A High-Efficiency Manufacturing Process for 6082 Aluminum Alloy Automotive Anti-collision Beams
By using synchronously calibrated samples in the same batch and the correction coefficient Kh, the problem of accurately predicting the changes in microstructure of 6082 aluminum alloy automotive anti-collision beams during natural aging and tensile bending was solved, enabling efficient and uniform anti-collision beam manufacturing, simplifying the production process and reducing costs.
Patent Information
- Application Number
- CN202611524492.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies cannot accurately predict the complex microstructure changes that occur in 6082 aluminum alloy automotive anti-collision beams during natural aging and tensile bending forming processes, resulting in inaccurate artificial aging responses, affecting the final strength and plasticity. Furthermore, small samples cannot reproduce the peak deformation of actual components.
Using samples calibrated simultaneously in the same batch, the natural aging and deformation state were reproduced physically. The bending and tension history was corrected using a correction factor Kh. Combined with the overall artificial aging parameters, the accurate response of the coupling effect between the natural aging and pre-deformation of the anti-collision beam was ensured.
This technology enables the efficient manufacturing of 6082 aluminum alloy automotive anti-collision beams, ensuring uniformity of microstructure and properties, simplifying the production process, reducing production costs, and improving the accuracy of artificial aging parameters and production efficiency.
Smart Images

Figure CN123102778A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of aluminum alloy plastic forming and heat treatment technology, specifically to an efficient manufacturing process for 6082 aluminum alloy automotive anti-collision beams. Background Technology
[0002] 6082 aluminum alloy belongs to the Al-Mg-Si system and is a heat-treatable alloy, commonly used in extruded profile components such as automotive crash beams. To balance formability and final strength, the production process typically involves extrusion, online quenching, natural aging to the T4 state, stretch bending, and artificial aging.
[0003] After online quenching, the matrix of 6082 profile is in a supersaturated solid solution state containing Mg and Si solute atoms and quenching vacancies. During the inspection, storage, transportation, and waiting processes after quenching and before bending, Mg and Si solute atoms continue to migrate and aggregate with the assistance of vacancies, forming Mg-Si atomic clusters and early precipitation structures. Changes in natural aging time and ambient temperature will alter the distribution of solutes and vacancy states that can participate in subsequent precipitation before the start of artificial aging; fluctuations in the composition of different extrusion batches, extrusion exit temperature, and quenching cooling conditions will further alter this initial microstructure.
[0004] When T4 profiles are stretched and bent, the outer, inner, and neutral layers exhibit different plastic strains. Plastic deformation introduces dislocations within the material, creating variations in dislocation density and residual stress along the cross-section. Dislocations provide heterogeneous nucleation sites for subsequent precipitates and alter solute diffusion paths, precipitate types, and their size and distribution. The influence of bending strain on artificial aging depends on the pre-formed naturally aged microstructure. Whether naturally aged atomic clusters can continue to transform during artificial aging is also affected by the state of bending dislocations. Therefore, the same bending strain may produce different artificial aging responses under different natural aging histories, and different bending strains under the same natural aging history may also produce different strengthening results. Mechanistically, natural aging has already consumed some supersaturated solute and quenched vacancies, forming Mg-Si clusters with varying stability. Subsequent stretching dislocations provide heterogeneous nucleation sites and alter the pathways of cluster dissolution, transformation, and solute segregation towards dislocations. The two states together determine the number of solute-vacancy combinations and nucleation sites available in the early stage of artificial aging. Therefore, the hardening increment of artificial aging has loading order dependence and nonlinearity. The sum of the measured "natural aging increment" and "pre-deformation increment" cannot accurately represent the net response when the two exist simultaneously, and cannot be simply superimposed as two independent correction quantities.
[0005] Directly calculating the aforementioned coupling effects requires obtaining or establishing parameters such as actual alloy composition, quenching vacancy concentration, natural aging cluster state, local plastic strain and dislocation density in the bending region, and precipitation kinetics, which are difficult to accurately measure individually on-site. While using calibration samples from the same batch can bypass these microstructure evolution calculations, it introduces a unique problem that only arises when "small samples reproduce actual components": industrial tensile bending typically involves axial tension, over-bending loading relative to the finished product shape, and unloading springback. The maximum loading state determines the degree of plastic strain and dislocation introduction, while product drawings or finished product testing provide the final shape after unloading. If the radius of the small sample is directly calculated from the final curvature, even if the small sample corresponds to the final curvature of the crash beam, the peak deformation experienced by the crash beam may be underestimated. Therefore, it is necessary to correct the pre-deformation degree of the calibration sample using loading-unloading parameters available on-site. Summary of the Invention
[0006] In view of this, the present invention provides an efficient manufacturing process for 6082 aluminum alloy automotive anti-collision beams, replacing the separate modeling and superimposed prediction of cluster density, vacancy concentration, dislocation density, and precipitation kinetic coupling relationship with solid reproduction and measured response. Artificial aging parameters for the entire component applicable to the current material batch and target bending state are determined.
