A high-stability, high-temperature and acid-resistant composite nanofiltration membrane, its preparation method and application

By constructing a nanofiltration membrane with a rigid cross-linked network and a weather-resistant protective structure, the problem of temperature and acid resistance of nanofiltration membranes under high temperature and strong acid environments has been solved, achieving efficient separation and long service life for industrial applications.

CN123102176APending Publication Date: 2026-11-17VONTRON TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611494011.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-23
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing nanofiltration membranes have mismatched temperature and acid resistance in high-temperature and strong acid environments, are prone to structural failure, and have a rapid decline in separation accuracy, thus failing to meet the needs of industrial high-temperature and strong acid wastewater treatment.

Method used

A rigid intermediate with telage bases was prepared by reacting halogenated aniline with formaldehyde. Combined with a polysulfonamide functional layer and fluorosilane modification, a rigid crosslinking network and weather-resistant protective structure were constructed to enhance the stability and separation performance of the membrane.

Benefits of technology

Maintaining membrane structure stability in high-temperature and strong acid environments improves flux and rejection rate, extends service life, reduces operation and maintenance costs, and is suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102176A_ABST
    Figure CN123102176A_ABST
Patent Text Reader

Abstract

This invention relates to the field of nanofiltration membrane technology, specifically to a high-stability, high-temperature and acid-resistant composite nanofiltration membrane, its preparation method, and its application. The method includes the following steps: Haloaniline is dissolved in glacial acetic acid, formaldehyde is added, and the reaction is carried out under constant temperature and sealed conditions. After purification and vacuum drying, a halophenyl-Tellerg base rigid intermediate is obtained. A hydrophilically modified base membrane is sequentially immersed in an aqueous solution containing the halophenyl-Tellerg base rigid intermediate and an oil solution containing sulfonyl chloride monomer. After interfacial polymerization and room temperature curing, a solution containing a fluorosilane coupling agent is used for constant-temperature crosslinking. Then, after cleaning, drying, and curing, the high-stability, high-temperature and acid-resistant composite nanofiltration membrane is obtained. The composite nanofiltration membrane of this invention exhibits excellent long-term operational stability under high temperature and strong acid conditions, and can stably adapt to harsh operating conditions of 60–85℃ and pH 0–4. The preparation method of this invention completely solves the technical problem that traditional nanofiltration membranes cannot simultaneously achieve both high temperature and acid resistance, and is simple and easy to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of nanofiltration membrane technology, specifically to a high-stability, high-temperature resistant, and acid-resistant composite nanofiltration membrane, its preparation method, and its application. Background Technology

[0002] Nanofiltration membranes are pressure-driven precision separation membrane materials that fall between ultrafiltration and reverse osmosis. Utilizing unique nanoscale pore size sieving effects and surface charge selective repulsion effects, they can precisely and efficiently retain large organic molecules, colloids, and divalent and polyvalent inorganic salt ions, while ensuring efficient permeation of water molecules and monovalent salt ions. They possess numerous advantages such as high separation precision, low operating energy consumption, mild operating conditions, and no phase change separation required, making them a core membrane material in water treatment purification, industrial material purification, and wastewater resource recovery. However, with the rapid development of industries such as fine chemicals, hydrometallurgy, pharmaceuticals, pickling and electroplating, and petrochemicals, large amounts of high-temperature, strongly acidic wastewater and acidic material systems are generated during industrial production processes. Typical examples include high-temperature acidic wastewater from metallurgical pickling, acidic mother liquor from chemical esterification reactions, acidic purification wastewater from the pharmaceutical industry, and high-temperature acidic heavy metal wastewater. These industrial materials are generally characterized by high temperature (60–85℃), high acidity (pH 0–4), complex impurity composition, and the need for continuous and stable treatment. This places extremely high demands on the high-temperature resistance, strong acid corrosion resistance, long-term structural stability, and separation accuracy stability of the separation membrane materials. However, most existing commercial nanofiltration membrane products and modified nanofiltration membrane technologies are developed for mild operating conditions such as room temperature, neutral, or weakly acidic environments. They generally suffer from mismatches in temperature and acid resistance and are prone to failure under harsh conditions, making it difficult to meet the continuous separation and resource recovery needs of high-temperature, strongly acidic industrial systems.

[0003] From the perspective of molecular structure and material system, existing acid-resistant nanofiltration membranes generally use traditional polyamide functional layers as the core separation structure. Polyamide amide bonds have low bond energies and inherently poor acid hydrolytic stability, making them prone to protonation breakage and molecular chain degradation in high-temperature, strongly acidic environments. This makes the membrane material susceptible to structural failure under high-temperature, strongly acidic conditions. Some existing technologies improve room-temperature acid resistance through shallow modification methods such as blending with hydrophilic additives and simple surface crosslinking end-capping. However, these methods only improve membrane surface wettability and cannot address the fundamental problem of high-temperature acid hydrolysis damage at the molecular level. Consequently, the membrane material is only suitable for mild, weakly acidic conditions at room temperature. Once exposed to high-temperature, strongly acidic environments (≥55℃, pH ≤4), it quickly exhibits structural failure problems such as membrane swelling, cracking, and damage, resulting in a significant decrease in separation accuracy.

