstone clamping part 8. The gemstone support 7 is a support step located on the lower part of the inner wall of the ring setting, used to support the girdle of the diamond; the gemstone clamping part 8 consists of four evenly distributed prongs 17 extending upwards from the upper edge of the ring setting. Gemstone 9 is a 1.0-carat round brilliant-cut diamond, placed on the gemstone setting 7. Four prongs 17 are bent and pressed against the girdle and crown edge of the diamond, completing the prong setting. The diamond is not directly pressed or in contact with the titanium base 1. In terms of volume proportion, the 18K gold setting is only about 15% the volume of the titanium base. Precious metal is used only in key areas required for gemstone support, clamping, and mechanical locking, reducing the amount of precious metal used while ensuring the setting function.

[0048] The preparation method in this embodiment is as follows: Figure 3The process is as follows: In step S1, a 3D model of the TA2 pure titanium ring body is created using 3D modeling software. A circular pre-fabricated setting 2 is preset on the top of the ring setting, and an annular groove 12 is preset on the inner wall of the setting. A stepped support surface is preset at the bottom of the setting. The 3D model is then exported as an STL format file. In step S2, the STL file is imported into slicing software for model repair, adding supports, layer slicing, and setting the scanning path. The forming material is TA2 pure titanium powder, which is spherical or near-spherical with a particle size range of 15-45μm. The main load-bearing areas (ring arm and ring setting body) are filled using a scanning strategy, while fine areas such as the edge of the pre-fabricated setting, the annular groove, and the stepped support surface are contoured using a scanning strategy. In step S3, under an argon protective atmosphere (purity not less than 99.99%, oxygen content controlled below 500ppm), a selective laser melting device is used to lay powder layer by layer and scan and melt layer by layer to prepare a TA2 pure titanium ring body with an integrated pre-fabricated setting and a mechanical locking structure. The forming parameters for the main load-bearing area are: laser power 200W, scanning speed 900mm / s, scanning interval 0.08mm, powder layer thickness 0.03mm, and volumetric energy density of approximately 93J / mm³. The forming parameters for the prefabricated inlay and mechanical locking structure area are: laser power 140W, scanning speed 850mm / s, scanning interval 0.06mm, powder layer thickness 0.03mm, and volumetric energy density of approximately 91J / mm³. Lower laser power and smaller scanning interval are used to ensure that the inner wall of the annular groove is smooth and the edges are clear, avoiding defects such as over-melting, edge collapse, and powder adhesion.

[0049] In step S4, after forming, the titanium substrate undergoes sequential cleaning, support removal, wire cutting separation, vacuum stress-relieving heat treatment (550℃ / 2h, furnace cooling), sandblasting, and mechanical polishing. Before assembling the precious metal inlays and gemstones, the pre-fabricated inlay openings and their internal annular grooves are microscopically observed and dimensionally inspected to ensure no residual powder or structural defects, and the dimensional tolerances of the depth and width of the annular grooves are controlled within ±0.02mm. It is particularly important to note that the post-processing steps of the titanium substrate—especially heat treatment, sandblasting, and mechanical polishing—are all completed before the assembly of the precious metal inlays and the setting of the gemstones. The advantage of this is that if the gemstones or precious metal inlays are involved in these processes too early, the gemstones may crack or discolor due to high temperatures, the precious metal inlays may deform or scratch due to sandblasting impact, or the dimensional accuracy may be lost due to mechanical polishing. Conversely, by placing the post-processing before assembly, the titanium substrate can freely accept any required post-processing without worrying about the impact on the gemstones or precious metal parts, thus ensuring a higher quality finished product.