[0007] The technical solution of this invention is implemented as follows: This invention provides an efficient manufacturing process for 6082 aluminum alloy automotive anti-collision beams, including the following steps: S1. After the 6082 aluminum alloy anti-collision beam profile is extruded, quenched and straightened, a reference sample and a synchronous calibration sample that are stored at the same time and in the same environment as the anti-collision beam profile to be formed and have undergone the same natural aging process are cut from the same extrusion and quenching batch. S2. Perform overall stretch bending of the profile to be formed, and obtain the radius of curvature R of the neutral layer when the bending moment in the deformation zone of the anti-collision beam reaches its peak during the stretch bending process. L After the external force is completely removed, the final neutral layer curvature radius R of the anti-collision beam reaches a stable state. U The true strain ε of axial tension applied during bending deformation t And the normal distance y from the outermost edge of the profile section to the neutral layer max And according to R L R U ε t and y max Determine the bending process correction factor K h ; S3, the bending process correction coefficient K obtained in step S2. h Corrected by R U Based on the determined true strain of the outer layer bending, the corrected target bending radius R of the synchronously calibrated specimen is determined. s,cPre-deform the synchronous calibration specimens to obtain calibration specimens with the coupled influence of natural aging and bending state. S4. For the calibration samples obtained in step S3, implement the preset candidate artificial aging system, measure the hardness of the calibration samples corresponding to each candidate artificial aging system, use the hardness of the calibration samples to characterize the artificial aging response after coupling the natural aging state and the pre-deformation state, and determine the overall artificial aging parameters of the current batch of anti-collision beams based on the artificial aging response. S5. Artificially age the current batch of anti-collision beam profiles to be artificially aged according to the overall artificial aging parameters determined in step S4, and obtain 6082 aluminum alloy automotive anti-collision beam components after cooling.
[0008] Reference samples and synchronous calibration samples were taken from the same extrusion and quenching batches as the anti-collision beam profiles. The calibration samples and the profiles to be formed underwent the natural aging process from the end of quenching to the start of bending forming, so as to reproduce the solute atoms, quenching vacancies and natural aging clusters of the actual batch. In step S2, R U Through ε max Indirectly affecting the bending process correction factor K h , ε max The maximum true strain of the outer layer bending when the anti-collision beam reaches a stable state after the external force is completely removed is determined according to equation (1): .
[0009] Based on the above technical solution, preferably, in step S2, the bending process correction coefficient K h Determine according to formula (2): .
[0010] In the formula, R L It can be obtained from the effective radius of the bending die, the contour scan under loading, or the equipment displacement-curvature correspondence after the first piece calibration; ε t It can be obtained from the change in neutral layer gauge length, surface mesh or DIC strain measurement, or from the effective stroke of the clamping end after deducting rigid body displacement; R U The profile was obtained by scanning the finished product after the external force was completely removed and a stable state was reached. The stable state was defined as a relative change of no more than 0.1% in the neutral layer curvature radius obtained from two adjacent profile measurements taken 5 minutes apart. max Obtained from profile cross-section drawings or cross-section scanning.
[0011] The molecule ε of equation (2) b,p =ε t +ln[(R L +y max ) / R L] represents the peak true strain at the surface of the anti-collision beam deformation zone under maximum loading conditions, formed by the combined axial tension and bending; denominator ε max This represents the true surface bending strain calculated solely from the final geometric curvature of the crash beam after unloading by external forces. For crash beams with multiple bending segments, K is calculated separately for each segment. h And with the maximum ε in the key bending area b,p As a benchmark target.
[0012] K h Instead of empirical fitting coefficients for precipitation kinetics, K is a geometric-process correction consisting of maximum loading curvature, curvature after unloading, and axial tensile strain; when there is no axial tension and bending and springback are negligible, K... h It approaches 1. This retains the advantage of physical calibration in bypassing the difficulties of two-factor coupled calculations, while reducing the error of small-sized calibration specimens underestimating the actual peak deformation because they only replicate the final shape.
[0013] Based on the above technical solution, preferably, in step S3, the target bending radius R is corrected. s,c Determine according to formula (3): .
[0014] Among them, y s To simultaneously calibrate the normal distance from the outermost part of the sample to its neutral layer.
[0015] Using a radius of R s,c The bending mold is used to pre-deform the synchronous calibration sample. The difference between the peak surface strain of the synchronous calibration sample and the critical bending area of the anti-collision beam does not exceed 0.3%, so that the calibration sample is closer to the peak plastic deformation and dislocation state formed by the anti-collision beam under the combined action of bending, tension and springback.