[0004] From the perspective of structural modification and process design, some studies focus on the heat resistance modification of the base film, optimizing the porosity and heat resistance of the base film by doping with inorganic fillers. However, they have not carried out acid-resistant structural design for the core functional separation layer. The heat-resistant modified film still cannot resist the corrosion and erosion of high-temperature acidic media, and cannot achieve both high-temperature resistance and strong acid resistance. Other studies rely on simple modification of rigid molecules to improve the mechanical strength of the film, without constructing a highly stable acid-resistant chemical bond system, nor with supporting interface reinforcement structure and surface protection structure. The above improvement methods can only improve the operational stability under normal temperature and neutral conditions, and have no adaptability to high-temperature and strong acid conditions.

[0005] From the perspective of finished product application performance, existing commercial and modified nanofiltration membranes generally lack three-dimensional rigid cross-linked network support and closed weather-resistant protective structure. The membrane molecular chains are prone to relaxation and slippage under high temperature environment, and the membrane pores are prone to collapse and deformation. At the same time, high temperature acidic media can continuously erode the internal structure of the membrane, ultimately resulting in rapid flux decay, poor retention stability, short service life, and high operation and maintenance costs under harsh operating conditions. They cannot meet the application requirements of continuous industrial production such as metallurgical pickling and purification of high temperature acidic chemical materials.

[0006] In summary, existing technologies suffer from problems such as poor acid and heat resistance of the material molecules, inability of the structure to simultaneously achieve both temperature and acid resistance, easy failure of the structure under harsh working conditions, significant degradation of separation performance, and weak industrial adaptability. Summary of the Invention

[0007] This invention addresses the shortcomings of existing acid-resistant nanofiltration membranes, such as poor high-temperature resistance, susceptibility to hydrolysis and damage under high-temperature and strongly acidic conditions, rapid decline in flux and rejection rate, insufficient structural stability, and short service life, making them unsuitable for harsh industrial conditions involving temperatures of 60–85°C and pH levels of 0–4. It provides a highly stable, high-temperature-resistant, and acid-resistant composite nanofiltration membrane, its preparation method, and its applications. By reconstructing the acid-resistant molecular system of the membrane layer, constructing a rigid cross-linked network, and adding a weather-resistant protective structure, this invention broadens the membrane's tolerance range under various operating conditions, extends its service life, reduces industrial maintenance costs, and adapts it to large-scale mass production and demanding industrial applications, while ensuring high flux and high sieving accuracy.

[0008] The technical solution of this invention: The first objective of this invention is to provide a method for preparing a highly stable, high-temperature resistant, and acid-resistant nanofiltration membrane, comprising the following steps: Step 1: Preparation of rigid functional intermediate: Dissolve haloaniline in glacial acetic acid, add formaldehyde, react under constant temperature and sealed conditions, and then purify and vacuum dry to obtain halophenyl teleg base rigid intermediate. Step 2: Preparation of the separation layer: The hydrophilic modified base film is sequentially immersed in an aqueous solution containing a halogenated phenyl telreg base rigid intermediate and an oil solution containing a sulfonyl chloride monomer. Interfacial polymerization is then performed, followed by room temperature curing to form a polysulfonamide-telreg base rigid functional separation layer. The mass fraction of the halogenated phenyl telreg base rigid intermediate in the aqueous solution is 0.2%-0.4%. Step 3 Fluorosilane modification: The membrane obtained in Step 2 is crosslinked at a constant temperature using a solution containing a fluorosilane coupling agent, and then cleaned, dried and cured to obtain a high-stability, high-temperature resistant, and acid-resistant composite nanofiltration membrane; the volume fraction of the fluorosilane coupling agent in the solution is 2%-4%.

[0009] The hydrophilic modified base film is obtained by immersing the base film in an aqueous solution containing polyvinyl alcohol and glutaraldehyde.

[0010] Preferably, the hydrophilic modified base film is obtained by immersing the base film in an aqueous solution containing polyvinyl alcohol and glutaraldehyde for 3 hours, then washing it until neutral, and finally drying it.

[0011] The base film is any one or a combination of two or more of polyethersulfone, polysulfone, polyvinylidene fluoride, and polyimide.

[0012] The pore size of the base membrane is 0.05-0.2 μm, preferably 0.1 μm.

[0013] The porosity of the base membrane is 75%-85%, preferably 80%.

[0014] The aqueous solution containing polyvinyl alcohol and glutaraldehyde has a polyvinyl alcohol mass fraction of 1% to 3% and a glutaraldehyde mass fraction of 0.5% to 1.2%. Preferably, the aqueous solution contains a polyvinyl alcohol mass fraction of 2% and a glutaraldehyde mass fraction of 0.8%.

[0015] The polyvinyl alcohol has a molecular weight of 10,000 to 100,000 Da, preferably 40,000 to 80,000 Da.

[0016] The aqueous solution containing the halogenated phenyl telrogal base rigid intermediate is composed of the following components by mass fraction: 0.3%-0.8% polyamine monomer, 0.2%-0.4% halogenated phenyl telrogal base rigid intermediate, and the balance being water.

[0017] Preferably, the aqueous solution containing the halogenated phenyl telreg base rigid intermediate has a polyamine monomer mass fraction of 0.5% and a halogenated phenyl telreg base rigid intermediate mass fraction of 0.3%.

[0018] The oil phase solution containing sulfonyl chloride monomer is composed of sulfonyl chloride monomer and organic solvent; the amount of sulfonyl chloride monomer added is 0.2%-0.5% by mass fraction, preferably 0.3%.

[0019] The sulfonyl chloride monomer is any one or a combination of two of 1,3,5-benzenetrisulfonyl chloride and p-benzenedisulfonyl chloride.