[0050] In step S5, an 18K gold ring-shaped prong setting is prepared using lost-wax casting combined with CNC precision finishing. An annular flange is machined on the outer side of the setting, and a supporting step and four prongs are machined on the inner side. Before assembly, the setting is annealed (650℃ / 30min, air-cooled) to reduce material hardness and improve plastic deformation capacity, ensuring sufficient filling of the annular groove during subsequent pressing and rolling processes. In step S6, the annealed 18K gold setting is pressed into the pre-made setting opening 2 of the TA2 pure titanium ring body along the pressing direction 18. During the pressing process, the annular flange on the outer wall of the setting corresponds to the annular groove 12 on the inner wall of the pre-made setting opening. Subsequently, a rolling tool is used to apply uniform circumferential pressure to the top of the setting, causing localized plastic deformation of the material in the outer connecting area 5 of the setting and squeezing it into the annular groove 12, forming a mechanical locking connection. This connection simultaneously restricts the axial pull-out, radial loosening, and circumferential rotation of the setting relative to the titanium substrate. Its fixation relies entirely on mechanical locking and does not depend on any adhesive. In step S7, diamond 9 is placed on the gemstone support 7 of the 18K gold setting, with the diamond's girdle resting on the support step. Using prong pliers, the four prongs 17 are pressed together sequentially, causing the prong tips to plastically bend and tightly fit against the diamond's girdle and crown edge, completing the prong setting. Throughout the setting process, the titanium base 1 does not have any direct contact or pressure transmission with the diamond; all the gemstone's holding force is provided by the 18K gold prongs. In step S8, the completed gemstone setting ring undergoes partial polishing and ultrasonic cleaning. The prong fit, diamond level, and overall assembly stability are inspected under a 10x magnifying glass. The inspection confirms no looseness between the setting and the titanium body, and the diamond is securely fixed, meeting jewelry quality requirements.

[0051] This embodiment utilizes selective laser melting to integrally form the setting opening and annular groove within the TA2 pure titanium ring body, avoiding the post-processing challenges of the complex microstructure of titanium. The 18K gold setting is mechanically locked between the annular flange and the annular groove, achieving multi-directional positioning to prevent axial pull-out, radial loosening, and circumferential rotation. The diamond is supported and held in place by 18K gold prongs, fully utilizing the malleable setting advantages of precious metals and avoiding the pressing difficulties, springback, and concentrated stress on the gemstone that may occur when directly setting gemstones into a titanium base. The titanium base provides structural support and lightweighting for the ring, while 18K gold is only used in key localized areas for gemstone support and holding, balancing material economy and process reliability.

[0052] Example 2 This embodiment provides a titanium-precious metal composite setting pendant structure, the structural diagram of which is shown below. Figure 5As shown. The main difference between this embodiment and Embodiment 1 is that the titanium base material is Ti-6Al-4V titanium alloy, the precious metal setting is a platinum (Pt950) bezel setting, and the gemstone is an emerald-cut emerald. This embodiment is particularly suitable for gemstone varieties such as emeralds, opals, and tourmalines that are sensitive to localized stress or have brittle edges.

[0053] The titanium base 1 serves as the pendant's main body, made of Ti-6Al-4V (TC4) titanium alloy, integrally formed using selective laser melting. Ti-6Al-4V is an α+β type dual-phase titanium alloy, with significantly higher strength than pure titanium, while maintaining lower density and good corrosion resistance, making it suitable as the main body material for pendants and other jewelry requiring high structural strength. The pendant's front face features a rectangular pre-fabricated setting 2, with a mechanical locking structure 3 on the inner wall of the setting. In this embodiment, the mechanical locking structure 3 includes an undercut groove 10 located at the bottom of the inner wall of the pre-fabricated setting 2 and a support cup or support groove 20 located at the bottom of the setting. The undercut groove 10 is continuously arranged along the four sides of the rectangle, with a depth of 0.20 mm, a width of 0.35 mm, a groove wall inclination angle of 15°, and an opening direction opposite to the pull-out direction of the precious metal setting. The support cup or support groove 20 provides stable axial support for the setting, transferring the load on the gemstone and setting to the titanium alloy pendant body.

