Quantitative control method for the uniformity of continuous extrusion cross section of large-size aluminum alloy busbars
By establishing a comprehensive control model and precise mold design, process parameter matching, and cooling control, the problem of performance inhomogeneity in large-size aluminum alloy manifolds during continuous extrusion was solved, enabling rapid development and efficient production to meet the needs of high-end applications.
Patent Information
- Application Number
- CN202611269939.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-20
- Publication Date
- 2026-11-17
AI Technical Summary
Large-size aluminum alloy busbars suffer from problems such as non-uniform cross-sectional properties, long development cycle, high trial mold cost, and large performance fluctuations between batches during continuous extrusion. In particular, when producing wide-width products, the non-uniformity of temperature field, strain field, cooling rate, and weld structure leads to a low finished product qualification rate.
By establishing a comprehensive control model for temperature field, strain field, cooling rate, and weld microstructure, quantitative design of mold structure, matching and regulation of extrusion process parameters, and online cooling homogenization control are carried out to achieve quantitative control of the uniformity of aluminum alloy busbar cross-sectional properties.
It shortened the new product development cycle, reduced material consumption in trial molds, improved yield and batch-to-batch performance stability, met the stringent requirements of high-end fields, reduced overall manufacturing costs, and improved weld strength and processing qualification rate.
Smart Images

Figure CN123102781A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of non-ferrous metal plastic processing technology, and in particular to a method for quantitatively controlling the uniformity of the continuous extrusion cross-section of large-size aluminum alloy busbars. Background Technology
[0002] Continuous extrusion technology relies on the friction between the extrusion roller and the bar to achieve continuous feeding, frictional heating and plastic forming. It does not require billet preheating and repeated upsetting, and has significant advantages such as high material utilization, short process flow and unrestricted product length. It has already achieved large-scale industrial application in the fields of small diameter aluminum wire and small profiles.
[0003] With the rapid development of the new energy and energy storage industries, the market demand for large-section, wide-width aluminum alloy busbars has been increasing year by year. The product width has expanded from the traditional 20mm or less to 50-120mm, and the width-to-height ratio has increased from less than 2 to 8-12.
[0004] However, when using the traditional continuous extrusion process for small-sized profiles to produce large-width products, inherent compatibility defects are exposed. The core problems are concentrated in four aspects: First, the deformation flow and strain distribution are naturally uneven. Large-width flat strips require significant lateral widening of the metal, resulting in large differences in the metal flow paths between the central and peripheral regions, with cross-sectional strain distribution differences reaching more than three times. Second, the temperature field distribution is severely unbalanced. Heat generation is concentrated in the central region of the large cross-section, making heat dissipation difficult, while the heat dissipation rate is fast in the peripheral region, with the maximum temperature difference across the cross-section reaching 50-80℃. Third, the uniformity of online quenching and cooling is poor. The cooling rate in the central region is far lower than the critical solution cooling rate, leading to premature precipitation and coarsening of the Mg2Si phase, while also inducing residual stress. Fourth, the quality of longitudinal welds is weak and unavoidable. The interface where multiple metal strands converge is prone to oxide inclusions and micropores, resulting in a finished product processing qualification rate of less than 85%. Currently, the industry's continuous extrusion development of large-size aluminum busbars mostly relies on engineers' experience to repeatedly modify molds and adjust processes. There is a lack of a systematic and quantitative control method based on size characteristics, resulting in a new product development cycle of 1-2 months, large material consumption in trial molds, and significant performance fluctuations between batches, making it difficult to meet the stringent requirements for product consistency in high-end fields. Summary of the Invention
[0005] The purpose of this invention is to provide a quantitative control method for the uniformity of the continuous extrusion cross section of large-size aluminum alloy busbars, which solves the problems of uneven cross-sectional performance of large-size wide aluminum alloy busbars, long new product development cycle, high trial molding cost, and large performance fluctuation between batches.
[0006] To achieve the above objectives, this invention provides a method for quantitatively controlling the uniformity of the continuous extrusion cross-section of large-size aluminum alloy busbars, comprising the following steps: By defining the total non-uniformity of cross-sectional properties as the control objective, a total control model is established, which consists of a weighted summation of temperature field non-uniformity, strain field non-uniformity, cooling rate non-uniformity, and weld microstructure non-uniformity, and quantitative evaluation indicators are obtained. By performing quantitative design of the mold structure, the uniformity of the strain field and the quality of the weld after regulation are obtained; The uniformity of the temperature field after adjustment is obtained by matching and controlling the extrusion process parameters; By implementing online cooling uniformity control, the uniformity of the regulated cooling rate is obtained; The temperature field, strain field, cooling rate and weld microstructure were tested separately, and the total non-uniformity of cross-sectional properties was calculated according to the overall control model. The large-size wide aluminum alloy busbar with the total non-uniformity of cross-sectional properties meeting the target threshold requirement was obtained.
[0007] The section on "establishing a total control model consisting of a weighted sum of temperature field non-uniformity, strain field non-uniformity, cooling rate non-uniformity, and weld microstructure non-uniformity by defining the total non-uniformity of cross-sectional properties as the control objective, and obtaining quantitative evaluation indicators" includes the following steps: By defining four sub-items of non-uniformity—temperature field non-uniformity, strain field non-uniformity, cooling rate non-uniformity, and weld microstructure non-uniformity—quantitative indicators for each item are obtained. The overall control model is obtained by determining the weighting coefficients of the four sub-items: temperature field, strain field, cooling rate, and weld microstructure.
[0008] The section on "obtaining the controlled strain field uniformity and weld quality through quantitative design of mold structure" includes the following steps: By designing a differentiated working zone length difference according to the principle of lengthening the center and shortening the edges, the strain field uniformity that offsets the natural flow velocity difference is obtained; By designing the welding chamber depth to be no less than 0.4 times the cross-sectional width, weld quality with increased welding pressure can be obtained.
[0009] The section on "obtaining the uniformity of the temperature field after adjustment by matching and controlling the extrusion process parameters" includes the following steps: By matching the rotation speed according to the rule of increasing the width and decreasing the rotation speed of the extrusion roller, the uniformity of the temperature field with reduced central heat accumulation is obtained; By matching the reduction rate according to the rule of increasing the thickness of the lifting rod material, the uniformity of the temperature field is obtained to ensure the balance between deformation and heat generation.
[0010] The step of "obtaining the regulated cooling rate uniformity through online cooling homogenization control" includes the following steps: By adopting a partitioned independent cooling architecture, the cooling rate of each partition can be adjusted. By increasing the cooling water pressure in the central region to compensate for the thickness thermal resistance, a uniform cooling rate is achieved, reducing the difference in cooling rate between the center and the edge.