[0020] The organic solvent is any one or a combination of two or more of n-hexane, cyclohexane, petroleum ether, and toluene; preferably n-hexane.

[0021] In step 2, the soaking time in the aqueous solution containing the halogenated phenyl telreg base rigid intermediate is 1-3 min, preferably 2 min.

[0022] In step 2, the immersion time in the oil phase solution containing sulfonyl chloride monomer is 45-90 seconds, preferably 60 seconds.

[0023] In step 2, the room temperature curing time is 5-10 minutes, preferably 8 minutes.

[0024] The fluorosilane coupling agent is any one or a combination of two of tridecylfluorooctyltriethoxysilane and trifluoropropyltrimethoxysilane.

[0025] Preferably, the volume fraction of the fluorosilane coupling agent in the solution is 3%.

[0026] In step 3, the reaction temperature for the isothermal crosslinking is 45-55℃, preferably 50℃; the crosslinking reaction time is 35-50 min, preferably 40 min.

[0027] The second objective of this invention is to provide a high-stability, high-temperature resistant, and acid-resistant composite nanofiltration membrane prepared according to the aforementioned preparation method.

[0028] The third objective of this invention is to provide the application of the highly stable, high-temperature resistant, and acid-resistant composite nanofiltration membrane in the treatment of high-temperature acidic wastewater in hydrometallurgy, the purification of acidic materials in fine chemicals, the purification of acidic mother liquor in the pharmaceutical industry, the resource recovery of pickling and electroplating wastewater, and the treatment of high-temperature acidic water in petrochemicals.

[0029] The beneficial effects of this invention are: The high-temperature and acid-resistant composite nanofiltration membrane of this invention exhibits excellent long-term operational stability in high-temperature and strong acid environments. It can stably adapt to harsh operating conditions of 60–85℃ and pH 0–4, i.e., the membrane can operate continuously for 30 days in a strongly acidic environment at 70℃ and pH=2, with a pure water flux of 185 L / m³ at an operating pressure of 1.0 MPa. 2The removal rate of divalent salts remained stable at 98.2% over h, with a flux decline rate of only 2.1% over 30 days. The membrane exhibited no swelling, cracking, or delamination, and its microstructure and macroscopic separation performance remained essentially stable. The preparation method of this invention completely solves the technical challenge of synergistically achieving both temperature and acid resistance in traditional nanofiltration membranes, and is simple and easy to operate.

[0030] (1) This invention uses polyvinyl alcohol (PVA) as a hydrophilic modifier, glutaraldehyde as a crosslinking curing agent, and Teleg base rigid cage molecular material as a temperature and acid resistant modifier to modify the structure and enhance the function of polyethersulfone-based membranes. Teleg base has a three-dimensional rigid cage structure, which can be uniformly doped between the molecular chains of the membrane layer. It can effectively improve the regularity of the arrangement of polymer molecular chains, inhibit the relaxation and slippage of molecular chains under high temperature conditions, avoid the high temperature collapse and deformation of membrane pores, and greatly improve the overall high temperature resistance and dimensional stability of the membrane. In addition, the rigid skeleton structure can effectively resist the swelling and erosion of strong acid media, improve the acid resistance and swelling resistance of the membrane, and prevent the membrane material from structurally failing under high temperature and strong acid conditions. At the same time, the polyvinyl alcohol-glutaraldehyde crosslinking system can build rich active crosslinking sites on the surface of the base membrane, effectively improve the interfacial bonding force between the upper functional layer and the base membrane, and eliminate the problem of membrane layer delamination.

[0031] (2) This invention uses sulfonyl chloride monomers and polyamine monomers as polymerization raw materials to construct a highly stable polysulfonamide functional separation layer through oil-water phase interface polymerization, forming a dense and precise nano-sieving functional layer. High-bond-energy S=O covalent bonds replace low-bond-energy amide bonds, effectively enhancing the high-temperature acid hydrolysis stability of the nanofiltration membrane. It can maintain the integrity of chemical bonds and prevent degradation under high-temperature and strong acid environments, thus solving the problem of membrane hydrolysis and damage under high-temperature and strong acid conditions, and significantly improving the membrane's acid hydrolysis stability. Simultaneously, combined with Teleg bases, the three-dimensional rigid cage structure of Teleg bases is interwoven and cross-linked between the polysulfonamide molecular chains, constructing a high-density rigid cross-linked network. This effectively optimizes the membrane pore structure and sieving precision, restricts molecular chain relaxation and slippage under high-temperature conditions, ensures stable salt rejection performance of the membrane under harsh conditions, and prevents membrane pore collapse, membrane swelling and deformation, achieving high-precision separation under high-temperature and strong acid environments, preventing flux disturbances and a sharp drop in rejection rate. For the specific microstructure, see [link to microstructure description]. Figure 1 .