[0054] The precious metal setting 4 is a platinum (Pt950) bezel setting, with an overall rectangular cup-shaped structure matching the rectangular pre-made setting opening 2. Platinum has excellent ductility, corrosion resistance, and chemical stability, and its malleability allows the bezel to evenly and smoothly cover the edge of the gemstone. The outer connecting area 5 has a flared flange that matches the undercut groove 10, and the inner setting area 6 includes a gemstone support 7 and a gemstone clamping part 8. The gemstone clamping part 8 is a continuous bezel 19 extending upward from the upper edge of the setting. The gemstone 9 is a 2.0-carat emerald-cut emerald, placed on the gemstone support 7 of the precious metal setting. The bezel 19 is bent and evenly covers and presses against the girdle edge of the emerald, completing the bezel setting. Emeralds usually contain natural inclusions and their edges are relatively brittle. The advantage of the bezel setting is that it can provide uniform peripheral support and clamping force, avoiding the local stress concentration that may occur at a few force points in prong setting, thus significantly reducing the risk of gemstone breakage during the setting process. Meanwhile, the platinum setting occupies only a small portion of the volume of the titanium alloy pendant, reducing the amount of precious metals used.

[0055] Regarding the preparation method, in step S3 of this embodiment, Ti-6Al-4V titanium alloy powder is used as the forming material. The powder is spherical or near-spherical with a particle size range of 15-45μm. The forming process is carried out in a high-purity argon protective environment (purity not less than 99.99%, oxygen content controlled below 500ppm). The forming parameters of the main load-bearing area (pendant body) are: laser power 280W, scanning speed 1000mm / s, scanning interval 0.10mm, powder layer thickness 0.04mm, and volumetric energy density of approximately 70J / mm³. This combination of parameters can achieve good comprehensive mechanical properties while ensuring the forming density. The forming parameters for the prefabricated setting and undercut groove areas are: laser power 160W, scanning speed 750mm / s, scanning interval 0.06mm, powder layer thickness 0.03mm, and volumetric energy density approximately 119J / mm³. Lower laser power and a thinner powder layer are used to reduce the heat-affected zone, ensure precise forming of the undercut angle of the groove, and avoid over-melting and closure of the groove opening and edge collapse. In step S4, the Ti-6Al-4V pendant body undergoes vacuum stress-relieving heat treatment (750℃ / 2h, furnace cooling), followed by sandblasting and mechanical polishing. The prefabricated setting and undercut groove are then subjected to microscopic observation and dimensional inspection. Similar to Example 1, these post-processing steps are completed before the precious metal setting and gemstone assembly, ensuring that the titanium alloy body can fully undergo heat treatment and surface treatment without affecting the subsequent platinum and emerald assembly.

[0056] In step S5, a platinum bezel setting is fabricated using a combination of stamping and CNC precision finishing. A flange structure is machined on the outer bottom of the setting to mate with the undercut groove, and a support surface and upright edging are machined on the inner side. Before assembly, the edging area undergoes localized annealing to reduce deformation resistance. In step S6, the platinum bezel setting is inserted along the pressing direction 18 into the rectangular pre-fabricated setting opening 2 of the titanium alloy pendant body. The bottom of the setting contacts and positions itself against the support cup or support groove 20. A flaring tool is used to apply outward expansion pressure to the outer connecting area 5 of the setting, causing the flange at the bottom of the outer connecting area to undergo plastic deformation and be squeezed into the undercut groove 10. The flange material gradually fills the inner wider-outer narrower space of the undercut groove, creating a wedge effect and forming a mechanical locking connection. This mechanical locking relies entirely on the structural interlocking between the materials and does not use adhesives for fixation. In step S7, the emerald 9 is placed on the gemstone support 7 of the setting. Using a bezel setting tool, the bezel 19 is gradually bent along the edge of the emerald to ensure it fits evenly and presses firmly against the girdle of the emerald, thus completing the bezel setting. The bezel pressure is evenly distributed across the entire girdle edge of the gemstone, avoiding localized stress concentration. The titanium alloy body does not participate in the clamping force of the gemstone during the entire gemstone setting process, nor does it directly contact the gemstone.