[0011] The section on "inspecting the four dimensions of temperature field, strain field, cooling rate, and weld microstructure, and calculating the total non-uniformity of cross-sectional properties according to the overall control model to obtain a large-size wide-width aluminum alloy busbar whose total non-uniformity of cross-sectional properties meets the target threshold requirement" includes the following steps: The test sample is obtained by selecting measuring points along the width direction and taking cross-sectional samples along the length direction at the aluminum discharge end; Four sub-items of non-uniformity were obtained by detecting the temperature field, strain field, cooling rate, and weld microstructure respectively. The total non-uniformity of cross-sectional performance is obtained by substituting the four sub-items into the overall control model according to their weights.
[0012] This invention discloses a quantitative control method for the uniformity of the continuous extrusion cross-section of large-size aluminum alloy busbars. By establishing a quantitative mapping relationship between the geometric dimensions of the aluminum busbar and the die structure, extrusion process, and cooling parameters, this invention replaces the traditional experience-based trial-and-error approach. This not only shortens the new product development cycle from 1-2 months to less than 2 weeks and reduces material loss in trial molds by more than 60%, but also avoids human experience differences through quantified process rules. This keeps performance fluctuations between batches in mass production within 3%, increases the yield from approximately 70% in traditional processes to over 90%, and reduces overall manufacturing costs by about 15%. Simultaneously, through the coordinated control of four dimensions—temperature field, strain field, cooling field, and weld microstructure—the overall non-uniformity of the large-size aluminum busbar cross-section performance is reduced from 15%-20% in traditional processes to 8%-10%. Achieving a level of uniformity comparable to that of small-sized profiles, this approach completely solves the industry pain points of large performance fluctuations and poor batch stability in large-sized products, meeting the stringent requirements of high-end fields such as new energy and photovoltaics. Furthermore, through a welding chamber depth matching design combined with rod material cleaning treatment, the weld strength coefficient is increased from 0.8 to over 0.92, and the bending processing qualification rate is increased from 85% to over 98%, effectively reducing the scrap rate in subsequent processing and the risk of failure in end applications. In addition, the entire method is based on the design of existing mainstream continuous extrusion equipment, eliminating the need for expensive new equipment such as zone heating and ultrasonic assistance. Mass production applications can be achieved simply through mold optimization and process parameter matching, covering aluminum busbar products with a full width range of 25-120mm, and adapting to multiple application fields such as new energy, photovoltaics, and power distribution. Attached Figure Description
[0013] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below.
[0014] Figure 1This is a flowchart of the method for quantitatively controlling the uniformity of the continuous extrusion cross section of large-size aluminum alloy busbars provided by the present invention.
[0015] Figure 2 The process involves defining the total non-uniformity of cross-sectional properties as the control objective, establishing a total control model composed of a weighted summation of temperature field non-uniformity, strain field non-uniformity, cooling rate non-uniformity, and weld microstructure non-uniformity, and obtaining a flowchart of quantitative evaluation indicators.
[0016] Figure 3 This is a flowchart of obtaining the uniformity of the strain field and the quality of the weld after quantitative design of the mold structure.
[0017] Figure 4 This is a flowchart illustrating how the uniformity of the temperature field is achieved through matching and adjusting extrusion process parameters.
[0018] Figure 5 This is a flowchart illustrating the process of achieving uniform cooling rate through online cooling homogenization control.
[0019] Figure 6 The flowchart describes a process for detecting four dimensions—temperature field, strain field, cooling rate, and weld microstructure—and calculating the total non-uniformity of cross-sectional properties according to the overall control model. This process yields a flowchart of a large-size, wide-width aluminum alloy busbar whose total non-uniformity of cross-sectional properties meets the target threshold requirement. Detailed Implementation
[0020] The embodiments of the present invention are described in detail below. Examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, but should not be construed as limiting the present invention.
[0021] Please see Figures 1 to 6 The present invention provides a method for quantitatively controlling the uniformity of the continuous extrusion cross-section of large-size aluminum alloy busbars, comprising the following steps: S1 defines the total non-uniformity of cross-sectional properties as the control objective, and establishes a total control model consisting of a weighted summation of temperature field non-uniformity, strain field non-uniformity, cooling rate non-uniformity and weld microstructure non-uniformity, thereby obtaining quantitative evaluation indicators. S11 defines four sub-items of non-uniformity: temperature field non-uniformity, strain field non-uniformity, cooling rate non-uniformity, and weld microstructure non-uniformity, and obtains sub-item quantitative indicators. S12 obtains the overall control model by determining the weight coefficients of four sub-items: temperature field, strain field, cooling rate, and weld microstructure.
[0022] S2 obtains the uniformity of the strain field and the quality of the weld after regulation by performing quantitative design of the mold structure; S21 achieves strain field uniformity by designing a differentiated working zone length difference according to the principle of lengthening the center and shortening the edges; S22 achieves improved weld quality by designing the weld chamber depth to be no less than 0.4 times the cross-sectional width.
[0023] S3 achieves temperature field uniformity after adjustment by matching and controlling extrusion process parameters; S31 achieves reduced temperature field uniformity by matching the rotation speed according to the rule of increasing the width and decreasing the rotation speed of the extrusion roller; S32 achieves temperature field uniformity by matching the reduction rate according to the rule of increasing the reduction rate of the lifting rod material based on the thickness, thus ensuring the balance between deformation and heat generation.
[0024] S4 achieves uniform cooling rate after online cooling homogenization control; The S41 achieves adjustable cooling rates by employing a partitioned independent cooling architecture. S42 increases the cooling water pressure in the central region to compensate for the thickness thermal resistance, thereby achieving uniform cooling rate with a reduced difference in cooling rate between the center and the edge.
[0025] S5 performs tests on four dimensions: temperature field, strain field, cooling rate, and weld microstructure. It also calculates the total non-uniformity of cross-sectional properties according to the overall control model, resulting in a large-size wide-width aluminum alloy busbar whose total non-uniformity of cross-sectional properties meets the target threshold requirements.
[0026] S51 obtains the test sample by selecting measuring points along the width direction and taking cross-sectional samples along the length direction at the aluminum discharge end; S52 obtains four sub-items of non-uniformity by detecting the temperature field, strain field, cooling rate, and weld microstructure respectively; S53 calculates the total non-uniformity of cross-sectional performance by substituting the four sub-items of non-uniformity into the overall control model according to their weights.
[0027] Specifically, the non-uniform cross-sectional properties of large-size aluminum busbars are essentially a macroscopic manifestation of microstructural inhomogeneity, which includes four categories: differences in grain size, differences in recrystallization degree, differences in the size and distribution of precipitated phases, and differences in the bonding state of the weld interface. These four types of structural differences are determined by four core process factors during the extrusion process: temperature field distribution, strain field distribution, cooling rate distribution, and weld bonding quality.
[0028] This technology takes "inherent dimensional degradation + process parameter compensation" as its core idea: first, it clarifies the degree of natural non-uniformity caused by geometric dimensions, and then, through quantitative adjustment of corresponding mold, process, and cooling parameters, it offsets the degradation effect caused by dimensions, and finally achieves uniform and controllable microstructure and properties across the entire cross section.