[0016] If we ignore the bending process, let K h =1, then equation (3) degenerates into the original formula: ; When ε t Approaching 0 and R L Approaching R U At that time, K h As K approaches 1, the improved formula naturally degenerates into the original formula; when there is axial tension or bending springback, K... h This is used to compensate for the underestimation of peak deformation caused by calculating the final curvature under steady-state conditions only after unloading the external force. The small-sized synchronous calibration specimen does not need to replicate the complete multi-cavity section of the anti-collision beam. Instead, it incorporates the initial microstructure formed by natural aging and the dislocation state formed by tension and bending into the subsequent artificial aging process through synchronous natural aging and pre-deformation corrected by the loading history.
[0017] Based on the above technical solutions, preferably, in step S4, there are no fewer than three candidates for each batch of artificial aging systems, all using the same artificial aging temperature T. a With different time limits, the time difference between two adjacent candidates in the same batch is 10 to 45 minutes.
[0018] Based on the above technical solutions, the preferred artificial aging temperature T is... a The temperature is 180–205℃, and the duration is 20–180 minutes.
[0019] Based on the above technical solution, preferably, in step S4, four coupled synchronous calibration samples are placed in a small air-circulating furnace at 190±3℃. After the sample center temperature reaches 185℃, they are held at that temperature for 45min, 60min, 75min, and 90min respectively. After each candidate time treatment, the samples are cooled to room temperature, and the hardness H is measured under the same hardness standard, load, holding time, and measurement point rules. i .
[0020] Based on the above technical solution, preferably, in step S4, using the hardness of the T6 state reference sample from the same batch as a benchmark, the hardness retention ratio λ corresponding to the i-th candidate aging regime is evaluated. i and the hardness increment ΔH of adjacent candidate times i Determine according to equations (4) and (5) respectively: ; Among them, H i H represents the hardness of the calibration sample after processing at the i-th candidate time. T6 The hardness of the reference sample in T6 condition from the same batch; H i+1 The hardness of the calibration sample after processing at the (i+1)th candidate time; when 0.97 ≤ λ i ≤1.03 and ΔH i When the value is ≤2.0HV, the corresponding candidate time will be determined as the qualified insulation time.
[0021] Based on the above technical solutions, the optimal shortest acceptable heat preservation time t is selected. * You can select according to formula (6): ; When using formula (6) to optimize production efficiency, candidate times are evaluated sequentially from shortest to longest. If none of the candidate times except the maximum candidate time meet the above conditions, the maximum candidate time is taken as the upper limit candidate point and additional in-furnace verification is added; if the hardness retention ratio after the maximum candidate time treatment is still less than 0.97, the batch will not directly adopt the short-time aging system of this invention, but will be transferred to conventional aging or re-evaluated. In the specific calibration combination of 190±3℃, 90min is the maximum candidate time.
[0022] To quickly determine the natural aging hardening potential of a material before candidate sample calibration, the pre-forming hardness H0 of the profile to be formed before entering the bending process and before artificial aging, and the reference hardness H of the same batch of samples after 24 hours of natural aging can be measured. 24 and the hardness H of the T6 state reference sample from the same batch T6 When the predetermined forming time is more than 24 hours earlier and the measurement regime is consistent, H0 < H is usually satisfied. 24 <H T6 Calculate the natural age hardening potential index S according to formula (7):
[0023] ; Based on the above technical solutions, preferably, when 0 < S < 1, S represents the proportion of the hardness increment from the forming point to the 24-hour natural aging period to the total hardening increment from the forming point to the T6 reference state; the larger S is, the greater the hardness difference between the pre-forming state and the 24-hour natural aging state. S is only used for pre-forming screening and does not replace batch calibration of coupled state calibration samples. When H0 ≥ H 24 H0≥H T6 When S≤0 or S≥1, the aging parameters should not be determined directly based on this. The sampling time, sample source, hardness measurement point and reference heat treatment should be verified, and batch calibration should be carried out again if necessary.
[0024] Based on the above technical solutions, the preferred method is to use a synchronous calibration sample with a length of 80–150 mm and a width of 15–30 mm.
[0025] Based on the above technical solution, preferably, in step S5, a sample with the same material batch, natural aging history, and equivalent pre-deformation state as the synchronous calibration sample is used as the furnace-loaded verification sample, and is loaded into the furnace together with the anti-collision beam profile to be artificially aged, with the artificial aging set temperature being T. a The temperature at the center of the sample reached T. a The determined heat preservation time is calculated starting at -5℃. After the heat preservation is completed, the anti-collision beam profile is cooled to obtain an aluminum alloy automotive anti-collision beam.
