A Li-Salt-Assisted High-Temperature Reforming Single-Crystal Nanocubic SrTiO3 Photocatalyst, Its Preparation Method and Application
Li-SrTiO3 nanoparticles were prepared by Li salt-assisted high-temperature reforming, and the crystal structure was controlled to transform into a cubic phase. This solved the problem of lattice defects in SrTiO3 photocatalysts in the high-temperature molten salt method, and achieved high efficiency and stability in photocatalytic water splitting, making it suitable for large-scale applications.
Patent Information
- Application Number
- CN202611100141.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-23
- Publication Date
- 2026-11-17
AI Technical Summary
In the existing high-temperature molten salt method for preparing SrTiO3 photocatalysts, oxygen atoms in the crystal lattice are easily removed, leading to lattice defects and the formation of tetragonal phases, which affects the photocatalytic activity and stability of the material and limits its application in photocatalytic pure water splitting.
Li-SrTiO3 nanoparticles were prepared by using a Li-salt-assisted high-temperature reforming method, which involves adding Li salt and SrCl2 flux to control the transformation of the SrTiO3 crystal structure from the tetragonal phase to the cubic phase. RhCrOx and CoOOH were also doped as co-catalysts.
It achieves efficient pure water decomposition with high hydrogen and oxygen evolution rates, a hydrogen-to-oxygen ratio close to 2:1, good catalyst stability, is suitable for large-scale production, and has low raw material prices.
Smart Images

Figure CN123102377A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photocatalytic nanomaterial synthesis technology, and particularly relates to a method for reforming the cubic structure of single-crystal SrTiO3 nanoparticles. Specifically, it relates to a Li salt-assisted high-temperature reforming method for single-crystal cubic SrTiO3 nanoparticles photocatalyst and its preparation method and application. Background Technology
[0002] Semiconductor photocatalysis technology can drive a variety of challenging chemical reactions under mild conditions, such as the degradation of organic pollutants, photocatalytic synthesis of ammonia, synthesis of chemical raw materials like methanol, and photocatalytic water splitting. Among these, photocatalytic water splitting technology can convert solar energy into storable hydrogen energy. Due to hydrogen's high calorific value and environmental friendliness, it is considered an ideal clean energy alternative. Theoretically, 2 mol of water splitting can produce 2 mol of hydrogen and 1 mol of oxygen. If light energy can be efficiently utilized and converted into hydrogen energy, photocatalytic pure water splitting technology has the potential to replace traditional fossil fuel consumption systems, making this field a current research hotspot. However, the water splitting reaction is thermodynamically a "climbing" process, and its high energy consumption limits the large-scale practical application of water splitting hydrogen production strategies.
[0003] Since Fujishima and Honda achieved photoelectrochemical water splitting using a rutile TiO2 anode and a platinum cathode in 1972, researchers have been dedicated to constructing efficient heterogeneous photocatalytic systems. To date, numerous semiconductor photocatalysts have been reported, including sulfides (such as CdS), nitrides (such as Ta3N5), and metal oxides (such as TiO2). SrTiO3, a semiconductor material with a simple cubic perovskite structure, exhibits n-type conductivity after reduction, with a band gap of 3.2 eV. Early studies have confirmed that SrTiO3 can be used as a photoelectrode for hydrogen production through water electrolysis. In recent years, SrTiO3-based semiconductor materials have been further demonstrated to convert solar energy into chemical energy without an external bias, achieving pure water splitting. Nevertheless, how to effectively excite photogenerated carriers and further improve carrier separation and migration efficiency remains a key focus and challenge in this field.
[0004] Currently, the high-temperature molten salt method for preparing highly crystalline SrTiO3-based semiconductor particles and their application in photocatalytic whole-body water splitting has become a widely studied technical route. Using SrCl2 as a flux, SrTiO3 single-crystal nanoparticles with a standard cubic phase structure can be synthesized. After supporting hydrogen evolution and oxygen evolution co-catalysts, their photocatalytic water splitting efficiency is significantly improved. However, this process still has technical drawbacks in practical applications: during the high-temperature molten salt reaction, oxygen atoms in the SrTiO3 lattice are easily removed by heat, leading to lattice defects and inducing abnormal grain growth. These problems can disrupt the stability of the cubic phase structure of SrTiO3, inducing the formation of tetragonal SrTiO3. Since the tetragonal phase structure significantly reduces the photocatalytic activity and stability of SrTiO3-based materials, this severely restricts their practical application in photocatalytic pure water splitting.