[0032] (3) This invention uses a fluorinated alkyl silane coupling agent as a surface weather-resistant modifier and employs a low-temperature isothermal cross-linking post-treatment process to construct a dense acid-resistant and high-temperature-resistant protective modification layer on the surface of the polysulfonamide functional layer. The silane coupling agent can undergo a covalent cross-linking reaction with the surface active groups of the functional layer, sealing the microscopic pore defects of the membrane surface, forming a closed protective barrier, and forming an integrated double cross-linked interpenetrating network structure, effectively isolating the high-temperature acidic corrosive medium from contact with the internal structure of the membrane, and inhibiting acid corrosion penetration damage; at the same time, fluorosilane modification can reduce the surface energy of the membrane surface, endowing the membrane with excellent anti-fouling and anti-corrosion properties, significantly delaying the aging rate of the membrane, and extending its service life. Attached Figure Description

[0033] Figure 1 This is a SEM image of the high-temperature and acid-resistant composite nanofiltration membrane of the present invention. Figure 2 This is a SEM image of the high-temperature and acid-resistant nanofiltration membrane after 30 days of operation in Example 1. Figure 3 This is a SEM image of the nanofiltration membrane without a functional layer in Comparative Example 1. Detailed Implementation

[0034] The present invention will be further described below with reference to specific embodiments; however, these embodiments should not be construed as limiting the scope of the present invention. Example 1 A method for preparing a highly stable, high-temperature resistant, and acid-resistant nanofiltration membrane includes the following steps: Step 1: Preparation of rigid functional intermediate: Dissolve 8g of haloaniline in 100g of glacial acetic acid, add 4g of formaldehyde solution, and react at a constant temperature of 25℃ for 48h. After purification and vacuum drying, the rigid intermediate of the Tereg base is obtained. Step 2: Hydrophilic modification of the base membrane: At room temperature, a polyethersulfone membrane with a pore size of 0.1 μm and a porosity of 80% was immersed in an aqueous solution containing 2% polyvinyl alcohol (50000 Da) and 0.8% glutaraldehyde for 3 hours, rinsed with deionized water until neutral, and dried at 60°C to obtain a hydrophilic modified porous support base membrane. Step 3: Prepare an aqueous solution: Use deionized water as a solvent to prepare an aqueous solution containing 0.5% piperazine and 0.3% telage base intermediate. Step 4: Prepare the oil phase solution: Prepare a 0.3% (w / w) 1,3,5-benzenetrisulfonyl chloride oil phase solution using n-hexane as the solvent; Step 5: Preparation of the separation layer: The hydrophilic modified base film is immersed in the aqueous solution obtained in step 3 for 2 min, then the surface liquid is removed and it is immersed in the oil solution obtained in step 4 for interfacial polymerization for 60 s, and cured at room temperature for 8 min to form a polysulfonamide-Tellerg base rigid functional separation layer. Step 6 Fluorosilane modification: Under constant temperature of 50℃, the membrane obtained in step 5 is crosslinked for 40 min using an ethanol solution containing 3% tridefluorooctyltriethoxysilane by volume. After washing with deionized water, it is dried and cured at 90℃ to obtain a high-stability, high-temperature resistant, and acid-resistant composite nanofiltration membrane.

[0035] In Example 1, the membrane prepared by the above operations was set as the experimental group, and a traditional polysulfonamide nanofiltration membrane without the addition of the Teleg base intermediate and without fluorosilane modification was set as the control group. Under the conditions of raw water temperature of 80℃, pH=4, and operating pressure of 1.0MPa, the membrane was continuously operated for 30 days. Compared with the control group, the divalent magnesium salt rejection rate of the experimental group increased from 88.5% to 98.2%, and the pure water flux increased from 182L / (m³) 2 ·h) optimized to 185L / (m 2 ·h), the flux decay rate decreased from 11.8% to 2.1% over 30 days, and the membrane did not swell or crack under high temperature and strong acid conditions (see Figure 2 It exhibits excellent high-temperature and acid resistance stability.

[0036] Example 2 A method for preparing a highly stable, high-temperature resistant, and acid-resistant nanofiltration membrane includes the following steps: Step 1: Preparation of rigid functional intermediate: Dissolve 8g of haloaniline in 100 parts by weight of glacial acetic acid, add 4g of formaldehyde solution, and react at a constant temperature of 25℃ for 48h. After purification and vacuum drying, the rigid intermediate of the Tereg base is obtained. Step 2: Hydrophilic modification of the base membrane: At room temperature, a polyethersulfone membrane with a pore size of 0.1 μm and a porosity of 77% was immersed in an aqueous solution containing 2% polyvinyl alcohol (60000 Da) and 0.8% glutaraldehyde for 3 hours, rinsed with deionized water until neutral, and dried at 60°C to obtain a hydrophilic modified porous support base membrane. Step 3: Prepare an aqueous solution: Use deionized water as a solvent to prepare an aqueous solution containing 0.5% m-phenylenediamine and 0.3% telrog base intermediate by mass concentration. Step 4: Prepare the oil phase solution: Prepare a 0.3% (w / w) 1,3,5-benzenetrisulfonyl chloride oil phase solution using n-hexane as the solvent; Step 5: Preparation of the separation layer: The hydrophilic modified base film is immersed in the aqueous solution obtained in step 3 for 2 min, then the surface liquid is removed and it is immersed in the oil solution obtained in step 4 for interfacial polymerization for 60 s, and cured at room temperature for 8 min to form a polysulfonamide-Tellerg base rigid functional separation layer. Step 6 Fluorosilane modification: Under constant temperature of 50℃, the membrane obtained in step 5 is crosslinked for 40 min using an ethanol solution containing 3% tridefluorooctyltriethoxysilane by volume. After washing with deionized water, it is dried and cured at 90℃ to obtain a high-stability, high-temperature resistant, and acid-resistant composite nanofiltration membrane.

