A multi-stage step-by-step deload forming method for Φ1600mm grade titanium alloy forgings

By using a split mold and a step-by-step forging method, the forming problem of Φ1600mm titanium alloy disc forgings on an 800MN press was solved, resulting in a significant reduction in load and mold maintenance costs, and improved microstructure and properties of the forgings.

CN123102897APending Publication Date: 2026-11-17CHINA NAT ERZHONG GRP DEYANG WANHANG DIE FORGING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611368405.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-04
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies make it difficult to safely and stably manufacture Φ1600mm titanium alloy disc forgings on an 800MN press, especially how to achieve automatic densification of the die under forging pressure during operation and how to coordinate the step-by-step forming strategy with the die's split structure.

Method used

The mold adopts a split mold, including an upper mold and a lower mold. The lower mold consists of a central mold core and radial split modules. The self-locking is achieved through the inclined surface cooperation. The opening and closing of the diversion channel is controlled. The step-forging process is divided into free forging upsetting rough billet, pre-forging diversion and load reduction filling, and final forging finishing. The radial component force is used to decompose the load and avoid metal accumulation.

Benefits of technology

It significantly reduces forming load, with a maximum load reduction of over 45%, enabling Φ1600mm-level titanium alloy disc die forging. It also reduces die maintenance costs by 60%, improves the microstructure and properties of forgings, and is suitable for various titanium alloys and high-temperature alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102897A_ABST
    Figure CN123102897A_ABST
Patent Text Reader

Abstract

This invention discloses a multi-stage, step-by-step load-reducing forming method for Φ1600mm titanium alloy forgings, belonging to the field of titanium alloy disc forging forming and manufacturing technology. It solves the problem in existing technologies where the peak load far exceeds the limits of existing presses. The forming method uses a split-type mold and includes the following steps: S1, free forging upsetting of the rough billet, assembling a flat anvil mold on the upper mold, fitting the radial split module with the central mold core, closing the flow channel of the lower mold, and axially pressing down the upper mold; S2, pre-forging flow-reducing filling, replacing the upper mold with the final forging mold, separating the radial split module from the central mold core, opening the flow channel of the lower mold, and axially pressing down the upper mold; S3, final forging finishing, fitting the radial split module with the central mold core, closing the flow channel of the lower mold, and axially pressing down the upper mold. The multi-stage step-by-step load reduction forming method for Φ1600mm grade titanium alloy forgings provided by this invention is used in the manufacturing of Φ1600mm grade titanium alloy forgings, which significantly reduces the forming load and can complete Φ1600mm grade titanium alloy disc die forging on an 800MN press.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of titanium alloy disc forging forming and manufacturing technology, specifically, it relates to a multi-stage step-by-step load reduction forming method for Φ1600mm grade titanium alloy forgings. Background Technology

[0002] Titanium alloys are widely used in key load-bearing components such as fan discs and compressor discs in aero engines due to their high specific strength, corrosion resistance, and excellent high-temperature mechanical properties. As the thrust-to-weight ratio of engines continues to increase, the size of disc components continues to grow, and the next generation of high-bypass turbofan engines requires the projected diameter of the fan disc to reach or exceed Φ1600mm.

[0003] Currently, the largest tonnage die forging press in the world is 800MN. For a Φ1600mm titanium alloy disc, if traditional one-time integral final forging is used, the required peak load far exceeds the limit of existing presses due to the high resistance of titanium alloy to high-temperature deformation and the multiplication effect of projected area.

[0004] Several technical solutions exist to address this issue. For example, the localized loading forging method uses internal and external washers for segmented forging, but it is mainly applicable to annular forgings and has limited adaptability to solid fan discs. Using a combination of pre-forging and final forging dies, along with a "multi-fire billet preparation + die forging" process, can reduce the load, but its two-step forming still does not sufficiently reduce the load on Φ1600mm discs. Other process studies focus on optimizing upsetting parameters and die forging temperature, without providing a systematic load-reducing forming strategy.

[0005] Regarding the mold, the split-inlay assembly structure uses multiple fan-shaped modules assembled and axially locked by a pre-tightening ring. This structure bears a significant radial force during forging, and separation gaps easily form between the fan-shaped modules, resulting in burrs and flash. Simultaneously, the splicing surface of the fan-shaped blocks is a radial plane, and differences in thermal expansion at high temperatures cause variations in the fit clearance. Furthermore, the mold's split design lacks coordination with the step-by-step forming process, resulting in a mismatch between the stress area at each stage and the projected area of ​​the billet, thus failing to fully realize the load reduction effect.