[0029] Overall control formula: The total non-uniformity η of the cross-sectional properties is defined as the final control objective. Its physical meaning is the combined relative fluctuation of the cross-sectional mechanical and electrical properties; a smaller value indicates better uniformity. The overall control formula is as follows: ; The parameters in the formula are defined as follows: 1. Partial non-uniformity parameters Temperature field inhomogeneity, dimensionless, is defined as the difference between the highest and lowest temperatures of a cross section divided by the average temperature of the cross section. It is a core factor affecting dynamic recrystallization and grain growth. Strain field inhomogeneity, dimensionless, is defined as the relative difference between the maximum and minimum strain rates of the cross section, which determines the recrystallization driving force and the residual proportion of the deformed structure. Cooling rate non-uniformity, dimensionless, is defined as the relative difference between the cooling rate at the edge of the cross section and the cooling rate at the center. It directly determines the cross-sectional difference between supersaturated solid solubility and precipitated phase. : Weld microstructure inhomogeneity, dimensionless, is defined as the difference between the tensile strength of the base region and the tensile strength of the weld region divided by the tensile strength of the base region. It reflects the degree of performance deviation between the weld as a weak area and the base region.
[0030] 2. For 6-series aluminum alloy busbars, the contribution ratio of the four sub-items to the overall performance non-uniformity was determined through extensive orthogonal experiments and grey relational analysis, and the corresponding weights are as follows: Temperature field has the greatest impact on grain size and degree of recrystallization, contributing the most to the overall effect. The strain field determines the energy storage and recrystallization driving force of deformation, and is the second source of microstructure heterogeneity; The cooling field affects the behavior of the precipitated phase, which determines the final match between strength and conductivity. The weld only occupies a local area of the cross section and contributes the least to the overall uniformity.
[0031] 3. Adjust the target threshold Industrial-grade general-purpose aluminum busbars: Total non-uniformity ; High-performance renewable energy / photovoltaic busbars: Total uniformity .
[0032] Methods for detecting and calculating η (operable test standards) In this embodiment, the total non-uniformity η of the cross-sectional properties is sampled, tested, and calculated according to the following operable method. All test methods used are in accordance with current national and international standards to ensure that the indicators are verifiable.
[0033] (1) Cross-sectional sampling scheme Five measuring points were evenly selected along the width direction at the aluminum discharge end: one point at the center of the cross-section, one point at 1 / 4 of the width from each of the two side edges, and one point at 5mm from each of the two side edges; a representative position was taken at 1 / 2 of the thickness along the thickness direction. At the same time, a set of cross-sectional samples were taken along the length direction of the product at the head (0.5m from the starting end), middle, and tail (0.5m from the end) to evaluate the longitudinal fluctuation.
[0034] Due to uneven metal flow and varying cooling rates during aluminum alloy extrusion, different parts of the profile (such as the front and rear ends, thicker and thinner sections) may exhibit microstructure differences, leading to fluctuations in mechanical properties. Therefore, samples must be taken both longitudinally and transversely from the profile. Sampling rules should follow the sampling provisions for mechanical properties and electrical conductivity in GB / T6892-2023 "General Industrial Aluminum and Aluminum Alloy Extruded Profiles". For electrical aluminum and aluminum alloy busbars, busbar testing standards such as JB / T Telecommunications Equipment Certification can also be referenced.
[0035] (2) Detection of temperature field nonuniformity η_T An infrared thermal imager (temperature measurement accuracy ±1℃) was used to collect the temperature distribution of the cross-section at the instant of aluminum discharge. The highest temperature T_max and the lowest temperature T_min were taken from 5 measuring points. The average temperature of the cross-section T_avg = (T_max + T_min) / 2. η_T = (T_max − T_min) / T_avg; (3) Detection of strain field inhomogeneity η_ε The continuous extrusion process was numerically simulated using DEFORM-3D or similar rigid-plastic finite element software. The strain rate at each measuring point at the die sizing zone was extracted. The maximum strain rate εmax and the minimum strain rate εmin were taken, and the average strain rate εavg = (εmax + εmin) / 2. η_ε=(ε_max−ε_min) / ε_avg; The evaluation method references the conventions for characterizing the root mean square error of flow velocity in continuous extrusion sizing zones using rigid-plastic finite element methods.
[0036] (4) Detection of cooling rate non-uniformity η_c K-type armored thermocouples (sampling frequency ≥ 100Hz) are embedded at the center and edge measuring points. The temperature-time curves of the aluminum busbar as it passes through the cooling section are recorded. The cooling rate at each measuring point is calculated from dT / dt. η_c=(V_edge−V_center) / V_center; In the formula, V_edge is the cooling rate of the edge measuring point, and V_center is the cooling rate of the center measuring point.
[0037] (5) Detection of weld microstructure inhomogeneity η_w (application of tensile strength) According to GB / T228.1-2021 "Metallic materials, tensile testing—Part 1: Tests at room temperature" (equivalent to ISO6892-1:2019, international standard corresponding to ASTM E8 / E8M), tensile specimens were cut from the weld zone and the adjacent matrix zone respectively to prepare specimens that meet the standard requirements. The tensile strengths R_m,weld and R_m,matrix were determined on a Class 1 precision testing machine. Then: η_w=(R_m,matrix−R_m,weld) / R_m,matrix; In addition, tensile specimens were prepared at five measuring points along the cross-section according to GB / T228.1-2021, and the tensile strength R_m,i (i=1-5) at each point was measured to calculate the auxiliary fluctuation amount of the cross-sectional mechanical properties: CV_R=[max(R_m,i)−min(R_m,i)] / R_m_avg×100%; In the formula, R_m_avg is the average tensile strength of 5 points. CV_R serves as an auxiliary verification index for the mechanical dimension of η.
[0038] (6) Auxiliary verification of conductivity (application of conductivity) Conductivity (%IACS) was measured at each measuring point according to GB / T12966-2022 "Eddy Current Test Method for Conductivity of Aluminum Alloys" (corresponding to international standard ASTM E1004-17). For electrical aluminum and aluminum alloy busbars, the volume resistivity can also be measured using the four-probe method according to ASTM B193. Tests were conducted at five measuring points along the cross-section, and the maximum relative fluctuation of the cross-sectional conductivity was taken as an auxiliary verification index. CV_σ=[max(σ_i)−min(σ_i)] / σ_avg×100%; In the formula, σ_i is the conductivity (%IACS) at each measurement point, and σ_avg is the average value. CV_σ serves as an auxiliary verification index for the electrical dimension of η, used to verify the cross-sectional uniformity of the precipitated phase distribution.
[0039] (7) Calculation of total nonuniformity η Substitute the four sub-items of unevenness into the overall control formula according to the predetermined weights: η=0.35·η_T+0.30·η_ε+0.20·η_c+0.15·η_w; The obtained η is the total non-uniformity of the cross-section. The physical meaning of η is the weighted sum of the non-uniformity of four process dimensions: temperature field, strain field, cooling field, and weld microstructure, rather than a direct weighted calculation of tensile strength and conductivity. Tensile strength data is used to calculate η_w and provide mechanical fluctuation auxiliary verification CV_R, and conductivity data is used to provide electrical fluctuation auxiliary verification CV_σ. The three together constitute a verifiable chain of evidence for η.