[0037] In Example 2, the membrane prepared by the above operation was set as the experimental group, and a nanofiltration membrane of m-phenylenediamine-polysulfonamide system without the addition of the telrogal base intermediate was set as the control group. Under the conditions of raw water temperature of 80℃, pH=4, and operating pressure of 1.0MPa, it was continuously operated for 30 days. Compared with the control group, the divalent magnesium salt rejection rate of the experimental group increased from 87.9% to 97.8%, and the pure water flux increased from 175L / (m³) 2 ·h) optimized to 178L / (m 2 The flux decay rate decreased from 12.3% to 2.5% over 30 days, significantly improving the structural stability under high temperature and strong acid conditions.

[0038] Example 3 A method for preparing a highly stable, high-temperature resistant, and acid-resistant nanofiltration membrane includes the following steps: Step 1: Preparation of rigid functional intermediate: Dissolve 8g of haloaniline in 100g of glacial acetic acid, add 4g of formaldehyde solution, and react at a constant temperature of 25℃ for 48h. After purification and vacuum drying, the rigid intermediate of the Tereg base is obtained. Step 2: Hydrophilic modification of the base membrane: At room temperature, a polyethersulfone membrane with a pore size of 0.1 μm and a porosity of 83% was immersed in an aqueous solution containing 2% polyvinyl alcohol (70000 Da) and 0.8% glutaraldehyde for 3 hours, rinsed with deionized water until neutral, and dried at 60°C to obtain a hydrophilic modified porous support base membrane. Step 3: Prepare an aqueous solution: Use deionized water as a solvent to prepare an aqueous solution containing 0.5% piperazine and 0.3% telage base intermediate. Step 4: Prepare the oil phase solution: Prepare a 0.3% (w / w) p-phenylenesulfonyl chloride oil phase solution using n-hexane as the solvent; Step 5: Preparation of the separation layer: The hydrophilic modified base film is immersed in the aqueous solution obtained in step 3 for 2 min, then the surface liquid is removed and it is immersed in the oil solution obtained in step 4 for interfacial polymerization for 60 s, and cured at room temperature for 8 min to form a polysulfonamide-Tellerg base rigid functional separation layer. Step 6 Fluorosilane modification: Under constant temperature of 50℃, the membrane obtained in step 5 is crosslinked for 40 min using an ethanol solution containing 3% tridefluorooctyltriethoxysilane by volume. After washing with deionized water, it is dried and cured at 90℃ to obtain a high-stability, high-temperature resistant, and acid-resistant composite nanofiltration membrane.

[0039] In Example 3, the membrane prepared by the above operation was designated as the experimental group, and a polyamide nanofiltration membrane polymerized by conventional trimesoyl chloride was used as the control group. Under conditions of raw water temperature of 85℃, pH=4, and operating pressure of 1.0MPa, after continuous operation for 30 days, compared with the control group, the divalent magnesium salt rejection rate of the experimental group increased from 72.3% to 97.9%, and the pure water flux increased from 190L / (m²) 2 ·h) fine-tuned to 181L / (m 2 The flux decay rate over 30 days decreased from 32.6% to 2.3%, completely solving the problem of high-temperature acid degradation failure of traditional polyamide membranes.

[0040] Example 4 A method for preparing a highly stable, high-temperature resistant, and acid-resistant nanofiltration membrane includes the following steps: Step 1: Preparation of rigid functional intermediate: Dissolve 8g of haloaniline in 100g of glacial acetic acid, add 4g of formaldehyde solution, and react at a constant temperature of 25℃ for 48h. After purification and vacuum drying, the rigid intermediate of the Tereg base is obtained. Step 2: Hydrophilic modification of the base membrane: At room temperature, a polyethersulfone membrane with a pore size of 0.1 μm and a porosity of 85% was immersed in an aqueous solution containing 2% polyvinyl alcohol (80000 Da) and 0.8% glutaraldehyde for 3 hours, rinsed with deionized water until neutral, and dried at 60°C to obtain a hydrophilic modified porous support base membrane. Step 3: Prepare an aqueous solution: Use deionized water as a solvent to prepare an aqueous solution containing 0.5% piperazine and 0.3% telage base intermediate. Step 4: Prepare the oil phase solution: Prepare a 0.3% (w / w) 1,3,5-benzenetrisulfonyl chloride oil phase solution using n-hexane as the solvent; Step 5: Preparation of the separation layer: The hydrophilic modified base film is immersed in the aqueous solution obtained in step 3 for 2 min, then the surface liquid is removed and it is immersed in the oil solution obtained in step 4 for interfacial polymerization for 60 s, and cured at room temperature for 8 min to form a polysulfonamide-Tellerg base rigid functional separation layer. Step 6 Fluorosilane modification: Under constant temperature of 50℃, the membrane obtained in step 5 is crosslinked for 40 min using an ethanol solution containing 3% trifluoropropyltrimethoxysilane by volume. After washing with deionized water, it is dried and cured at 90℃ to obtain a high-stability, high-temperature resistant, and acid-resistant composite nanofiltration membrane.

[0041] In Example 4, the membrane prepared by the above operation was designated as the experimental group, and a polysulfonamide-Tellerg base nanofiltration membrane with a fluorine-free silane surface protection was used as the control group. Under the conditions of raw water temperature 70℃, pH=4, and operating pressure 1.0MPa, after continuous operation for 30 days, compared with the control group, the divalent magnesium salt rejection rate of the experimental group increased from 92.1% to 97.5%, and the pure water flux increased from 186L / (m³)2 ·h) fine-tuned to 176L / (m 2 ·h), the flux decay rate over 30 days decreased from 7.5% to 2.8%, and the acid corrosion resistance of the membrane surface was significantly improved.