[0005] Therefore, how to regulate the grain growth of SrTiO3, avoid the formation of tetragonal phase, and promote the growth of cubic single crystal particles is of great significance for maintaining the efficient and stable photocatalytic water splitting performance of SrTiO3 semiconductor materials. Summary of the Invention
[0006] To address the shortcomings of existing technologies, this invention provides a Li-salt-assisted high-temperature reforming single-crystal nano-cubic SrTiO3 photocatalyst, its preparation method, and its application. By adding Li salt at high temperature, the tetragonal phase SrTiO3 is transformed into cubic phase SrTiO3, resulting in single-crystal nano-SrTiO3 with excellent catalytic activity and stability. Moreover, the preparation process is simple, the reaction conditions are mild, and the reagents used are inexpensive.
[0007] To achieve the above objectives, the present invention adopts the following technical solution: A method for preparing a Li salt-assisted high-temperature reforming single-crystal nanocubic SrTiO3 photocatalyst includes the following steps: Step 1: The Li-containing compound is uniformly mixed with SrTiO3 nanoparticles to obtain a mixture; Step 2: After uniformly mixing the mixture from Step 1 with SrCl2, keep it at 800-1300 ℃ for 4-12 hours, then wash to remove excess SrCl2, and dry to obtain Li-SrTiO3 nanoparticles. Step 3: Li-SrTiO3 nanoparticles are uniformly mixed with NaRhCl6 and Cr(NO3)3 for 1-5 hours, and then kept at 200-800℃ for 1-5 hours to obtain RhCrO3. x / Li-SrTiO3 nanoparticles; Step 4, RhCrO xLi-SrTiO3 nanoparticles were dispersed in water, then cobalt nitrate hexahydrate was added. After irradiation with a 300W xenon lamp for 1-5 hours, the mixture was filtered, washed, and dried to obtain RhCrO. x / Li-SrTiO3 / CoOOH nanocomposite photocatalyst.
[0008] Preferably, the uniform mixing method in step 1 is ball milling, and the mixing time is 1-24 hours.
[0009] Preferably, the Li-containing compound in step 1 is one or more of lithium carbonate, lithium acetate, lithium nitrate, and lithium chloride.
[0010] Preferably, the molar ratio of Li to SrTiO3 in the Li-containing compound in step 1 is (1-3):100.
[0011] Preferably, in step 3, the amounts of NaRhCl6 and Cr(NO3)3 added are calculated as Rh elements and Cr elements, respectively, accounting for 0.9-1.1 wt% and 0.3-0.5 wt% of the mass of SrTiO3; in step 4, the amount of Co(NO3)2·6H2O added is calculated as Co elements, accounting for 0.3-0.5 wt% of the mass of SrTiO3.
[0012] Single-crystal nanocubic SrTiO3 photocatalysts prepared based on any of the methods described above.
[0013] Preferably, the photocatalyst is Li alkali metal ion-doped cubic SrTiO3 single-crystal nanoparticles. The nanoparticles have a cubic morphology and a particle size of 100-500 nm. The X-ray diffraction pattern of the nanoparticles corresponds to cubic SrTiO3 (JCPDS No. 35-0734), and RhCrO is supported on the surface of the nanoparticles. x CoOOH is used as a co-catalyst.
[0014] The above-mentioned single-crystal nanocubic phase SrTiO3 photocatalyst is used in photocatalytic water splitting.
[0015] Preferably, the photocatalytic water splitting is a photocatalytic whole-body water splitting.
[0016] Preferably, the application is carried out under ultraviolet-visible full-spectrum irradiation with pure water as the reaction medium.