[0040] When the relative fluctuation of the η value of the three sets of cross-sectional samples (head, middle, and tail) along the length direction is ≤3%, and CV_R≤8% and CV_σ≤5%, the quantitative control method is deemed to have met the mass production stability requirements.
[0041] Basis for determining weighting coefficients: To determine the contribution percentage of the four component nonuniformities to the overall performance nonuniformity, the inventors designed a four-factor, three-level orthogonal experiment (L9(3)). 4 The influence of each factor was quantified and ranked using grey relational analysis to determine the final weight coefficients. The specific process is as follows.
[0042] (1) Orthogonal experimental design Using a 50×6mm 6061 aluminum alloy busbar as the test platform, four factors were selected: temperature field nonuniformity η_T, strain field nonuniformity η_ε, cooling rate nonuniformity η_c, and weld microstructure nonuniformity η_w. Each factor was set to three levels: low, medium, and high (achieved by adjusting parameters such as the difference in the working zone length of the die, the speed of the extrusion roller, the cooling water pressure, and the depth of the welding chamber). The total nonuniformity of the cross-sectional properties η was used as the evaluation index. The test scheme and results are shown in Table 1.
[0043] Table 1 Orthogonal experimental scheme L9(3) 4 ) and results
[0044] Note: In the table, η_T, η_ε, η_c, and η_w are all dimensionless percentages calculated using the aforementioned method.
[0045] (2) Grey relational analysis The minimum total unevenness η of each experiment (11.6% in this example) is used as the reference sequence X0, and the four factor sequences are X1 (η_T), X2 (η_ε), X3 (η_c), and X4 (η_w). Following the steps of classic grey relational analysis: The original data is subjected to mean-dimension-free processing; Calculate the absolute difference between each comparison sequence and the reference sequence; With the resolution coefficient ξ=0.5, calculate the correlation coefficient γ(x0(k),xᵢ(k)); Calculate the average correlation rᵢ of each factor across all test points.
[0046] The calculation results are shown in Table 2.
[0047] Table 2 Results of Grey Relational Analysis
[0048] The correlation degree ranking is: η_T>η_ε>η_c>η_w, indicating that the temperature field has the greatest impact on the total non-uniformity, while the weld microstructure has the least impact. After normalizing the correlation degree, the weighting coefficients are obtained as follows: w_T=0.35, w_ε=0.30, w_c=0.20, w_w=0.15.
[0049] (3) Verification of weighting coefficients Substituting the above weights into the actual test data of Example 1 (50×6mm 6061): η_T=5.1% (temperature difference 26℃ / average temperature 510℃), η_ε=4.0% (obtained from finite element simulation), η_c=12.5% (edge cooling rate 36℃ / s, center cooling rate 32℃ / s), η_w=3.0% (base strength 265MPa, weld strength 257MPa), the calculation yields: η=0.35×5.1+0.30×4.0+0.20×12.5+0.15×3.0=1.785+1.200+2.500+0.450=5.935%; The total non-uniformity of 7.8% measured directly in Example 1 deviates from the actual value (because the weighting coefficient is based on the statistical mean of orthogonal experiments, while individual examples exhibit random fluctuations), but the two are on the same order of magnitude and show a consistent trend, verifying the effectiveness of the weighting allocation. In practical engineering applications, the weighting coefficient can be used for direct calculation, or it can be fine-tuned after a small number of calibration tests for specific alloys and specifications.
[0050] Quantitative Design of Mold Structure – Synergistic Control of Strain Field and Weld Uniformity: This method is suitable for mold systems with uniform preheating (without zoned temperature control). It controls the uniformity of the strain field through differentiated working zone design and improves the weld quality through welding chamber depth matching design, thereby reducing the inherent level of non-uniformity from the tooling source.
[0051] Differentiated working zone design (strain field control): The larger the aspect ratio, the more significant the natural velocity difference in the lateral flow of metal. By using a differentiated working zone structure with a "longer center and shorter edges," the natural velocity difference is offset by the difference in flow resistance, achieving uniform velocity discharge across the entire cross-section. Strain field non-uniformity control formula: ; Detailed explanation of variables: The cross-sectional width of the aluminum busbar, in mm, is a core geometric dimension variable. The larger the width, the longer the lateral expansion distance of the metal, and the greater the flow velocity difference naturally becomes. : Aluminum busbar cross-sectional thickness, in mm. The greater the thickness, the higher the overall resistance to metal flow, but the lower the relative proportion of the lateral velocity difference. Aspect ratio (width-to-height ratio), dimensionless, is the core geometric indicator that determines strain unevenness; The difference in working zone length between the center and the edge, in mm, is defined as the difference between the working zone length at the center of the die and the working zone length at the edge. It is a core adjustable parameter in die design. The longer the working zone, the greater the frictional resistance between the metal and the die, and the slower the flow rate. : The inherent coefficient of strain non-uniformity, dimensionless, is related to the alloy deformation resistance, the cavity expansion angle structure, and the tonnage of the equipment. The value range for conventional streamlined cavities of 6-series aluminum alloys is 0.08-0.12, and the lower limit is taken for large-tonnage equipment. The working zone velocity compensation coefficient is dimensionless and reflects the ability of the difference in working zone velocity per unit length to compensate for uneven strain rate. It is related to the surface roughness of the mold, lubrication status, and high-temperature friction coefficient of the alloy. The typical value range is 0.6-0.8, and the upper limit is used for nitriding molds.
[0052] Quantitative design rules: Hierarchical design based on aspect ratio: Aspect ratio 3 / 5: Recommended difference in working belt length 0.3 / 0.5mm; Width-to-height ratio 5 / 8: Recommended difference in working belt length 0.6 / 0.9mm; Aspect ratio of 8 / 12: Recommended working belt length difference of 1.0 / 1.4mm. In engineering applications, for every 10mm increase in width, the working belt length difference increases by 0.15 / 0.2mm; for every 1mm increase in thickness, the overall length of the working belt increases by 0.1 / 0.15mm.
[0053] Welding chamber depth matching design (weld quality control): Increasing the weld width requires more feed rods, thus increasing the number of welds. Deepening the weld chamber to increase welding pressure and extending welding time promotes atomic-level bonding at the interface, reducing the difference in microstructure and properties between the weld and the substrate. Weld microstructure inhomogeneity control formula: ; Detailed explanation of variables: The number of longitudinal welds is dimensionless and determined by the width of the aluminum busbar cross-section and the supply capacity of a single bar. Single bar feeding at time, ; Twin-bar feeding, ; Three-pole feeding, ; Welding chamber depth, in mm, is defined as the vertical depth of the cavity from the feed rod confluence point to the die working zone inlet. It is a core mold parameter that determines welding quality. The deeper the welding chamber, the longer the metal remains under high pressure and high temperature, the more fully the interface oxide film breaks down, and the higher the weld strength. : Weld influence coefficient, dimensionless, directly related to the surface cleanliness of the bar material and the welding temperature: 0.15 / 0.20 for bar material after precision peeling, and 0.20 / 0.25 for bar material without peeling.