[0057] This embodiment demonstrates the application of the present invention in a Ti-6Al-4V titanium alloy system and bezel setting structure. Ti-6Al-4V titanium alloy has higher strength than pure titanium, meeting the structural support requirements of larger jewelry pieces such as pendants. The platinum bezel in the emerald setting fully demonstrates the core value of precious metals in bezel setting—it can evenly and smoothly cover the edge of the gemstone, providing uniform peripheral holding force and significantly reducing the risk of gemstone breakage during the setting process. The titanium alloy body does not directly participate in gemstone holding, avoiding the problem of difficulty in achieving fine bezel bending due to the high hardness and significant elastic recovery of titanium alloy.

[0058] Example 3 This embodiment provides a titanium-precious metal composite setting jewelry module with a multi-set array structure, suitable for bracelets, necklaces, or watches where multiple gemstones need to be arranged in an array or track. This embodiment illustrates that the invention is not only applicable to jewelry structures with a single main stone, but can also be extended to array or track setting applications with multiple small-sized gemstones.

[0059] The titanium base 1 serves as the bracelet connection module, made of Ti-6Al-4V titanium alloy and integrally formed using selective laser melting. Five equally spaced circular pre-fabricated inlay slots 2 are arranged along the arc direction on the module surface, forming an arc array. The radius of curvature of the array matches the curvature of the bracelet. Each pre-fabricated inlay slot 2 has a mechanical locking structure 3 on its inner wall, including micro-toothed structures 14 (circumferentially distributed, tooth height 0.05mm, tooth pitch 0.10mm) on the inner wall of each inlay slot 2, and a positioning hole 13 (blind hole, depth 0.30mm, diameter 0.40mm) at the bottom of the inlay slot.

[0060] The precious metal setting 4 consists of five independent 18K white gold micro-pavement sets, each corresponding to a pre-made setting opening. The outer connecting area 5 of the setting has a roughened surface (obtained through sandblasting, with a surface roughness Ra of approximately 3.2μm), and the bottom has a positioning protrusion that mates with the positioning hole 13. The inner setting area 6 has a gemstone support 7 and a gemstone clamping part 8. The gemstone support 7 is a support step located on the lower part of the inner wall of the setting, and the gemstone clamping part 8 consists of four micro-prongs evenly distributed on the upper edge of the setting. The gemstones 9 are five 2.5mm diameter round faceted sapphires, each placed in one of the five micro-pavement sets and fixed by the micro-prongs after being pressed and deformed. The total volume of the five 18K white gold settings is much smaller than that of the titanium alloy bracelet module, and the precious metal is only used in the localized areas necessary for gemstone setting, taking into account material economy.

[0061] In terms of the preparation method, step S3 uses the same Ti-6Al-4V powder (spherical, particle size 15-45μm) and main region forming parameters as in Example 2 (laser power 280W, scanning speed 1000mm / s, scanning interval 0.10mm, powder layer thickness 0.04mm, volumetric energy density approximately 70J / mm³). The five pre-fabricated inlay openings and their internal micro-texture structure and positioning holes employ fine-area parameters: laser power 160W, scanning speed 750mm / s, scanning interval 0.05mm, powder layer thickness 0.03mm, and volumetric energy density approximately 142J / mm³. This high local energy input ensures the complete forming of the micro-texture structure and the precise dimensions of the positioning holes. The micro-texture structure is directly formed using a contour scanning strategy: the scanning path is set with multiple concentric circular contours along the circumferential direction of the inner wall of the inlay opening, with a micro-gap of approximately 0.05mm between adjacent contours, thus naturally forming circumferential micro-textures on the forming surface. The positioning holes are pre-designed as blind holes in the 3D model, and a local fine scanning strategy is used to ensure the dimensional accuracy of the hole diameter and depth. The relative positional tolerance of the five prefabricated setting openings is guaranteed by the accuracy of the 3D model and the uniformity of the forming parameters of the selective laser melting process, and can be controlled within ±0.02mm. In step S4, the Ti-6Al-4V bracelet module is subjected to vacuum stress-relieving heat treatment (750℃ / 2h), sandblasting, and mechanical polishing in sequence. Before assembly, each of the five prefabricated setting openings is observed and dimensionally inspected under a microscope to ensure that the micro-textures are intact and the positioning holes are not blocked. Similarly, all post-processing steps are completed before the setting and gemstone assembly to avoid affecting subsequent assembly.