[0006] In summary, existing technologies have not yet solved the systemic challenges of safely and stably manufacturing Φ1600mm titanium alloy disc forgings on an 800MN press, particularly in achieving automatic die densification under forging pressure during operation and ensuring the synergy between the step-by-step forming strategy and the die's modular structure. Therefore, there is an urgent need to develop a novel forming method and matching die that can significantly reduce forming load. Summary of the Invention

[0007] The present invention provides a multi-stage step-by-step load reduction forming method for Φ1600mm grade titanium alloy forgings, which significantly reduces the forming load and can complete Φ1600mm grade titanium alloy disc die forging on an 800MN press.

[0008] To achieve the above objectives, the technical solution adopted by the present invention is as follows: This invention discloses a multi-stage, step-by-step load reduction forming method for Φ1600mm grade titanium alloy forgings. The forming method employs a split-type mold, comprising an upper mold and a lower mold used in conjunction. The upper mold is an integral structure, and depending on the forming steps, it can be equipped with either a flat anvil mold or a final forging mold. The cavity of the final forging mold mates with the upper surface of the forging blank. The lower mold includes a frustum-shaped central core and radially split modules. The central core is fixedly mounted on the lower mold base, and multiple radially split modules are evenly distributed circumferentially around the central core, with the radially split modules facing away from the central core. Alternatively, the radially split module can be slidably disposed on the lower mold base in a direction close to the central mold core. The inner surface of the radially split module is an inclined surface that mates with the outer surface of the central mold core. When the inner surface of the radially split module is in contact with the outer surface of the central mold core, the inner surface of the radially split module is located at the top of the outer surface of the central mold core. The radial gap between adjacent radially split modules forms a diversion channel. When the inner surface of the radially split module is separated from the outer surface of the central mold core, the diversion channel is opened. When the inner surface of the radially split module is in contact with the outer surface of the central mold core, the diversion channel is closed. The forming method includes the following steps: S1. Free forging and upsetting of rough billet: The upper die is assembled into a flat anvil die, and the radial split module is controlled to slide towards the central die core, so that the inner side of the radial split module is in contact with the outer side of the central die core, and the flow channel of the lower die is closed; the titanium alloy billet is heated and placed in the center of the cavity of the lower die, and the flat anvil die is controlled to be pressed down axially to perform free forging and upsetting of the titanium alloy billet into an upsetting billet, and the lower end of the titanium alloy billet forms a positioning contour with the cavity of the lower die; S2. Pre-forging diversion and load reduction filling: Replace the upper die with the final forging die, control the radial split module to slide away from the central die core, so that the inner side of the radial split module separates from the outer side of the central die core, the diversion channel of the lower die opens, and the cavity diameter of the lower die increases; after reheating the upsetting billet, place it in the center of the cavity of the lower die, control the final forging die to press down axially, pre-forge the upsetting billet into a disc pre-forging part, and discharge the process residue in the spoke area of ​​the disc pre-forging part outward along the opened diversion channel until the rim cavity of the lower die is filled; S3. Final forging and finishing: Control the radial split module to slide towards the central die core, with the inner surface of the radial split module fitting against the outer surface of the central die core. The flow channel of the lower die is closed, and the cavity diameter of the lower die is restored to the design size of the disc forging blank. After reheating the disc pre-forging, place it in the center of the cavity of the lower die. Control the final forging die to press down axially to perform final forging of the disc pre-forging into a disc forging blank. The disc pre-forging continues to fill the cavity of the lower die until the rim cavity of the lower die is completely filled. The process residue discharged through the flow channel is pressed back into the cavity of the lower die and fused with the disc pre-forging body. When the final forging die is pressed down to the designed under-pressure amount, the final dimensional finishing of the disc forging blank is completed.

[0009] Furthermore, the angle between the axis of the frustum-shaped central mold core and the generatrix is ​​α, where 5°≤α≤20°.

[0010] Furthermore, the angle between the axis of the central mold core and the generatrix is ​​10°≤α≤15°.

[0011] Furthermore, the number of radially split modules is 4 to 6.

[0012] Furthermore, the aspect ratio of the titanium alloy billet is 0.8 to 1.2.

[0013] Furthermore, the titanium alloy billet is TC4, TC17, or TA15.

[0014] Furthermore, the free forging upsetting heating temperature of the titanium alloy billet, the pre-forging heating temperature of the upsetting billet, and the final forging heating temperature of the disc pre-forging are all T. β -40℃, where T β This is the β phase transformation point of the titanium alloy.