[0026] Based on the above technical solutions, the preferred method is to measure the hardness H of the furnace-tested sample after the artificial aging process. w When H w H T6 When <0.97, the anti-collision beam and the furnace-tested sample are subjected to a set temperature T. a Next, supplement with artificial aging time of 10-30 minutes.
[0027] Based on the above technical solutions, the preferred method is air cooling after the artificial aging process, cooling the temperature to ≤60℃.
[0028] The beneficial effects of the efficient manufacturing process for the 6082 aluminum alloy automotive anti-collision beam of the present invention are as follows: (1) The composition, quenching state and solute, vacancy and cluster state formed by natural aging of the current batch of materials are reproduced by using synchronous calibration samples of the same batch; the net response of artificial aging after coupling of natural aging and deformation state is characterized by solid samples; it is not necessary to measure cluster density, vacancy concentration and dislocation density on the production site, nor is it necessary to establish a complex coupled precipitation kinetic model.
[0029] (2) Introduce correction coefficient K h The maximum loading curvature, the curvature after unloading the external force, and the axial tensile strain are combined into a measurable process correction amount to compensate for the peak strain deviation caused by the small sample being pre-deformed only according to the final geometry of the finished product. When no correction is needed, it can degenerate back to the original formula. The corrected pre-deformation further reproduces the plastic strain and dislocation state in the key bending area of the anti-collision beam.
[0030] (3) The overall aging process is adopted. The entire anti-collision beam is artificially aged at a uniform temperature and time, which not only ensures the high uniformity of the anti-collision beam's structural properties, but also greatly reduces the requirements for equipment, making the process window wide and the operation simple, effectively simplifying the production process and reducing production costs. Attached Figure Description
[0031] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0032] Figure 1 This is a flowchart of the efficient manufacturing process of the 6082 aluminum alloy automotive anti-collision beam of the present invention; Figure 2 This is a schematic diagram illustrating the relationship between the bending loading process and the correction radius of the calibrated specimen; Figure 3 This is a graph showing the relationship between candidate holding time and hardness retention ratio for candidate times under different artificial aging temperatures and candidate time intervals in Examples 1-3. Detailed Implementation
[0033] The technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention. In the following embodiments, unless otherwise specified, the materials used are all commercially available materials, and the testing means and methods used are all conventional testing means and methods in the art.
[0034] Example 1 This embodiment provides a crash beam manufactured using an efficient manufacturing process for 6082 aluminum alloy automotive crash beams employing an improved formula (3). The beam is prepared according to the following steps: 1) After homogenization, 6082 aluminum alloy ingots are extruded into multi-cavity anti-collision beam profiles at 520℃. After demolding, they are quenched with water mist and then stretched and straightened by 1% to obtain the anti-collision beam profiles.
[0035] 2) Select a complete profile from this batch as the first calibration beam in the bending process. Also select a reference sample and a synchronous calibration sample from the non-welded wall panel area of the same batch of profiles. The reference sample and the synchronous calibration sample are 150mm long and 30mm wide, and the thickness is maintained at the profile extrusion wall thickness in step 1).
[0036] 3) Take a reference sample and measure H after quenching and natural aging for 24 hours. 24 Another reference sample was prepared as a T6 reference sample by holding it at 165±5℃ for 10h and the H was measured. T6 .
[0037] 4) The synchronous calibration sample obtained in step 2) and the profile to be formed are stored in the same constant temperature environment, with the end of online quenching as the common starting point of natural aging and the entry of the profile to be formed into the bending process as the common ending point of natural aging. When the profile is transferred to the bending process, the synchronous calibration sample is simultaneously transferred to the pre-deformation and candidate artificial aging calibration process, so that the calibration sample has a natural aging microstructure corresponding to the profile to be formed before pre-deformation.
[0038] 5) Perform loading and unloading state detection on the first calibration beam during the bending process: obtain the neutral layer curvature radius R when the bending moment reaches its peak during the bending process by scanning the loading state profile. L The final neutral layer curvature radius R was obtained by contour scanning of the target finished product in this batch after the external force was completely removed and a stable state was reached. U The normal distance y from the outermost edge of the profile section to the neutral layer is obtained from the profile section drawing. max The true strain ε of the axial tensile stress applied during bending deformation was obtained through the neutral layer gauge length. t Calculate ε according to formula (1)max Calculate K according to formula (2) h The calculation results are shown in Table 1.
[0039] ; ; 6) The thickness of the sample is h when calibrated simultaneously. s, When the synchronously calibrated sample is symmetrically bent, y s Take h s / 2. Calculate R according to formula (3). s,c The sample was pre-deformed using a bending die with a corresponding fillet radius. After pre-deformation, the actual bending radius was verified using DIC to obtain a calibration sample for the coupled state.