[0054] Quantitative design rules: The depth of the welding chamber should be designed to be no less than 0.4 times the cross-sectional width, with the following recommended values for different grades: Width 30 / 50mm: Recommended welding chamber depth 15 / 22mm; Width 50 / 80mm: Recommended welding chamber depth 22 / 32mm; For widths of 80 / 120mm, a weld chamber depth of 32 / 45mm is recommended. For every 10mm increase in width, the weld chamber depth should be increased by 2 / 3mm. When the width exceeds the threshold for the number of welds, the weld chamber depth should be increased by an additional 3 / 5mm to offset the quality degradation caused by the addition of new welds.
[0055] Extrusion process parameter matching and control—temperature field uniformity control: Under overall mold preheating conditions, by quantitatively matching the extrusion speed and reduction rate, the total heat generation and rate of heat generation during deformation are controlled, thus weakening the central heat accumulation effect and suppressing natural temperature field unevenness. Temperature field non-uniformity control formula: ; Detailed explanation of variables: The extrusion roller speed, measured in r / min, is a core process parameter that can be adjusted in real time during production. The faster the speed, the greater the amount of metal deformation per unit time, the higher the rate of heat generation from friction and deformation, the more significant the heat accumulation at the center, and the greater the temperature difference across the cross-section. The bar reduction ratio, dimensionless (usually expressed as a percentage), is defined as the proportion of the reduction deformation of the bar by the extrusion rollers to the original diameter of the bar. A higher reduction ratio indicates a higher degree of plastic deformation, resulting in more heat generated during deformation and friction, and a simultaneous increase in both overall temperature rise and cross-sectional temperature difference. : Average extrusion temperature of cross section, in °C, refers to the average temperature of the cross section when aluminum is discharged from the die. The reasonable range for 6 series aluminum alloys is 480-550°C, and it is usually controlled at 500-520°C. Temperature change heat generation coefficient, unit ℃・mm / (r・min), reflects the increase in cross-sectional temperature difference per unit width, rotation speed, and reduction rate. It is related to the alloy deformation resistance, thermal conductivity, and mold heat dissipation conditions. The typical value range for 6-series aluminum alloys is 1.2-1.8, and the lower limit is used for water-cooled molds.
[0056] Quantitative control rules: 1. Based on the 50×6mm specification, the recommended extrusion roller speed is 2.0 / 2.5 r / min, and the reduction rate is 18% / 22%; 2. For every 10mm increase in width, the extrusion roller speed is reduced by 0.2-0.3 r / min to decrease the heat accumulation at the center by slowing down the heat generation rate; 3. For every 1mm increase in thickness, the reduction rate increases by 1.5%-2%, ensuring sufficient overall deformation while matching heat generation balance; 4. The reduction rate shall not be less than 15%, otherwise the welding pressure will be insufficient and the weld quality will be reduced; it shall not be higher than 28%, otherwise the equipment load will be too large and the rod material will easily slip.
[0057] Online cooling homogenization control – control of cooling field and precipitated phase uniformity: To address the issue of insufficient cooling rate at the center of large cross-sections, a zoned independent cooling architecture is adopted. This compensates for the thickness thermal resistance by increasing the cooling intensity in the central region, reducing the difference in cooling rate across the cross-section and ensuring that the entire cross-section reaches the critical solution cooling rate. The formula for controlling cooling rate non-uniformity is as follows: ; Detailed explanation of variables: The thickness of the aluminum busbar cross-section, measured in mm, is the core source of cooling thermal resistance. Heat dissipation from the aluminum busbar primarily relies on its two large surface areas. The greater the thickness, the greater the thermal resistance from the center to the surface, resulting in a slower cooling rate at the center and a greater difference in cooling rate between the edge and the center. Width has a much smaller impact on cooling than thickness, and is simplified by incorporating a coefficient. The central cooling water pressure, measured in MPa, is a core adjustable parameter in the online cooling process. The cooling system is divided into a central cooling zone and an edge cooling zone along the width of the aluminum busbar, each equipped with an independent nozzle array and pressure regulating valve. The heat transfer intensity is increased by raising the water pressure in the central zone. Cooling thermal resistance coefficient, unit (℃ / s) / mm, reflects the increase in cooling rate per unit thickness. The typical value is 0.15-0.20 under high-pressure water mist cooling, and the value doubles under pure air cooling. Water pressure cooling efficiency coefficient, unit (℃ / s) / MPa, reflects the increase in cooling rate caused by a unit increase in water pressure. It is related to nozzle orifice diameter, spray angle and spray distance. The typical value is 12-18 under standard atomizing nozzle.
[0058] Supplementary correction: When the aluminum busbar width is greater than 80mm, the proportion of side heat dissipation is further reduced, and the formula needs to be multiplied by a correction factor. (W is in mm).
[0059] Quantitative control rules: 1. The cooling medium should preferably be a high-pressure air-water mixture mist, which balances cooling efficiency and deformation control, and avoids excessive residual stress caused by pure water cooling; 2. The nozzles are arranged symmetrically in the upper and lower and left and right sides of the cooling section to avoid lateral bending and warping caused by uneven cooling on one side. The nozzles are at a 45° angle to the surface of the profile, and the spray distance is 100-150mm. 3. For every 1mm increase in thickness, the cooling water pressure in the central area increases by 0.10-0.15MPa to ensure a cooling rate of ≥28℃ / s at the center of the cross-section; 4. For every 10mm increase in width, add 1-2 sets of nozzles in the central area to ensure uniform cooling coverage.
[0060] On-site rapid verification criteria: Without requiring complex calculations or organizational testing, meeting the following three core intermediate indicators guarantees a total non-uniformity of cross-sectional performance η≤10%, achieving industrial-grade high-performance requirements: 1. Maximum temperature difference of discharge cross section ≤30℃: The recrystallization temperature range of 6 series aluminum alloy is 350-450℃. When the temperature difference is less than 30℃, the recrystallization kinetics difference in different regions can be controlled and the grain size difference does not exceed 2 times. 2. Cooling rate at the center of the cross section ≥ 28℃ / s: close to the critical cooling rate for 6-series aluminum alloys to obtain a fully supersaturated solid solution, which can ensure that the Mg2Si phase does not precipitate prematurely on a large scale; 3. Welding chamber depth ≥ 0.4 times the cross-sectional width: This provides sufficient welding pressure and dwell time to ensure atomic bonding at the weld interface, with a weld strength coefficient ≥ 0.9.
[0061] Example 1: 50×6mm 6061 aluminum alloy new energy power battery busbar Basic parameters: Finished product width ,thickness Aspect ratio ≈ 8.3, twin-bar feeding, number of welds With a fixed length of 6m, it is used for internal conductive connections in power battery packs.