[0015] The beneficial effects of this invention are: This invention provides a multi-stage step-by-step deload forming method for Φ1600mm grade titanium alloy forgings, which is implemented using a split mold. The upper mold of the split mold can be equipped with a flat anvil mold or a forging final forging mold. The lower mold of the split mold consists of a central mold core and multiple radially arranged split modules. The inner surface of the radial split modules and the outer surface of the central mold core are fitted with inclined surfaces. The downward axial pressure applied by the upper mold is decomposed by the inclined surfaces to generate a radial component force towards the central mold core, pressing each radial split module against the peripheral wall of the central mold core. The greater the axial load, the stronger the locking force. Therefore, no additional locking device is required, and the radial split modules can achieve self-locking by pressing them against the central mold core. The radial gaps between adjacent radial split modules form a diversion channel. When the radial split modules move radially away from the central mold core, the diversion channel is opened. When the radial split modules move radially towards the central mold core, the diversion channel is closed, thus realizing the control of opening or closing the diversion channel. This forming method divides the entire forging process of the disc forging into three stages of loading forging: free forging upsetting rough billet, pre-forging diversion and load reduction filling, and final forging finishing. In each forging stage, the process waste material in the spoke area of ​​the disc pre-forging is guided to be discharged in an orderly manner from the diversion channel by controlling the real-time closing or opening of the diversion channel of the lower die during the pre-forging process, so as to avoid the continuous accumulation of metal in the cavity and the sudden increase of load. This forming method makes the forming force of each forging stage significantly lower than that of a single overall final forging, and the peak load is effectively distributed, thereby realizing the overall die forging of Φ1600mm titanium alloy forgings within the capacity of an 800MN press. Using the multi-stage step-by-step load reduction forming method for Φ1600mm titanium alloy forgings of this invention, the load exceeding 1000MN is decomposed into multiple stage loads not exceeding 800MN, with a maximum load reduction of over 45%, significantly reducing the forming load. Φ1600mm titanium alloy disc forging can be completed on an 800MN press. Utilizing the radial component of the axial pressing pressure of the upper die during forging, each radially segmented module is pressed tightly against the peripheral wall of the central die core. The radially segmented modules and the central die core achieve self-locking; the greater the forging pressing pressure, the stronger the locking force, preventing separation of the radially segmented modules during final forging. It generates flash and burrs; the flow of billet from the center to the rim is controlled by the spacing of the radial split modules, suppressing folding and incomplete filling, and precisely controlling metal flow; each radial split module can be replaced independently, and local wear only requires replacement of the corresponding worn part, reducing mold maintenance costs by more than 60%, thus reducing mold costs and maintenance difficulty; multiple firings and small deformations are beneficial to the dynamic recrystallization and grain refinement of titanium alloys, improving the uniformity of the structure and the microstructure and properties of forgings; it is suitable for titanium alloys such as TC4, TC17, and TA15, and can also be applied to large disc parts of difficult-to-deform materials such as high-temperature alloys and ultra-high-strength steels, with strong adaptability. Attached Figure Description

[0016] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0017] Figure 1 This is a process flow diagram of a multi-stage step-by-step load reduction forming method for Φ1600mm titanium alloy forgings provided in an embodiment of the present invention; Figure 2 This is a cross-sectional view of the inner side of the split module and the outer side of the central mold core fitting together, provided in an embodiment of the present invention. Figure 3 This is a top view of the lower mold's flow channel in the open state according to an embodiment of the present invention; Figure 4 This is a top view of the lower mold's flow channel in the closed state according to an embodiment of the present invention; Figure 5 This is a cross-sectional view of the Φ1600mm grade titanium alloy disc forging blank provided in an embodiment of the present invention.

[0018] Figure label: 1. Central mold core, 2. Radial split module, 3. Diversion channel, 4. Disc forging blank. Detailed Implementation

[0019] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be described in detail below. Obviously, the described embodiments are merely some embodiments of this invention, and not all embodiments. Based on the embodiments of this invention, all other implementation methods obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

[0020] The present invention will be further described below with reference to the accompanying drawings and embodiments.