[0017] Beneficial effects: Compared with existing technologies, the present invention provides a Li salt-assisted high-temperature reforming single-crystal nanocubic SrTiO3 photocatalyst, its preparation method, and its application, which have the following advantages: First, this invention achieves a controllable transformation of the SrTiO3 crystal structure from a tetragonal phase to a cubic phase by introducing Li salt and SrCl2 flux together for high-temperature heat treatment. When the molar proportion of Li is 1%-3%, the resulting SrTiO3 has a standard cubic phase crystal structure, while the pure phase SrTiO3 without added Li salt and the sample with a Li molar proportion of 5% both have a tetragonal phase structure. This indicates that appropriate Li doping is the key to inducing the formation of the cubic phase. The RhCrO prepared by this invention x The / Li-SrTiO3 / CoOOH nanocomposite photocatalyst can achieve the overall decomposition of pure water under UV-Vis full-spectrum irradiation, wherein RhCrO x The average hydrogen evolution rate of / 1%Li-SrTiO3 / CoOOH reached 2.26 mmol / h, the average oxygen evolution rate reached 1.11 mmol / h, the hydrogen-oxygen ratio was close to 2:1, and the catalyst maintained good catalytic activity after recycling. The Li-SrTiO3 nanoparticles obtained by this invention have a regular cubic morphology with a size of 400~600 nm and single crystal characteristics; This invention employs a high-temperature molten salt method combined with Li salt doping. The process is simple, and the raw materials used, such as SrCl2 and Li salt, are inexpensive, making it suitable for large-scale production. Attached Figure Description
[0018] Figure 1 These are X-ray diffraction patterns of the catalysts prepared in Examples 1-3 and Comparative Examples 1 and 2 of this invention; Figure 2 This is a scanning electron microscope image of the 1% Li-SrTiO3 catalyst prepared in Example 1 of this invention; Figure 3 The RhCrO prepared in Examples 1-3 and Comparative Examples 1 and 2 of this invention. x Photocatalytic activity diagram of Li-SrTiO3 / CoOOH for pure water splitting; Figure 4 The RhCrO prepared in Example 1 of this invention x Stability diagram of pure water decomposition cycle under photocatalysis of / 1%Li-SrTiO3 / CoOOH. Detailed Implementation
[0019] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments: Example 1
[0020] A method for preparing a Li salt-assisted high-temperature reforming single-crystal nanocubic SrTiO3 photocatalyst includes the following steps: 0.005 mol of lithium carbonate and 1 mol of SrTiO3 were weighed separately and ground together in an agate mortar for 1 hour. The ground mixture was then placed in a ball mill and milled at 4000 rpm for 24 hours. 1 mol of SrCl2 was then added and milled for another hour. The milled mixture was sieved and placed in a muffle furnace at 1000 °C for 8 hours. After removal, it was washed with a large amount of deionized water and then dried overnight at 80 °C in a drying oven to obtain 1% Li-SrTiO3 nanocatalyst material.
[0021] 0.5 g of 1% Li-SrTiO3 nanoparticles were mixed with 18.7 mg of NaRhCl6 and 11.4 mg of Cr(NO3)3, ball-milled for 1 hour, calcined in air at 400 °C for 3 hours, dispersed in 100 mL of water, and 7.92 mg of Co(NO3)2·6H2O was added. After irradiation with a 300 W xenon lamp for 5 hours, the mixture was filtered, washed, and dried to obtain RhCrO3 nanoparticles. x / 1%Li-SrTiO3 / CoOOH nanocomposite photocatalyst.
[0022] RhCrO prepared by the above method x Scanning electron microscopy image of / 1%Li-SrTiO3 / CoOOH nanocomposite photocatalyst as shown below Figure 2 As shown, the size of 1% Li-SrTiO3 nanoparticles is 100-500 nm, and the X-ray diffraction pattern is as follows. Figure 1 As shown, the crystal form is a cubic phase structure (JCPDS No. 35-0734). Figure 4 Its performance was tested for cycle stability. After 6 cycles, its performance showed almost no decline, indicating that the catalyst has good stability.
[0023] Example 2
[0024] A method for preparing a Li salt-assisted high-temperature reforming single-crystal nanocubic SrTiO3 photocatalyst includes the following steps: 0.010 mol of lithium carbonate and 1 mol of SrTiO3 were weighed separately and mixed and ground in an agate mortar for 1 h. The ground mixture was then placed in a ball mill and ball-milled at 4000 rpm for 24 h. Then, 1 mol of SrCl2 was added and ball-milled for another 1 h. The ball-milled mixture was sieved and placed in a muffle furnace and kept at 1000 ℃ for 8 h. After removal, it was washed with a large amount of deionized water by vacuum filtration, and then dried overnight in a drying oven at 80 ℃ to obtain 2% Li-SrTiO3 nanocatalyst material.
[0025] 0.5 g of 2% Li-SrTiO3 nanoparticles were mixed with 18.7 mg of NaRhCl6 and 11.4 mg of Cr(NO3)3, ball-milled for 1 hour, calcined in air at 400 °C for 3 hours, dispersed in 100 mL of water, and 7.92 mg of Co(NO3)2·6H2O was added. After irradiation with a 300 W xenon lamp for 5 hours, the mixture was filtered, washed, and dried to obtain RhCrO3 nanoparticles. x / 2%Li-SrTiO3 / CoOOH nanocomposite photocatalyst.
[0026] The X-ray diffraction pattern of the 2% Li-SrTiO3 nanocatalyst material obtained by the above method is shown in the figure. Figure 1 As shown, its crystal form belongs to the cubic phase crystal structure (JCPDS No. 35-0734).