[0062] Mold parameters: Center working strip length 1.4mm, edge working strip length 0.6mm, working strip length difference Depth of welding chamber It meets the 0.4 times width requirement; the mold cavity adopts a two-stage streamline expansion, with a first-stage expansion angle of 15° and a second-stage expansion angle of 6°, and the cavity corners are rounded with a radius of R5mm.
[0063] Extrusion process: Overall die preheating temperature 420℃, φ20mm aluminum rod preheating temperature 400℃; extrusion roller speed... Sliming rate The rod material undergoes precision peeling and ultrasonic alkaline washing, removing 0.3mm of oxide film from the surface, and is protected by argon gas before feeding.
[0064] Cooling parameters: The cooling system is divided into a central zone and an edge zone along its width, with independent water supply and pressure regulation; the central zone cooling water pressure... The cooling water pressure in the edge area is 0.4MPa; the upper and lower symmetrical high-pressure water mist cooling is used, and the length of the cooling section is 3m.
[0065] Verification results: Thermal performance indicators: average temperature of discharge section is 510℃, maximum temperature difference of cross section is 26℃; cooling rate of cross section center is 32℃ / s, all of which meet the control criteria. Microstructure: The average grain size in the central region is about 45 μm, in the edge region it is about 58 μm, and the maximum grain size in the transition region is 80 μm, with no abnormally large grain bands; the grain size in the weld area is about 25 μm, the interface is intact, and there are no micropores or continuous oxide films. Mechanical properties: The average tensile strength of the cross section is 265 MPa, with a maximum difference of 18 MPa and a relative fluctuation of 6.8%; the average elongation is 12.5%, and the elongation at the weld is 11.2%. Electrical conductivity: The average cross-sectional conductivity is 56% IACS, with a maximum difference of 2.3% IACS and a relative fluctuation of 4.1%. Processing performance: No cracks were found in the 180° cold bending test (bending mandrel diameter equals thickness), and the bending pass rate was 100%. Uniformity calculation: Total non-uniformity It meets the requirement of ≤8% for high-performance busbars.
[0066] 5. Vertical performance fluctuations (mass production stability verification) On a product of the same fixed length of 6m, a set of cross-sectional samples were taken from the head (0.5m from the starting end), the middle (3m), and the tail (5.5m). The tensile strength and electrical conductivity were tested using the aforementioned method. The results are as follows:
[0067] Longitudinal fluctuations: relative fluctuations in tensile strength ≤2.3%, and relative fluctuations in electrical conductivity ≤0.9%. This indicates that the method not only achieves excellent uniformity within the cross-section but also maintains high performance consistency along the entire product length, effectively overcoming the performance fluctuation problems at the beginning, middle, and end of the traditional continuous extrusion process caused by factors such as temperature drift and bar material connection. This fully demonstrates the mass production stability advantage of the quantitative control method.
[0068] Comparative Example 1: Preparation of 50×6mm 6061 aluminum busbars of the same specifications using traditional empirical processes The process of using small-sized profiles, which is common in the industry, is adopted. No quantitative design for size matching is performed. All other raw materials and equipment conditions are completely consistent with those in Example 1.
[0069] Process parameters: uniform working zone (total length 1.0mm, no length difference), welding chamber depth 15mm, extrusion roller speed 2.5r / min, reduction rate 20%, uniform cooling water pressure across the entire cross section 0.5MPa.
[0070] Comparison results: Thermal properties: Maximum temperature difference at the discharge section is 62℃, and the central cooling rate is 14℃ / s, which is far below the critical solution cooling rate. Microstructure: The central region has coarse grains up to 120 μm, the edges retain a large number of deformed substructures, and the transition region has abnormally large grains of more than 200 μm; the weld area has continuous oxide film inclusions and micropores. Mechanical properties: The tensile strength of the cross section fluctuated by 17.2%, the weld strength coefficient was only 0.81, and the elongation fluctuated by 25%. Electrical conductivity: The conductivity fluctuates by 9.5%. The central region has higher conductivity and lower strength due to coarsening of the precipitated phase, resulting in poor performance matching. Processing performance: The cracking rate at the weld reached 12% in the 180° bending test, and the delamination rate at the edge of the punching process was 8%; Uniformity calculation: Total non-uniformity It cannot meet the usage requirements of high-end new energy fields.
[0071] Example 2: 80×8mm 6101B photovoltaic power station conductive bus: Basic parameters: Finished product width ,thickness Aspect ratio = 10, three-bar parallel feeding, number of welds (Symmetrically distributed at 1 / 4 width from the edge), fixed length 8m, used for AC side conductive connection of photovoltaic inverter.
[0072] Mold parameters: Center working strip length 1.7mm, edge working strip length 0.7mm, working strip length difference Depth of welding chamber It just meets the 0.4 times width threshold; a shear ridge structure is set in the welding chamber to strengthen the breaking of the oxide film in the weld.
[0073] Extrusion process: Die preheating temperature 415℃, bar preheating temperature 395℃; Extrusion roller speed... Sliming rate The three-bar feeding system adopts a servo synchronous control system, and the feeding speed deviation is ≤0.5%.
[0074] Cooling parameters: Central cooling water pressure The cooling water pressure in the edge zone is 0.5MPa; two additional sets of nozzles are added in the center zone, and the cooling section is 3.5m long.
[0075] Verification results: Thermal properties: Average temperature of the discharge section is 505℃, maximum temperature difference of the cross section is 28℃; cooling rate at the center of the section is 30℃ / s, reaching the critical solution treatment requirement; Microstructure: The average grain size of the matrix is 50-65μm, the microstructure of the two welds is uniform, and there is no obvious interface with abrupt change in performance. Mechanical properties: Average tensile strength of the cross section is 240 MPa, with a relative fluctuation of 7.5%; Conductivity: Average conductivity 58% IACS, relative fluctuation 4.8%, meeting the high conductivity requirements of the photovoltaic industry; Processing performance: Both welds passed the 180° bend test; punching and shearing processes showed no delamination or cracking. Uniformity calculation: Total non-uniformity It meets the industrial-grade high performance requirement of ≤10%.
[0076] Example 3: 30×4mm 6063 universal power distribution aluminum busbar Basic parameters: Finished product width ,thickness Aspect ratio = 7.5, twin-bar feeding, number of welds The standard length is 6m, and it is used for the busbars of low-voltage distribution cabinets.
[0077] Mold parameters: Center working strip length 1.1mm, edge working strip length 0.5mm, working strip length difference Depth of welding chamber It meets the 0.4 times width requirement; the first-level expansion angle is 12°, and the second-level expansion angle is 5°.
[0078] Extrusion process: Die preheating temperature 430℃, bar preheating temperature 410℃; Extrusion roller speed... Sliming rate The rod material is treated with ordinary alkaline washing.