[0040] ; 7) Verify the peak strain of the surface layer of the coupled state calibration specimen obtained in step 6); take four coupled state calibration specimens after verifying the peak strain of the surface layer, and artificially age them at 190℃ for 45 min, 60 min, 75 min and 90 min respectively, and test their hardness. The hardness retention ratio λ corresponding to the i-th candidate time is... i and the hardness increment ΔH of adjacent candidate times i Determine according to equations (4) and (5) respectively: ; Among them, H i H represents the hardness of the calibration sample after processing at the i-th candidate time. T6 The hardness of the reference sample in T6 condition from the same batch; H i+1 The hardness of the calibration sample after processing at the (i+1)th candidate time; when 0.97 ≤ λ i ≤1.03 and ΔH i When the value is ≤2.0HV, the corresponding candidate time will be determined as the qualified insulation time.
[0041] The test results are shown in Table 2. The above process flow is then summarized to obtain... Figure 1 The diagram shows the efficient manufacturing process flow of the 6082 aluminum alloy automotive anti-collision beam of the present invention.
[0042] The reference peak strain of the crash beam is denoted as ε. b,p The peak strain of the calibrated specimen is denoted as ε. s The hardness of the calibration sample and the critical area of the anti-collision beam after the same artificial aging is denoted as H. s and H b Peak strain relative error E ε and relative error of hardness E H The calculations are performed according to equations (8) and (9) respectively, and the results are shown in Tables 1 and 3. The overall process route is as follows: Figure 1 The flowchart of the efficient manufacturing process of the 6082 aluminum alloy automotive anti-collision beam of the present invention is shown.
[0043] .
[0044] Example 2 This embodiment provides a high-efficiency manufacturing process for a 6082 aluminum alloy automotive anti-collision beam using an improved formula (3). The preparation steps are as follows: 1) After homogenization, 6082 aluminum alloy ingots are extruded into multi-cavity anti-collision beam profiles at 520℃. After demolding, they are quenched with water mist and then stretched and straightened by 1% to obtain the anti-collision beam profiles.
[0045] 2) Select a complete profile from this batch as the first calibration beam in the bending process. Also select a reference sample and a synchronous calibration sample from the non-welded wall panel area of the same batch of profiles. The reference sample and the synchronous calibration sample are 150mm long and 30mm wide, and the thickness is maintained at the profile extrusion wall thickness in step 1).
[0046] 3) Take a reference sample and measure H after quenching and natural aging for 24 hours. 24 Another reference sample was prepared as a T6 reference sample by holding it at 165±5℃ for 10h and the H was measured. T6 .
[0047] 4) The synchronous calibration sample obtained in step 2) and the profile to be formed are stored in the same constant temperature environment, with the end of online quenching as the common starting point of natural aging and the entry of the profile to be formed into the bending process as the common ending point of natural aging. When the profile is transferred to the bending process, the synchronous calibration sample is simultaneously transferred to the pre-deformation and candidate artificial aging calibration process, so that the calibration sample has a natural aging microstructure corresponding to the profile to be formed before pre-deformation.
[0048] 5) Perform loading and unloading state detection on the first calibration beam during the bending process: obtain the neutral layer curvature radius R when the bending moment reaches its peak during the bending process by scanning the loading state profile. L The final neutral layer curvature radius R was obtained by contour scanning of the target finished product in this batch after the external force was completely removed and a stable state was reached. U The normal distance y from the outermost edge of the profile section to the neutral layer is obtained from the profile section drawing. max The true strain ε of the axial tensile stress applied during bending deformation was obtained through the neutral layer gauge length. t ε is calculated according to formula (1) max Calculate K according to formula (2) h .
[0049] ; ; 6) The thickness of the sample is h when calibrated simultaneously. s, When the synchronously calibrated sample is symmetrically bent, y s Take h s / 2. Calculate R according to formula (3). s,c The sample was pre-deformed using a bending die with a corresponding fillet radius. After pre-deformation, the actual bending radius was verified using DIC to obtain a calibration sample for the coupled state.
[0050] ; 7) Verify the peak strain of the surface layer of the coupled state calibration specimen obtained in step 6); take four coupled state calibration specimens after verifying the peak strain of the surface layer, and artificially age them at 180℃ for 90 min, 100 min, 110 min and 120 min respectively, and test their hardness. The hardness retention ratio λ corresponding to the i-th candidate time is... i and the hardness increment ΔH of adjacent candidate times i Determine according to equations (4) and (5) respectively: ; The test results are shown in Table 2.
[0051] The reference peak strain of the crash beam is denoted as ε. b,p The peak strain of the calibrated specimen is denoted as ε. s The hardness of the calibration sample and the critical area of the anti-collision beam after the same artificial aging is denoted as H. s and H b Peak strain relative error E ε and relative error of hardness E H Calculate according to equations (8) and (9) respectively.