[0062] In step S5, five 18K white gold micro-pavement settings are mass-produced using metal injection molding to ensure dimensional consistency and production efficiency. The outer walls of the settings are sandblasted before assembly to create a roughened surface. In step S6, the five 18K white gold micro-pavement settings are sequentially pressed into their corresponding pre-made setting openings 2, with the positioning protrusions at the bottom of each setting aligned with the positioning holes 13 at the bottom of the setting opening. During the pressing process, the roughened surface of the setting's outer wall interlocks with the micro-toothed structure 14 of the pre-made setting opening's inner wall. The precious metal material undergoes localized plastic flow and fills the depressions in the micro-toothed structure, forming multi-point engagement, significantly improving contact resistance and mechanical locking force. The cooperation between the positioning protrusions and the positioning holes 13 prevents the settings from rotating circumferentially within the setting opening, while ensuring that the gemstone support direction of the five settings is consistent. In step S7, five sapphires 9 are placed on the gemstone support 7 of five micro-pavement sets respectively. Under a microscope, a micro-pavement tool is used to press the four micro-pavement prongs of each set in sequence, so that the tips of the micro-pavement prongs undergo plastic deformation and press the girdle edge of the sapphire to complete the micro-pavement fixation.

[0063] The multi-set array structure in this embodiment demonstrates the unique advantages of this invention in large-scale, small-sized gemstone setting scenarios. By simultaneously and integrally forming multiple precision pre-fabricated setting slots on a single titanium alloy module, the problems of multi-station clamping, accumulated positioning errors, and low processing efficiency in traditional CNC machining are avoided. The dimensional consistency and positional accuracy of the five setting slots are guaranteed by the accuracy of the three-dimensional model and the uniformity of forming parameters of the selective laser melting process. The combination of the micro-tooth structure and the roughened surface provides reliable contact resistance, and the cooperation between the positioning holes and positioning protrusions provides precise circumferential positioning, enabling the array-type multi-gemstone setting jewelry module to have good consistency and reliability.

[0064] The above three embodiments illustrate specific implementations of the present invention in three typical scenarios: prong setting for rings, bezel setting for pendants, and micro-pavement array for bracelet modules. It should be noted that the scope of application of the present invention is not limited to the above embodiments. Regarding the form of jewelry products, the titanium substrate 1 can also be other jewelry structural components such as earring bodies, brooch bodies, necklace connectors, watchmaking modules, or modular jewelry components. Regarding the structure of the titanium substrate, in addition to the solid structures shown in the embodiments, the advantages of selective laser melting technology in complex geometric forming can be fully utilized to design the titanium substrate as a hollow structure, lattice structure, thin-walled structure, curved surface structure, or mesh structure, thereby further reducing weight and enriching the appearance while ensuring structural strength. Regarding the post-processing of the titanium substrate, in addition to the heat treatment, sandblasting, and mechanical polishing used in the embodiments, anodizing can be performed to obtain rich surface colors, or PVD coating can be applied to obtain specific metallic luster and wear resistance, depending on the jewelry design requirements. These post-processing steps should also be completed before the precious metal settings and gemstone assembly. Regarding gemstone setting methods, in addition to prong setting, bezel setting, and micro-pave setting shown in the embodiments, other methods such as pave setting, channel setting, channel setting, or clamp setting can also be used to accommodate gemstones of different shapes, sizes, and hardness characteristics. Those skilled in the art can, based on the above embodiments, rationally select and adjust the material and structure of the titanium base, the specific combination of the mechanical locking structure, the material and setting method of the precious metal inlays, and the type and cutting form of the gemstones according to the design requirements of specific jewelry products. All such adjustments fall within the scope of protection of this invention.