[0079] Cooling parameters: Central cooling water pressure The cooling water pressure in the edge area is 0.35MPa; the cooling section length is 2.5m, and it uses conventional water mist cooling.
[0080] Verification results: Thermal performance indicators: maximum temperature difference at the discharge section is 22℃, central cooling rate is 35℃ / s, and the solution treatment effect is sufficient; Mechanical properties: Average tensile strength of cross section is 220 MPa, with a relative fluctuation of 5.2%; Electrical conductivity: Average conductivity 57% IACS, relative fluctuation 3.3%; Processing performance: 100% weld bending qualification rate, punching burr height ≤0.1mm; Uniformity calculation: Total non-uniformity The homogenization effect is far superior to the approximately 12% unevenness level of products of the same specifications produced by traditional processes, verifying that this method also has a significant homogenization effect on small and medium-sized products.
[0081] Example 4: Large cross-section busbar of 100×10mm 6061 energy storage power station Basic parameters: Finished product width ,thickness Aspect ratio = 10, three-bar feeding, number of welds With a standard length of 10m, it is used in high-current conductive busbars on the DC side of industrial and commercial energy storage power stations.
[0082] Mold parameters: Center working strip length 1.9mm, edge working strip length 0.7mm, working strip length difference Depth of welding chamber It is slightly higher than the basic requirement of 0.4 times the width; the mold cavity adopts a three-stage streamline expansion, gradually reducing the expansion angle to avoid flow dead zones.
[0083] Extrusion process: Die preheating temperature 410℃, bar preheating temperature 390℃; Extrusion roller speed... Sliming rate It is equipped with a three-bar synchronous feeding system that provides real-time feedback and adjusts the feeding pressure.
[0084] Cooling parameters: Central cooling water pressure The cooling water pressure in the edge area is 0.55MPa; the central area adopts a double-row dense nozzle arrangement, and the total length of the cooling section is 4m.
[0085] Verification results: Thermal performance indicators: average temperature of discharge section is 500℃, maximum temperature difference of cross section is 29℃, controlled within the 30℃ threshold; cooling rate of cross section center is 29℃ / s, close to the critical solution cooling rate. Microstructure: The matrix grain size is 55-75μm, there are no abnormally large grains in the transition zone, and the weld interface is intact; Mechanical properties: Average tensile strength of cross section is 255 MPa, with a relative fluctuation of 8.2%; Electrical conductivity: Average conductivity 55.5% IACS, relative fluctuation 5.3%; Processing performance: No cracks were found when the weld was bent at 90°, and no local overheating was observed during high current energization testing; Uniformity calculation: Total non-uniformity This achieves uniform performance control of aluminum bars with widths of up to 100 millimeters, breaking through the application limitations of traditional continuous extrusion processes with widths below 60mm.
[0086] Comparative Example 2: 50×6mm 6061 aluminum busbar with insufficient working belt length difference Only the parameters of the mold working belt were adjusted, while the other conditions were completely consistent with those in Example 1, to verify the effect of the differentiated working belt.
[0087] Variable setting: Difference in length between center and edge working zones The value is far lower than the recommended 0.8 mm in this method, and the flow rate difference caused by the wide width is not fully compensated.
[0088] Comparison results: Deformation and Flow: After discharge, the profile exhibits obvious lateral bending, with a planar waviness of up to 2mm / m and dimensional deviations. Microstructure: The central region has a large amount of deformation and fine grains, while the edge region has insufficient deformation and retains a large amount of fibrous structure, resulting in a significant increase in cross-sectional strain non-uniformity. Performance data: tensile strength cross-sectional fluctuation 12.1%, electrical conductivity fluctuation 7.3%; Uniformity calculation: Total non-uniformity Compared to Example 1, the performance deteriorated significantly, verifying the core regulatory role of the differentiated working zone design in the uniformity of the strain field.
[0089] Comparative Example 3: 80×8mm 6101B aluminum busbar with insufficient welding chamber depth Only the welding chamber depth parameter was adjusted, and all other conditions were completely consistent with those in Example 2 to verify the effect of the welding chamber depth.
[0090] Variable setting: Welding chamber depth This is far below the 32mm recommended by this method and does not conform to the design rule of 0.4 times the width.
[0091] Comparison results: Weld quality: Both welds have obvious oxide film inclusions and micropores, and the weld interface is not fully bonded; Performance data: Weld strength coefficient is only 0.78, cross-sectional tensile strength fluctuates by 11.5%, and electrical conductivity fluctuates by 8.6%; Processing performance: The weld cracking rate reached 22% in the 180° bending test, becoming the main source of product failure; Uniformity calculation: Total non-uniformity The proportion of weld-related non-uniformity increased significantly, verifying the decisive role of weld chamber depth matching design in the weld quality of wide products.
[0092] Comparative Example 4: 100×10mm 6061 aluminum busbar with excessively high extrusion speed Only the extrusion wheel speed parameter was adjusted, and all other conditions were exactly the same as in Example 4, to verify the effect of speed matching.
[0093] Variable setting: Extrusion roller speed The rotation speed was not reduced proportionally to the increase in width, resulting in an excessively rapid rate of heat generation during deformation.
[0094] Comparison results: Temperature field: The maximum temperature difference at the discharge section is 58℃, and the peak temperature in the central region reaches 565℃, which is close to the overheating temperature of 6061 alloy, posing a risk of grain boundary melting. Microstructure: The grains in the central region grow abnormally to more than 150 μm, and overheated structures appear locally. The deformation in the edge region is insufficient and recrystallization is incomplete. Performance data: Tensile strength cross-sectional fluctuation of 16.8%, with the strength in the central area significantly lower than that at the edges; conductivity fluctuation of 10.2%. Uniformity calculation: Total non-uniformity Uneven temperature field became the most significant deterioration factor, verifying the crucial role of extrusion speed matching and control in ensuring temperature uniformity of large-size products.
[0095] Optional extensions and variations: Micro-dispersion alloying strengthening. For applications requiring extremely high uniformity, 0.08%-0.15% Zr or Sc can be added to 6-series aluminum alloys to form high-temperature stable nanoscale Al3Zr / Al3Sc dispersed phases, which pin grain boundaries and subgrain boundaries, suppress the abnormal growth of oversized grains in the transition region, and further reduce the total non-uniformity by 1%-2%.
[0096] Ultrasonic vibration-assisted extrusion. Applying high-frequency ultrasonic vibration to the die welding chamber can reduce the metal's resistance to deformation and improve the uniformity of lateral flow. It can also break up oxide film inclusions at the weld, thereby improving the welding quality. This method is particularly suitable for the preparation of ultra-wide aluminum busbars with an aspect ratio greater than 10.
[0097] The system features a dual-stage aging heat treatment process. Offline aging employs a dual-stage process of "low-temperature nucleation + high-temperature growth," which involves holding at 115 / 125℃ for 3 / 4 hours, followed by raising the temperature to 155 / 165℃ and holding for 5 / 8 hours. This promotes the homogenization of precipitated phases between the high-supersaturation region at the edge and the low-supersaturation region at the center, further reducing performance differences while also ensuring a balance between strength and conductivity.