[0052] .
[0053] Example 3 This embodiment provides a high-efficiency manufacturing process for a 6082 aluminum alloy automotive anti-collision beam using an improved formula (3). The preparation steps are as follows: 1) After homogenization, 6082 aluminum alloy ingots are extruded into multi-cavity anti-collision beam profiles at 520℃. After demolding, they are quenched with water mist and then stretched and straightened by 1% to obtain the anti-collision beam profiles.
[0054] 2) Select a complete profile from this batch as the first calibration beam in the bending process. Also select a reference sample and a synchronous calibration sample from the non-welded wall panel area of the same batch of profiles. The reference sample and the synchronous calibration sample are 150mm long and 30mm wide, and the thickness is maintained at the profile extrusion wall thickness in step 1).
[0055] 3) Take a reference sample and measure H after quenching and natural aging for 24 hours. 24 Another reference sample was prepared as a T6 reference sample by holding it at 165±5℃ for 10h and the H was measured. T6 .
[0056] 4) The synchronous calibration sample obtained in step 2) and the profile to be formed are stored in the same constant temperature environment, with the end of online quenching as the common starting point of natural aging and the entry of the profile to be formed into the bending process as the common ending point of natural aging. When the profile is transferred to the bending process, the synchronous calibration sample is simultaneously transferred to the pre-deformation and candidate artificial aging calibration process, so that the calibration sample has a natural aging microstructure corresponding to the profile to be formed before pre-deformation.
[0057] 5) Perform loading and unloading state detection on the first calibration beam during the bending process: obtain the neutral layer curvature radius R when the bending moment reaches its peak during the bending process by scanning the loading state profile. L The final neutral layer curvature radius R was obtained by contour scanning of the target finished product in this batch after the external force was completely removed and a stable state was reached. U The normal distance y from the outermost edge of the profile section to the neutral layer is obtained from the profile section drawing. max The true strain ε of the axial tensile stress applied during bending deformation was obtained through the neutral layer gauge length. t ε is calculated according to formula (1) max Calculate K according to formula (2) h .
[0058]
[0059] ; 6) The thickness of the sample is h when calibrated simultaneously. s, When the synchronously calibrated sample is symmetrically bent, y s Take h s / 2. Calculate R according to formula (3). s,c The sample was pre-deformed using a bending die with a corresponding fillet radius. After pre-deformation, the actual bending radius was verified using DIC to obtain a calibration sample for the coupled state.
[0060] ; 7) Verify the peak strain of the surface layer of the coupled state calibration specimen obtained in step 6); take four coupled state calibration specimens after verifying the peak strain of the surface layer, and artificially age them at 205℃ for 20 min, 65 min, 110 min and 155 min respectively, and test their hardness. The hardness retention ratio λ corresponding to the i-th candidate time is... i and the hardness increment ΔH of adjacent candidate times i Determine according to equations (4) and (5) respectively: ; The test results are shown in Table 2.
[0061] The reference peak strain of the crash beam is denoted as ε. b,p The peak strain of the calibrated specimen is denoted as ε. s The hardness of the calibration sample and the critical area of the anti-collision beam after the same artificial aging is denoted as H. s and H b Peak strain relative error E ε and relative error of hardness E H Calculate according to equations (8) and (9) respectively.
[0062] .
[0063] Example 4 This embodiment provides a K h =1, meaning the anti-collision beam is manufactured using the original formula for 6082 aluminum alloy automotive anti-collision beams before modification. The manufacturing process is completely consistent with Example 1, except that K is set to... h =1, meaning that the pre-deformation of the synchronous calibration sample is performed using the original formula calculation results before the improvement.
[0064] Example 5 This embodiment provides a crash beam that simply superimposes the effects of natural aging and pre-deformation as independent hardening increments. The manufacturing process is completely consistent with that of Embodiment 1, except that the artificial aging is changed to artificial aging of the profile at 190±3℃ for 75 minutes, and synchronous calibration samples and reference samples are not used. The effects of natural aging and pre-deformation are simply superimposed as independent hardening increments. Hardness tests were performed on the reference sample that was not synchronously natural aged and did not undergo pre-deformation to obtain H. B The hardness of the sample subjected to simultaneous natural aging was measured to be 106.2 HV. The influence of natural aging, ΔH, was obtained by comparing the two results. NA =3.2HV; the hardness of the pre-deformed sample alone is 109.0HV, and the pre-deformation ΔH is obtained. PD =6.0HV. The simple superposition prediction value H is obtained by the following formula. add :
[0065] H add =H B +ΔH NA +ΔH PD (Simple superimposed comparison); H is obtained by simple superposition add =112.2HV, while the hardness H of the deformation zone of the same batch of anti-collision beams b The value is 109.8 HV; the same batch of products using this invention are synchronously and naturally aged and subjected to K... h Correcting the pre-deformation coupling state to calibrate the hardness H of the specimens The value is 109.5 HV. According to Equation (9), the relative error of simple superposition is 2.19%, and the relative error of coupled state entity calibration is 0.27%. The specific results are shown in Table 3.