[0065] Those skilled in the art should understand that the specific process parameters in the above three embodiments are not limitations on the present invention, but rather exemplary demonstrations of preferred parameter combinations for different materials and structural characteristics. Regarding material selection, the titanium base material can be pure titanium or titanium alloy, depending on the specific needs of the jewelry product: pure titanium (TA1, TA2) has lower hardness, better plasticity, and superior anodizing coloring effect, making it suitable for jewelry products such as rings and earrings that require high color decoration and are subjected to relatively mild stress environments; titanium alloys (TC4, Ti-6Al-4V, Ti-6Al-7Nb) have higher strength and hardness, making them suitable for products such as pendants, bracelet modules, and brooches that require high structural strength. Ti-6Al-7Nb contains niobium instead of vanadium, resulting in better biocompatibility, making it particularly suitable for jewelry that needs to be worn close to the body for extended periods. Precious metal inlays can be made of 18K gold, pure gold, silver, platinum (Pt950), palladium or their alloys, depending on the setting method and the characteristics of the gemstones. Appropriate annealing treatment should be carried out before assembly to optimize the plastic deformation ability: the annealing temperature of 18K gold inlays is preferably 550-680℃, and the annealing temperature of platinum inlays is preferably 700-850℃. After annealing, air cooling or furnace cooling is recommended.

[0066] The volumetric energy density Ev of selective laser melting (SLM) is calculated using the following formula: Ev = P / (v·h·t), where P is the laser power (W), v is the scanning speed (mm / s), h is the scanning distance (mm), and t is the powder layer thickness (mm). For pure titanium bodies, the volumetric energy density Ev of the load-bearing area is preferably controlled within the range of 30-100 J / mm³, more preferably within 35-80 J / mm³; the Ev of the prefabricated inlay and mechanical locking structure areas is preferably controlled within 35-80 J / mm³. For titanium alloy bodies, the Ev of the load-bearing area is preferably controlled within 30-120 J / mm³, more preferably within 45-90 J / mm³; the Ev of the prefabricated inlay and mechanical locking structure areas is preferably controlled within 45-90 J / mm³. It should be noted that volumetric energy density is only used to characterize the overall energy input relationship. In actual forming, different combinations of parameters may produce different molten pool shapes and surface qualities even with the same volumetric energy density. The optimization of process parameters should be carried out by combining laser power, scanning speed, scanning spacing and powder layer thickness.

[0067] The assembly clearance or interference between the prefabricated setting and the precious metal setting should be adjusted according to the hardness, annealing state, and depth of the mechanical locking structure of the precious metal material. For prong setting and bezel setting, the assembly clearance is preferably 0.03-0.10 mm, and the interference is preferably 0.01-0.05 mm; for micro-setting and track setting, the assembly clearance is preferably 0.01-0.08 mm, and the interference is preferably 0.005-0.03 mm.

[0068] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A titanium-noble metal composite rim structure, characterized by, include: A titanium substrate has a pre-fabricated inlay opening, the inner wall of which is provided with a mechanical locking structure. The pre-fabricated inlay opening and the mechanical locking structure are integrally formed with the titanium substrate by selective laser melting process. A precious metal inlay is set in the pre-made setting opening, having an outer connecting area facing the titanium substrate and an inner setting area facing the gemstone; the outer connecting area forms a mechanical locking connection with the mechanical locking structure through local plastic deformation to restrict the axial pull-out, circumferential rotation and radial loosening of the precious metal inlay relative to the titanium substrate; The gemstone is supported and held in place by the inner setting area of ​​the precious metal inlay, and the titanium base does not directly contact or press the gemstone.