[0098] Straightening and stress relief are combined for long-length products. For products with a length of 8m or more, a combination of "roller straightening + small deformation stretching straightening" process is used, with the stretching deformation controlled at 0.5% / 1%. This is followed by low-temperature stress relief annealing at 200 / 230℃ for 2-3 hours to eliminate residual stress from cooling and heat treatment, ensuring the dimensional stability and reliability of long-length products.
[0099] Beneficial effects: 1. Significantly improved development efficiency and reduced R&D costs. A quantitative mapping rule for size-mold-process-cooling has been established, replacing the traditional experience-based trial and error model. This eliminates the need for repeated mold repairs and adjustments, shortening the new product development cycle from 1-2 months to less than 2 weeks. Material waste in trial molding has been reduced by more than 60%, significantly reducing R&D and mass production introduction costs.
[0100] 2. A qualitative leap in product uniformity, achieving performance consistency that meets high-end application standards. Through multi-dimensional collaborative control, the overall performance non-uniformity of large-size aluminum profiles has been reduced from 15%-20% in traditional processes to 8%-10%, achieving a uniformity level comparable to that of small-size profiles. This completely solves the industry pain points of large performance fluctuations and poor batch stability in large-size products, meeting the stringent requirements of high-end fields such as new energy and photovoltaics.
[0101] 3. Significantly improved weld quality and processing yield, enhancing product reliability. The depth-matched welding chamber design, combined with clean material treatment, increased the weld strength coefficient from 0.8 to over 0.92, and the bending processing qualification rate from 85% to over 98%, effectively reducing the scrap rate in subsequent processing and the failure risk in end-use applications.
[0102] 4. Highly adaptable to engineering implementation, compatible with existing production lines and all product specifications. The entire method is designed based on existing mainstream continuous extrusion equipment, eliminating the need for expensive new equipment such as zone heating and ultrasonic assistance. It can be implemented simply through mold optimization and process parameter matching, and can be directly promoted and applied. At the same time, it covers aluminum busbar products with a full width range of 25-120mm, and is suitable for multiple application fields such as new energy, photovoltaics, and power distribution.
[0103] 5. Improved mass production stability and reduced overall manufacturing costs. Quantified process rules avoid human experience differences, and the performance fluctuation between batches is controlled within 3% during mass production. The yield rate has increased from about 70% in traditional processes to over 90%, and the overall manufacturing cost has been reduced by about 15%.
[0104] The above-disclosed embodiments are merely one or more preferred embodiments of this application and should not be construed as limiting the scope of this application. Those skilled in the art can understand that all or part of the processes for implementing the above embodiments and equivalent changes made in accordance with the claims of this application still fall within the scope of this application.
Claims
1. A method for quantitatively controlling the uniformity of the continuous extrusion cross-section of large-size aluminum alloy busbars, characterized in that, Includes the following steps: By defining the total non-uniformity of cross-sectional properties as the control objective, a total control model is established, which consists of a weighted summation of temperature field non-uniformity, strain field non-uniformity, cooling rate non-uniformity, and weld microstructure non-uniformity, and quantitative evaluation indicators are obtained. By performing quantitative design of the mold structure, the uniformity of the strain field and the quality of the weld after regulation are obtained; The uniformity of the temperature field after adjustment is obtained by matching and controlling the extrusion process parameters; By implementing online cooling uniformity control, the uniformity of the regulated cooling rate is obtained; The temperature field, strain field, cooling rate and weld microstructure were tested separately, and the total non-uniformity of cross-sectional properties was calculated according to the overall control model. The large-size wide aluminum alloy busbar with the total non-uniformity of cross-sectional properties meeting the target threshold requirement was obtained.
2. The method for quantitatively controlling the uniformity of the continuous extrusion cross-section of large-size aluminum alloy busbars as described in claim 1, characterized in that, The section "By defining the total non-uniformity of cross-sectional properties as the control objective, establishing a total control model composed of a weighted summation of temperature field non-uniformity, strain field non-uniformity, cooling rate non-uniformity, and weld microstructure non-uniformity, and obtaining quantitative evaluation indicators" includes the following steps: By defining four sub-items of non-uniformity—temperature field non-uniformity, strain field non-uniformity, cooling rate non-uniformity, and weld microstructure non-uniformity—quantitative indicators for each item are obtained. The overall control model is obtained by determining the weighting coefficients of the four sub-items: temperature field, strain field, cooling rate, and weld microstructure.
3. The method for quantitatively controlling the uniformity of the continuous extrusion cross-section of large-size aluminum alloy busbars as described in claim 2, characterized in that, The section on "Obtaining the Uniformity of the Controlled Strain Field and the Quality of the Weld through Quantitative Design of the Mold Structure" includes the following steps: By designing a differentiated working zone length difference according to the principle of lengthening the center and shortening the edges, the strain field uniformity that offsets the natural flow velocity difference is obtained; By designing the welding chamber depth to be no less than 0.4 times the cross-sectional width, weld quality with increased welding pressure can be obtained.
4. The method for quantitatively controlling the uniformity of the continuous extrusion cross-section of large-size aluminum alloy busbars as described in claim 3, characterized in that, The step of "obtaining the uniformity of the temperature field after adjustment by matching and controlling the extrusion process parameters" includes the following steps: By matching the rotation speed according to the rule of increasing the width and decreasing the rotation speed of the extrusion roller, the uniformity of the temperature field with reduced central heat accumulation is obtained; By matching the reduction rate according to the rule of increasing the thickness of the lifting rod material, the uniformity of the temperature field is obtained to ensure the balance between deformation and heat generation.
5. The method for quantitatively controlling the uniformity of the continuous extrusion cross-section of large-size aluminum alloy busbars as described in claim 4, characterized in that, The step of "obtaining regulated cooling rate uniformity through online cooling homogenization control" includes the following steps: By adopting a partitioned independent cooling architecture, the cooling rate of each partition can be adjusted. By increasing the cooling water pressure in the central region to compensate for the thickness thermal resistance, a uniform cooling rate is achieved, reducing the difference in cooling rate between the center and the edge.
6. The method for quantitatively controlling the uniformity of the continuous extrusion cross-section of large-size aluminum alloy busbars as described in claim 5, characterized in that, The process of "inspecting four dimensions—temperature field, strain field, cooling rate, and weld microstructure—and calculating the total non-uniformity of cross-sectional properties according to the overall control model to obtain a large-size, wide-width aluminum alloy busbar whose total non-uniformity of cross-sectional properties meets the target threshold requirements" includes the following steps: The test sample is obtained by selecting measuring points along the width direction and taking cross-sectional samples along the length direction at the aluminum discharge end; Four sub-items of non-uniformity were obtained by detecting the temperature field, strain field, cooling rate, and weld microstructure respectively. The total non-uniformity of cross-sectional performance is obtained by substituting the four sub-items into the overall control model according to their weights.