[0042] Example 5 A method for preparing a highly stable, high-temperature resistant, and acid-resistant nanofiltration membrane includes the following steps: Step 1: Preparation of rigid functional intermediate: Dissolve 8g of haloaniline in 100g of glacial acetic acid, add 4g of formaldehyde solution, and react at a constant temperature of 25℃ for 48h. After purification and vacuum drying, the rigid intermediate of the Tereg base is obtained. Step 2: Hydrophilic modification of the base membrane: At room temperature, a polyethersulfone membrane with a pore size of 0.1 μm and a porosity of 75% was immersed in an aqueous solution containing 2% polyvinyl alcohol (40000 Da) and 0.8% glutaraldehyde for 3 hours, rinsed with deionized water until neutral, and dried at 60°C to obtain a hydrophilic modified porous support base membrane. Step 3: Prepare an aqueous solution: Use deionized water as a solvent to prepare an aqueous solution containing 0.5% piperazine and 0.2% telage base intermediate. Step 4: Prepare the oil phase solution: Prepare a 0.3% (w / w) 1,3,5-benzenetrisulfonyl chloride oil phase solution using n-hexane as the solvent; Step 5: Preparation of the separation layer: The hydrophilic modified base film is immersed in the aqueous solution obtained in step 3 for 2 min, then the surface liquid is removed and it is immersed in the oil solution obtained in step 4 for interfacial polymerization for 60 s, and cured at room temperature for 8 min to form a polysulfonamide-Tellerg base rigid functional separation layer. Step 6 Fluorosilane modification: Under constant temperature of 50℃, the membrane obtained in step 5 is crosslinked for 40 min using an ethanol solution containing 3% tridefluorooctyltriethoxysilane by volume. After washing with deionized water, it is dried and cured at 90℃ to obtain a high-stability, high-temperature resistant, and acid-resistant composite nanofiltration membrane.

[0043] In Example 5, the membrane prepared by the above operation was designated as the experimental group, and a nanofiltration membrane modified with a high doping level of 0.4% Teleg bases was used as the control group. Under the conditions of raw water temperature of 85℃, pH=4, and operating pressure of 1.0MPa, after continuous operation for 30 days, compared with the control group, the divalent magnesium salt rejection rate of the experimental group fluctuated slightly to 97.6%, and the pure water flux increased from 179L / (m³) to 97.6%. 2 •h) increased to 183L / (m 2 The flux decay rate stabilized at 3.0% over 30 days, achieving a balanced optimization of flux and acid resistance stability.

[0044] Example 6 A method for preparing a highly stable, high-temperature resistant, and acid-resistant nanofiltration membrane includes the following steps: Step 1: Preparation of rigid functional intermediate: Dissolve 8g of haloaniline in 100g of glacial acetic acid, add 4g of formaldehyde solution, and react at a constant temperature of 25℃ for 48h. After purification and vacuum drying, the rigid intermediate of the Tereg base is obtained. Step 2: Hydrophilic modification of the base membrane: At room temperature, a polyethersulfone membrane with a pore size of 0.1 μm and a porosity of 77% was immersed in an aqueous solution containing 2% polyvinyl alcohol (70000 Da) and 0.8% glutaraldehyde for 3 hours, rinsed with deionized water until neutral, and dried at 60°C to obtain a hydrophilic modified porous support base membrane. Step 3: Prepare an aqueous solution: Use deionized water as a solvent to prepare an aqueous solution containing 0.5% piperazine and 0.3% telage base intermediate. Step 4: Prepare the oil phase solution: Prepare a 0.3% (w / w) 1,3,5-benzenetrisulfonyl chloride oil phase solution using n-hexane as the solvent; Step 5: Preparation of the separation layer: The hydrophilic modified base film is immersed in the aqueous solution obtained in step 3 for 2 min, then the surface liquid is removed and it is immersed in the oil solution obtained in step 4 for interfacial polymerization for 45 s, and cured at room temperature for 8 min to form a polysulfonamide-Tellerg base rigid functional separation layer. Step 6 Fluorosilane modification: Under constant temperature of 50℃, the membrane obtained in step 5 is crosslinked for 40 min using an ethanol solution containing 3% tridefluorooctyltriethoxysilane by volume. After washing with deionized water, it is dried and cured at 90℃ to obtain a high-stability, high-temperature resistant, and acid-resistant composite nanofiltration membrane.

[0045] In Example 6, the membrane obtained by the above operation was designated as the experimental group, and a dense nanofiltration membrane with an interfacial polymerization time of 90 s was used as the control group. Under the conditions of raw water temperature of 85℃, pH=4, and operating pressure of 1.0 MPa, after continuous operation for 30 days, compared with the control group, the divalent magnesium salt rejection rate of the experimental group was slightly adjusted from 98.5% to 97.3%, and the pure water flux increased from 165 L / (m²) to 165 L / (m³). 2 •h) increased to 188L / (m 2 ·h), with a 30d flux decay rate of 2.9%, significantly improving permeable flux while ensuring acid and high temperature resistance.