[0027] Example 3
[0028] A method for preparing a Li salt-assisted high-temperature reforming single-crystal nanocubic SrTiO3 photocatalyst includes the following steps: 0.015 mol of lithium carbonate and 1 mol of SrTiO3 were weighed separately and mixed and ground in an agate mortar for 1 h. The ground mixture was then placed in a ball mill and ball-milled at 4000 rpm for 24 h. Then, 1 mol of SrCl2 was added and ball-milled for another 1 h. The ball-milled mixture was sieved and placed in a muffle furnace and kept at 1000 ℃ for 8 h. After removal, it was washed with a large amount of deionized water by vacuum filtration, and then dried overnight in a drying oven at 80 ℃ to obtain 3% Li-SrTiO3 nanocatalyst material.
[0029] 0.5 g of 3% Li-SrTiO3 nanoparticles were mixed with 18.7 mg of NaRhCl6 and 11.4 mg of Cr(NO3)3, ball-milled for 1 hour, calcined in air at 400 °C for 3 hours, dispersed in 100 mL of water, and 7.92 mg of Co(NO3)2·6H2O was added. After irradiation with a 300 W xenon lamp for 5 hours, the mixture was filtered, washed, and dried to obtain RhCrO3 nanoparticles. x / 3%Li-SrTiO3 / CoOOH nanocomposite photocatalyst.
[0030] The X-ray diffraction pattern of the 3% Li-SrTiO3 nanocatalyst material obtained by the above method is shown in the figure. Figure 1 As shown, its crystal form belongs to the cubic phase crystal structure (JCPDS No. 35-0734).
[0031] Comparative Example 1 The preparation of pure-phase SrTiO3 includes the following steps: Weigh out 1 mol of SrTiO3 and grind it in an agate mortar for 1 h. Place the ground mixture in a ball mill and ball mill at 4000 rpm for 24 h. Then add 1 mol of SrCl2 and continue ball milling for 1 h. Separate the ball-milled mixture by sieving and place it in a muffle furnace, where it is kept at 1000 ℃ for 8 h. After removal, filter and wash with a large amount of deionized water, and then place the material in a drying oven at 80 ℃ overnight to dry, thus obtaining pure-phase SrTiO3 nanocatalyst material.
[0032] 0.5 g of SrTiO3 nanoparticles were mixed with 18.7 mg of NaRhCl6 and 11.4 mg of Cr(NO3)3, ball-milled for 1 hour, calcined in air at 400 °C for 3 hours, dispersed in 100 mL of water, and 7.92 mg of Co(NO3)2·6H2O was added. After irradiation with a 300 W xenon lamp for 5 hours, the mixture was filtered, washed, and dried to obtain RhCrO3 nanoparticles. x / SrTiO3 / CoOOH nanocomposite photocatalyst.
[0033] The XRD pattern of the pure-phase SrTiO3 nanocatalyst material obtained by the above method is shown below. Figure 1 As shown, its crystal form belongs to the tetragonal phase crystal structure (JCPDS No. 47-0228).
[0034] Comparative Example 2 A method for preparing a Li salt-assisted high-temperature reforming single-crystal nanocubic SrTiO3 photocatalyst includes the following steps: 0.025 mol of lithium carbonate and 0.95 mol of SrTiO3 were weighed separately and mixed and ground in an agate mortar for 1 h. The ground mixture was then placed in a ball mill and ball-milled at 4000 rpm for 24 h. Then, 1 mol of SrCl2 was added and ball-milled for another 1 h. The ball-milled mixture was sieved to separate the contents and placed in a muffle furnace and kept at 1000 ℃ for 8 hours. After removal, the material was filtered and washed with a large amount of deionized water, and then dried overnight at 80 °C in a drying oven to obtain 5% Li-SrTiO3 nanocatalyst material. 0.5 g of 5% Li-SrTiO3 nanoparticles were taken, and 18.7 mg of NaRhCl6 and 11.4 mg of Cr(NO3)3 were added. The mixture was ball-milled for 1 hour, calcined in air at 400 °C for 3 hours, dispersed in 100 mL of water, and 7.92 mg of Co(NO3)2·6H2O was added. After irradiation with a 300W xenon lamp for 5 hours, the mixture was filtered, washed, and dried to obtain RhCrO3. x / 5%Li-SrTiO3 / CoOOH nanocomposite photocatalyst.
[0035] The X-ray diffraction pattern of the 5% Li-SrTiO3 nanocatalyst material obtained by the above method is shown in the figure. Figure 1 As shown, its crystal form belongs to the tetragonal phase crystal structure (JCPDS No. 47-0228), indicating that an excess of Li alkali metal ions is also not conducive to the formation of SrTiO3 cubic phase single crystals.