[0066] Table 1 Calculation Table of Process Parameters Group <![CDATA[K h ]]> Target bending radius / mm Peak strain at the surface / % <![CDATA[E ε / %]]> Reference for anti-collision beams — — 5.02 — Example 1: Improved Formula 1.1726 29.13 4.98 0.80 Example 4: Original Formula 1.0000 34.29 4.31 14.14 Table 2 Relationship between Artificial Aging Insulation Time and Hardness Group Artificial aging time / min <![CDATA[Sample hardness H i / HV]]> <![CDATA[H T6 / HV]]> <![CDATA[Hardness retention ratio λ i > <![CDATA[ΔH i / HV]]> Insulation time qualification Example 1 (190℃) 45 104.6 112.4 0.931 3.7 Not satisfied 60 108.3 112.4 0.964 1.2 Maintaining a ratio of insufficient 75 109.5 112.4 0.974 0.3 <![CDATA[satisfies, t * =75min]]> 90 109.8 112.4 0.977 — Upper limit point Example 2 (180℃) 90 104.8 110.6 0.948 3.1 Not satisfied 100 107.9 110.6 0.976 1.7 <![CDATA[satisfy, t * =100min]]> 110 109.6 110.6 0.991 0.4 Satisfactory but takes a long time 120 110.0 110.6 0.995 — Upper limit point Example 3 (205℃) 20 105.0 113.0 0.929 6.2 Not satisfied 65 111.2 113.0 0.984 0.5 <![CDATA[satisfy, t * =65min <!-- 9 -->]]> 110 110.7 113.0 0.980 1.8 Satisfactory but takes a long time 155 108.9 113.0 0.964 — Upper limit point Table 3. Hardness equivalence between simple superposition comparison and coupled state entity calibration. Group <![CDATA[H B / HV]]> <![CDATA[ΔH NA / HV]]> <![CDATA[ΔH PD / HV]]> Compare hardness / HV <![CDATA[H b / HV]]> <![CDATA[E H / %]]> Simple overlay comparison 103.0 3.2 6.0 <![CDATA[112.2(H add )]]> 109.8 2.19 Coupled state entity calibration — — — <![CDATA[109.5(H s )]]> 109.8 0.27 The test results for the candidate time and hardness retention ratio of Examples 1-3 were as follows: Figure 3 The diagrams shown in Examples 1-3 illustrate the candidate holding time-hardness retention ratio relationship under different artificial aging temperatures and candidate time intervals. In each example, the temperature and candidate interval are independent factors. The three sets of experiments belong to independent process calibration batches. Each group varied the candidate holding time under a fixed temperature condition to determine the shortest holding time required to meet the hardness retention ratio requirement at that temperature. The candidate holding times and time intervals used are not entirely the same. This solution can preset artificial aging temperatures for different needs and determine the appropriate holding time through candidate time calibration.
[0067] Compare the tensile bending loading history with the corrected radius relationship of the calibrated specimen, and test or calculate the maximum loading radius R under the original formula and the corrected formula. L The radius R, determined by the geometric curvature of the steady state, after reaching a stable state. U The original formula for radius R s,0 With the corrected radius R s,c The correspondence between them is obtained as follows Figure 2 The diagram shows the relationship between the tensile bending loading process and the corrected radius of the calibrated specimen.
[0068] As can be seen from Table 1, the introduction of K h Afterwards, the relative error of peak strain E ε Example 4 does not introduce K h The original formula calculated that the pre-deformed profile was 14.14%, which was reduced to the value introduced in Example 1 by K. h The 0.80% obtained after correcting the calculation formula indicates that the bending process correction can solve the peak deformation mismatch caused by only copying the final geometry of the calibration sample after unloading.
[0069] As shown in Table 3, if the natural aging hardening increment obtained in Example 5 is simply added to the pre-deformation hardening increment, the hardness equivalence error is 2.19%; compared with the same batch of materials that underwent synchronous natural aging and K...h Compared to Example 1, which corrects the pre-deformed coupled state entity calibration, the hardness equivalence error is reduced to 0.27%, indicating that entity calibration can directly reproduce the nonlinear net response when both factors coexist.