[0046] Example 7 A method for preparing a highly stable, high-temperature resistant, and acid-resistant nanofiltration membrane includes the following steps: Step 1: Preparation of rigid functional intermediate: Dissolve 8g of haloaniline in 100g of glacial acetic acid, add 4g of formaldehyde solution, and react at a constant temperature of 25℃ for 48h. After purification and vacuum drying, the halophenyl teleg base rigid intermediate is obtained. Step 2: Hydrophilic modification of the base membrane: At room temperature, a polyethersulfone membrane with a pore size of 0.1 μm and a porosity of 82% was immersed in an aqueous solution containing 2% polyvinyl alcohol (55000 Da) and 0.8% glutaraldehyde for 3 hours, rinsed with deionized water until neutral, and dried at 60°C to obtain a hydrophilic modified porous support base membrane. Step 3: Prepare an aqueous solution: Use deionized water as a solvent to prepare an aqueous solution containing 0.5% piperazine and 0.3% telage base intermediate. Step 4: Prepare the oil phase solution: Prepare a 0.3% (w / w) 1,3,5-benzenetrisulfonyl chloride oil phase solution using n-hexane as the solvent; Step 5: Preparation of the separation layer: The hydrophilic modified base film is immersed in the aqueous solution obtained in step 3 for 2 min, then the surface liquid is removed and it is immersed in the oil solution obtained in step 4 for interfacial polymerization for 60 s, and cured at room temperature for 8 min to form a polysulfonamide-Tellerg base rigid functional separation layer. Step 6 Fluorosilane modification: Under constant temperature of 55℃, the membrane obtained in step 5 is crosslinked for 35 min using an ethanol solution containing 3% tridefluorooctyltriethoxysilane by volume. After washing with deionized water, it is dried and cured at 90℃ to obtain a high-stability, high-temperature resistant, and acid-resistant composite nanofiltration membrane.

[0047] In Example 7, the membrane prepared by the above operation was used as the experimental group, and a conventional modified membrane cross-linked at 50°C for 40 min was used as the control group. Under the conditions of raw water temperature of 85°C, pH=4, and operating pressure of 1.0 MPa, after continuous operation for 30 days, compared with the control group, the divalent magnesium salt rejection rate of the experimental group increased from 98.0% to 98.0%, and the pure water flux increased from 180 L / (m²) 2 ·h) optimized to 182L / (m 2 With a flux decay rate as low as 2.4% over 30 days, the overall separation performance and weather resistance achieve the optimal balance.

[0048] Comparative Example 1 A method for preparing a composite nanofiltration membrane includes the following steps: Step 1: Hydrophilic modification of the base membrane: At room temperature, a polyethersulfone membrane with a pore size of 0.1 μm and a porosity of 75% was immersed in an aqueous solution containing 2% polyvinyl alcohol (40000 Da) and 0.8% glutaraldehyde for 3 hours. After rinsing with deionized water until neutral, it was dried at a constant temperature of 60°C to obtain a hydrophilic modified porous support base membrane. Step 2: Prepare an aqueous solution: Use deionized water as a solvent to prepare an aqueous solution with a mass concentration of 0.5% piperazine. Step 3: Prepare the oil phase solution: Prepare a 0.3% (w / w) trimesoyl chloride oil phase solution using n-hexane as the solvent; Step 5: Preparation of the separation layer: Immerse the hydrophilic modified base membrane in the aqueous solution obtained in step 2 for 2 minutes, then remove the residual liquid on the surface and immerse it in the oil solution obtained in step 3 for interfacial polymerization for 60 seconds, and cure at room temperature for 8 minutes to obtain the composite nanofiltration membrane.

[0049] In Comparative Example 1, the obtained composite nanofiltration membrane was operated under standard conditions for 7 days, with a pure water flux of 190 L / (m²). 2 (h), salt rejection rate 72.3%, flux decline rate 32.6%, membrane layer showed obvious hydrolysis, swelling, cracking and damage, see Figure 3 .

[0050] Comparative Example 2 A method for preparing a composite nanofiltration membrane includes the following steps: Step 1: Hydrophilic modification of the base membrane: At room temperature, a polyethersulfone membrane with a pore size of 0.1 μm and a porosity of 75% was immersed in an aqueous solution containing 2% polyvinyl alcohol (50000 Da) and 0.8% glutaraldehyde for 3 hours. After rinsing with deionized water until neutral, it was dried at a constant temperature of 60°C to obtain a hydrophilic modified porous support base membrane. Step 2: Prepare an aqueous solution: Use deionized water as a solvent to prepare an aqueous solution with a mass concentration of 0.5% piperazine. Step 4: Prepare the oil phase solution: Prepare a 0.3% (w / w) 1,3,5-benzenetrisulfonyl chloride oil phase solution using n-hexane as the solvent; Step 5: Preparation of the separation layer: The hydrophilic modified base film is immersed in the aqueous solution obtained in step 3 for 2 min, then the surface liquid is removed and it is immersed in the oil solution obtained in step 4 for interfacial polymerization for 60 s, and cured at room temperature for 8 min to form a polysulfonamide-Tellerg base rigid functional separation layer. Step 6 Fluorosilane modification: Under constant temperature of 50℃, the membrane obtained in step 5 is crosslinked for 40 min using a 3% (v / v) tridefluorooctyltriethoxysilane solution. After washing with deionized water, it is dried and cured at 90℃ to obtain the composite nanofiltration membrane.

[0051] In Comparative Example 2, the obtained composite nanofiltration membrane was operated under standard conditions for 30 days, with a pure water flux of 182 L / (m²). 2 ·h), salt rejection rate 88.5%, flux decay rate 11.8%, molecular chains are prone to slippage at high temperature, structural stability decreases significantly.