[0036] RhCrO₂ with different Li metal ion molar ratios prepared in Examples 1-3 and Comparative Examples 1-2 above x The / Li-SrTiO3 / CoOOH nanocomposite photocatalyst was applied to the photocatalytic water splitting. The photocatalytic water splitting performance test was carried out in a closed quartz reactor. The catalyst dosage was 40 mg, which was uniformly dispersed in 80 mL of pure water and continuously stirred. The specific instruments and test methods used for the test can be referred to Advanced Functional Materials, 2022, 33(24), 2215242 (Figure S2 in the article). Before the reaction, the system was degassed under vacuum. A 300W xenon lamp (ultraviolet-visible full spectrum) was used as the irradiation source. The average light intensity of the light source was measured to be 1184 mW·cm according to the test method of Angewandte Chemie International Edition 2023, 63(30), e202405807 (Figure S39). -2 Gas production samples were taken every 0.5 hours and analyzed using a gas chromatograph.
[0037] The results are as follows Figure 3 As shown. RhCrO x The 1%Li-SrTiO3 / CoOOH nanocatalyst exhibits an average hydrogen evolution rate of 2.26 mmol / h and an oxygen evolution rate of 1.11 mmol / h, with a hydrogen-to-oxygen ratio close to 2:1, demonstrating good stability.
[0038] The above description is only a preferred embodiment of the present invention. It should be noted that those skilled in the art can make several improvements without departing from the principle of the present invention, and these improvements should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a Li salt-assisted high-temperature reforming single-crystal nanocubic SrTiO3 photocatalyst, characterized in that, Includes the following steps: Step 1: The Li-containing compound is uniformly mixed with SrTiO3 nanoparticles to obtain a mixture; Step 2: After uniformly mixing the mixture from Step 1 with SrCl2, keep it at 800-1300 ℃ for 4-12 hours, then wash to remove excess SrCl2, and dry to obtain Li-SrTiO3 nanoparticles. Step 3: Li-SrTiO3 nanoparticles are uniformly mixed with NaRhCl6 and Cr(NO3)3 for 1-5 hours, and then kept at 200-800 ℃ for 1-5 hours to obtain RhCrO3. x / Li-SrTiO3 nanoparticles; Step 4, RhCrO x Li-SrTiO3 nanoparticles were dispersed in water, then cobalt nitrate hexahydrate was added. After irradiation with a 300W xenon lamp for 1-5 hours, the mixture was filtered, washed, and dried to obtain RhCrO. x / Li-SrTiO3 / CoOOH nanocomposite photocatalyst.
2. The preparation method according to claim 1, characterized in that, The uniform mixing method described in step 1 is ball milling, and the mixing time is 1-24 hours.
3. The preparation method according to claim 1, characterized in that, The Li-containing compound mentioned in step 1 is one or more of lithium carbonate, lithium acetate, lithium nitrate, and lithium chloride.
4. The preparation method according to claim 1, characterized in that, The molar ratio of Li to SrTiO3 in the Li-containing compound mentioned in step 1 is (1-3):
100.
5. The preparation method according to claim 1, characterized in that, In step 3, the amounts of NaRhCl6 and Cr(NO3)3 added are calculated as Rh elements and Cr elements, respectively, accounting for 0.9-1.1 wt% and 0.3-0.5 wt% of the mass of SrTiO3; in step 4, the amount of Co(NO3)2·6H2O added is calculated as Co elements, accounting for 0.3-0.5 wt% of the mass of SrTiO3.
6. A single-crystal nanocubic SrTiO3 photocatalyst prepared by the method according to any one of claims 1-5.
7. The single-crystal nanocubic SrTiO3 photocatalyst according to claim 6, characterized in that, The photocatalyst is Li alkali metal ion-doped cubic SrTiO3 single-crystal nanoparticles. The nanoparticles have a cubic morphology and a particle size of 100-500 nm. The X-ray diffraction pattern of the nanoparticles corresponds to cubic SrTiO3 (JCPDS NO. 35-0734), and RhCrO is supported on the surface of the nanoparticles. x CoOOH is used as a co-catalyst.
8. The application of the single-crystal nanocubic phase SrTiO3 photocatalyst according to claim 6 or 7 in photocatalytic water splitting.
9. The application according to claim 8, characterized in that, The photocatalytic water splitting is a photocatalytic overall water splitting.
10. The application according to claim 8, characterized in that, The application is carried out under ultraviolet-visible full-spectrum irradiation with pure water as the reaction medium.