[0070] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A high-efficiency manufacturing process for 6082 aluminum alloy automotive anti-collision beams, characterized in that, Includes the following steps: S1. After the 6082 aluminum alloy anti-collision beam profile is extruded, quenched and straightened, a reference sample and a synchronous calibration sample that are stored at the same time and in the same environment as the anti-collision beam profile to be formed and have undergone the same natural aging process are cut from the same extrusion and quenching batch. S2. Perform overall stretch bending of the profile to be formed, and obtain the radius of curvature R of the neutral layer when the bending moment in the deformation zone of the anti-collision beam reaches its peak during the stretch bending process. L After the external force is completely removed, the final neutral layer curvature radius R of the anti-collision beam reaches a stable state. U The true strain ε of axial tension applied during bending deformation t And the normal distance y from the outermost edge of the profile section to the neutral layer max And according to R L R U ε t and y max Determine the bending process correction factor K h ; S3, the bending process correction coefficient K obtained in step S2. h Corrected by R U Based on the determined true strain of the outer layer bending, the corrected target bending radius R of the synchronously calibrated specimen is determined. s,c Pre-deform the synchronous calibration specimens to obtain calibration specimens with the coupled influence of natural aging and bending state. S4. For the calibration samples obtained in step S3, implement the preset candidate artificial aging system, measure the hardness of the calibration samples corresponding to each candidate artificial aging system, use the hardness of the calibration samples to characterize the artificial aging response after coupling the natural aging state and the pre-deformation state, and determine the overall artificial aging parameters of the current batch of anti-collision beams based on the artificial aging response. S5. Artificially age the current batch of anti-collision beam profiles to be artificially aged according to the overall artificial aging parameters determined in step S4, and obtain 6082 aluminum alloy automotive anti-collision beam components after cooling.
2. The efficient manufacturing process for 6082 aluminum alloy automotive anti-collision beams as described in claim 1, characterized in that, In step S2, R U Through ε max Indirectly affecting the bending process correction factor K h , ε max The maximum true strain of the outer layer bending when the anti-collision beam reaches a stable state after the external force is completely removed is determined according to equation (1): 。 3. The efficient manufacturing process for 6082 aluminum alloy automotive anti-collision beams as described in claim 2, characterized in that, In step S2, the bending process correction coefficient K h Determine according to formula (2): 。 4. The efficient manufacturing process for 6082 aluminum alloy automotive anti-collision beams as described in claim 3, characterized in that, In step S3, the target bending radius R is corrected. s,c Determine according to formula (3): ; Among them, y s To simultaneously calibrate the normal distance from the outermost part of the sample to its neutral layer.
5. The efficient manufacturing process for 6082 aluminum alloy automotive anti-collision beams as described in claim 1, characterized in that, In step S4, each batch of candidates shall have no fewer than three candidates under the artificial aging system, and the same artificial aging temperature T shall be used. a With different time limits, the time difference between two adjacent candidates in the same batch is 10 to 45 minutes.
6. The efficient manufacturing process for 6082 aluminum alloy automotive anti-collision beams as described in claim 5, characterized in that, Artificial aging temperature T a The temperature is 180–205℃, and the duration is 20–180 minutes.
7. The efficient manufacturing process for 6082 aluminum alloy automotive anti-collision beams as described in claim 1, characterized in that, In step S4, using the hardness of the T6 state reference sample from the same batch as a benchmark, the hardness retention ratio λ corresponding to the i-th candidate aging regime is evaluated. i and the hardness increment ΔH of adjacent candidate times i Determine according to equations (4) and (5) respectively: ; Among them, H i H represents the hardness of the calibration sample after processing at the i-th candidate time. T6 The hardness of the reference sample in T6 condition from the same batch; H i+1 The hardness of the calibration sample after processing at the (i+1)th candidate time; when 0.97 ≤ λ i ≤1.03 and ΔH i When the value is ≤2.0HV, the corresponding candidate time will be determined as the qualified insulation time.
8. The efficient manufacturing process for 6082 aluminum alloy automotive anti-collision beams as described in claim 1, characterized in that, The length of the synchronous calibration sample is 80-150 mm and the width is 15-30 mm.
9. The efficient manufacturing process for 6082 aluminum alloy automotive anti-collision beams as described in claim 1, characterized in that, In step S5, a sample with the same material batch, natural aging history, and equivalent pre-deformation state as the synchronous calibration sample is used as the furnace verification sample. It is loaded into the furnace together with the anti-collision beam profile to be artificially aged, and the artificial aging temperature is set to T. a The temperature at the center of the sample reached T. a The determined heat preservation time is calculated starting at -5℃. After the heat preservation is completed, the anti-collision beam profile is cooled to obtain an aluminum alloy automotive anti-collision beam.
10. The efficient manufacturing process for 6082 aluminum alloy automotive anti-collision beams as described in claim 9, characterized in that, After the artificial aging process is completed, the cooling method is air cooling, cooling to ≤60℃.