[0052] Comparative Example 3 A method for preparing a composite nanofiltration membrane includes the following steps: Step 1: Preparation of rigid functional intermediate: Dissolve 8g of haloaniline in 10g of glacial acetic acid, add 4g of formaldehyde solution, and react at a constant temperature of 25℃ for 48h. After purification and vacuum drying, the rigid intermediate of the Tereg base is obtained. Step 2: Hydrophilic modification of the base membrane: At room temperature, a polyethersulfone membrane with a pore size of 0.1 μm and a porosity of 85% was immersed in an aqueous solution containing 2% polyvinyl alcohol (60000 Da) and 0.8% glutaraldehyde for 3 hours, rinsed with deionized water until neutral, and dried at 60°C to obtain a hydrophilic modified porous support base membrane. Step 3: Prepare an aqueous solution: Use deionized water as a solvent to prepare an aqueous solution containing 0.5% piperazine and 0.3% telage base intermediate. Step 4: Prepare the oil phase solution: Prepare a 0.3% (w / w) 1,3,5-benzenetrisulfonyl chloride oil phase solution using n-hexane as the solvent; Step 5: Preparation of the separation layer: Immerse the hydrophilic modified base membrane in the aqueous solution obtained in step 3 for 2 min, then remove the residual liquid on the surface and immerse it in the oil solution obtained in step 4 for interfacial polymerization for 60 s, and cure at room temperature for 8 min to form a composite nanofiltration membrane.

[0053] In Comparative Example 3, the obtained composite nanofiltration membrane was operated under standard conditions for 30 days, with a pure water flux of 186 L / (m²). 2 The salt rejection rate was 92.1%, the flux decay rate was 7.5%, the film surface had micro-corrosion defects, and the long-term stability was insufficient.

Claims

1. A method for preparing a highly stable, high-temperature resistant, and acid-resistant nanofiltration membrane, characterized in that, Includes the following steps: Step 1: Preparation of rigid functional intermediate: Dissolve haloaniline in glacial acetic acid, add formaldehyde, react under constant temperature and sealed conditions, and then purify and vacuum dry to obtain halophenyl teleg base rigid intermediate. Step 2: Preparation of the separation layer: The hydrophilic modified base film is sequentially immersed in an aqueous solution containing a halogenated phenyl telreg base rigid intermediate and an oil solution containing a sulfonyl chloride monomer. Interfacial polymerization is then performed, followed by room temperature curing to form a polysulfonamide-telreg base rigid functional separation layer. The mass fraction of the halogenated phenyl telreg base rigid intermediate in the aqueous solution is 0.2%-0.4%. Step 3 Fluorosilane modification: The membrane obtained in Step 2 is crosslinked at a constant temperature using a solution containing a fluorosilane coupling agent, and then cleaned, dried and cured to obtain a high-stability, high-temperature resistant, and acid-resistant composite nanofiltration membrane; the volume fraction of the fluorosilane coupling agent in the solution is 2%-4%.

2. The method for preparing a high-stability, high-temperature resistant, and acid-resistant nanofiltration membrane as described in claim 1, characterized in that, The hydrophilic modified base film is obtained by immersing the base film in an aqueous solution containing polyvinyl alcohol and glutaraldehyde.

3. The method for preparing a high-stability, high-temperature resistant, and acid-resistant nanofiltration membrane as described in claim 1, characterized in that, The aqueous solution containing the halogenated phenyl telrogal base rigid intermediate is composed of the following components by mass fraction: 0.3%-0.8% polyamine monomer, 0.2%-0.4% halogenated phenyl telrogal base rigid intermediate, and the balance being water; the oil phase solution containing the sulfonyl chloride monomer is composed of the sulfonyl chloride monomer and an organic solvent; the amount of the sulfonyl chloride monomer added is 0.2%-0.5% by mass fraction.

4. The method for preparing a high-stability, high-temperature resistant, and acid-resistant nanofiltration membrane as described in claim 3, characterized in that, The sulfonyl chloride monomer is any one or a combination of two of 1,3,5-benzenetrisulfonyl chloride and p-benzenedisulfonyl chloride.

5. The method for preparing a high-stability, high-temperature resistant, and acid-resistant nanofiltration membrane as described in claim 1, characterized in that, The fluorosilane coupling agent is any one or a combination of two of tridecylfluorooctyltriethoxysilane and trifluoropropyltrimethoxysilane.

6. The method for preparing a high-stability, high-temperature resistant, and acid-resistant nanofiltration membrane as described in claim 1, characterized in that, The volume fraction of the fluorosilane coupling agent in the solution is 3%.

7. The method for preparing a high-stability, high-temperature resistant, and acid-resistant nanofiltration membrane as described in claim 1, characterized in that, In step 3, the isothermal crosslinking reaction temperature is 45-55℃, and the crosslinking reaction time is 35-50 min.

8. A high-stability, high-temperature resistant, and acid-resistant composite nanofiltration membrane is prepared by the method described in any one of claims 1-7.

9. The application of the high-stability, high-temperature and acid-resistant composite nanofiltration membrane prepared by the preparation method according to any one of claims 1-7, or the high-stability, high-temperature and acid-resistant composite nanofiltration membrane according to claim 8, in the treatment of high-temperature acidic waste liquid in hydrometallurgy, purification of acidic materials in fine chemicals, purification of acidic mother liquor in the pharmaceutical industry, resource recovery of pickling and electroplating wastewater, and treatment of high-temperature acidic water in petrochemicals.