2. The titanium-noble metal composite rim structure according to claim 1, wherein The mechanical locking structure includes one or more combinations of the following structures: An undercut groove, dovetail groove, or annular groove is provided on the inner wall of the prefabricated inlay opening; A stepped support surface is provided at the bottom of the prefabricated inlay opening; Anti-rotation plane, anti-rotation boss, locking hole or positioning hole provided on the side wall or bottom of the prefabricated inlay opening; Micro-tooth structure or porous rough interface is provided on the inner surface of the prefabricated inlay.

3. The titanium-noble metal composite inlay structure according to claim 1 or 2, characterized in that, The outer connecting area of ​​the precious metal inlay is provided with a connecting structure adapted to the mechanical locking structure. The connecting structure includes one or more of the following: flange, folded edge, riveted part, flared part, undercut part, positioning part, meshing part, or roughened surface.

4. The titanium-noble metal composite inlay structure according to claim 1 or 2, characterized in that, The connecting structure in the outer connecting area undergoes local plastic deformation through at least one of the following methods: pressing, riveting, flaring, flanging, rolling, or interference fit, thereby forming the mechanical locking connection with the mechanical locking structure.

5. The titanium-noble metal composite rim structure according to claim 1, wherein The inner setting area includes a gemstone support portion and a gemstone holding portion; the gemstone holding portion is one or a combination of prongs, bezels, edging, prongs, track walls or micro-prongs, which fixes the gemstone through its own plastic deformation.

6. A method of preparing the titanium-noble metal composite rim structure according to any one of claims 1 to 5, characterized in that Includes the following steps: S1. Establish a three-dimensional model of the titanium substrate, and pre-set the pre-fabricated inlay and mechanical locking structure in the model; S2. Generate selected area laser melting forming data based on the three-dimensional model, using titanium or titanium alloy powder; S3. Selective laser melting process is used to melt powder layer by layer to prepare an integrated titanium matrix and prefabricated inlay. When forming the prefabricated inlay and its mechanical locking structure area, contour scanning or local fine scanning strategy is adopted, and the laser power and / or powder layer thickness are lower than those of the main load-bearing area. S4. Prepare a precious metal inlay that matches the pre-made inlay opening; S5. Place the precious metal inlay into the prefabricated inlay opening, and cause local plastic deformation of the outer connecting area by pressing, riveting, flaring, flanging or rolling, so as to form a mechanical locking connection with the mechanical locking structure. S6. Place the gemstone on the precious metal setting and fix it in place by plastically deforming the inner setting area of ​​the precious metal setting.

7. The production method according to claim 6, wherein After step S3 and before step S5, there is a post-processing step for the titanium substrate, which includes one or more of the following: powder removal, support removal, heat treatment, sandblasting, polishing, anodizing, or PVD coating.

8. The preparation method according to claim 6, characterized in that, In step S3, when forming the main load-bearing area of ​​the titanium substrate, the volumetric energy density Ev of selective laser melting is controlled at 30-100 J / mm³; when forming the prefabricated inlay and mechanical locking structure area, the volumetric energy density Ev is controlled at 35-80 J / mm³. The volumetric energy density Ev = P / (v·h·t), where P is the laser power, v is the scanning speed, h is the scanning interval, and t is the powder layer thickness.

9. The preparation method according to claim 6, characterized in that, The inner setting area of ​​the precious metal setting is provided with prongs, bezels or track walls. In step S6, the gemstone is fixed by pressing, bending or rolling the prongs, bezels or track walls.

10. A piece of jewelry, characterized in that Includes the titanium-precious metal composite inlay structure as described in any one of claims 1-5.

Citation Information

Patent Citations

  • Dovetail micro-inlaying process

    CN101991251A

  • Shape memory alloy mounting collet with grooved gemstone

    CN103653576A

  • Method for producing titanium alloy artware by adopting selective laser melting

    CN104259459A

  • Titanium metal rimless inlaying method

    CN111202320A