[0021] like Figure 1 , Figure 2 , Figure 3 , Figure 4 , Figure 5As shown, this embodiment provides a multi-stage step-by-step deload forming method for Φ1600mm grade titanium alloy forgings. The forming method is implemented using a split mold, which includes an upper mold and a lower mold used in conjunction. The upper mold is an integral structure, and the upper mold can be equipped with a flat anvil mold or a forging final forging mold according to the forming step requirements. The cavity of the forging final forging mold fits with the upper surface of the forging blank. The lower mold includes a frustum-shaped central mold core 1 and radially split modules 2. The central mold core 1 is fixedly mounted on the lower mold base, and multiple radially split modules 2 are evenly distributed around the central mold core 1 in the circumference. The radially split modules 2 are oriented away from or towards the central mold core 1. The central mold core 1 is slidably disposed on the lower mold base. The inner surface of the radial split module 2 is an inclined surface that mates with the outer surface of the central mold core 1. When the inner surface of the radial split module 2 is in contact with the outer surface of the central mold core 1, the inner surface of the radial split module 2 is located at the top of the outer surface of the central mold core 1. The radial gap between adjacent radial split modules 2 forms a diversion channel 3. When the inner surface of the radial split module 2 is separated from the outer surface of the central mold core 1, the diversion channel 3 is opened. When the inner surface of the radial split module 2 is in contact with the outer surface of the central mold core 1, the diversion channel 3 is closed. The forming method includes the following steps: S1. Free forging and upsetting of rough billet: Assemble the upper die into a flat anvil die, control the radial split module 2 to slide towards the central die core 1, so that the inner side of the radial split module 2 fits against the outer side of the central die core 1, and the flow channel 3 of the lower die is closed; After heating the titanium alloy billet, place it in the center of the cavity of the lower die, control the flat anvil die to press down axially, and perform free forging and upsetting of the titanium alloy billet to form an upsetting billet, and the lower end of the titanium alloy billet forms a positioning contour with the cavity of the lower die; S2. Pre-forging diversion and load reduction filling: Replace the upper die with the final forging die, control the radial split module 2 to slide away from the central die core 1, so that the inner side of the radial split module 2 separates from the outer side of the central die core 1, the diversion channel 3 of the lower die opens, and the cavity diameter of the lower die increases; after reheating the upsetting billet, place it in the center of the cavity of the lower die, control the final forging die to press down axially, and pre-forge the upsetting billet into a disc pre-forging part. The process residue in the spoke area of ​​the disc pre-forging part is discharged outward along the opened diversion channel 3 until the rim cavity of the lower die is filled; the upper inner edge surfaces of all radial split modules 2 together constitute the rim forming surface of the disc forging part; S3. Final forging and finishing: Control the radial split module 2 to slide towards the central die core 1, the inner side of the radial split module 2 is in contact with the outer side of the central die core 1, the flow channel 3 of the lower die is closed, and the cavity diameter of the lower die is restored to the design size of the disc forging blank 4; After reheating the disc pre-forging, place it in the center of the cavity of the lower die, control the final forging die to press down axially, and perform final forging of the disc pre-forging to form the disc forging blank 4. The disc pre-forging continues to fill the cavity of the lower die until the rim cavity of the lower die is completely filled. The process residue discharged through the flow channel 3 in step 2 is pressed back into the cavity of the lower die and fused with the disc pre-forging body. When the final forging die is pressed down to the design under-pressure amount, the final dimensional finishing of the disc forging blank 4 is completed.

[0022] Hydraulic cylinders can be installed on the outside of each radial split module 2. These cylinders are bolted to the lower mold base. The piston rod of the hydraulic cylinder drives the radial split module 2 to move. When the flow channel 3 of the lower mold is open, a limiting plate is inserted into the flow channel 3. Alternatively, a slide rail can be installed on the lower mold base, and the radial split module 2 slides on the slide rail. The radial displacement of the radial split module 2 is controlled by a drive mechanism that links the press stroke. The design underpressure is such that the final position of the upper mold pressing down does not reach the theoretical fully closed position of the mold cavity, leaving a specific micro-gap.

[0023] Based on the above-mentioned multi-stage step-by-step deload forming method for Φ1600mm grade titanium alloy forgings, the present invention provides a multi-stage step-by-step deload forming method for Φ1600mm grade titanium alloy forgings, which is implemented using a split mold. The upper mold of the split mold can be equipped with a flat anvil mold or a forging final forging mold. The lower mold of the split mold consists of a central mold core 1 and multiple radially arranged split modules 2. The inner surface of the radial split modules 2 and the outer surface of the central mold core 1 are fitted with inclined surfaces. The downward axial pressure applied by the upper mold is decomposed by the inclined surfaces to generate a radial component force toward the central mold core 1. Each radial split module 2 is pressed against the peripheral wall of the central mold core 1. The greater the axial load, the stronger the locking force. Therefore, no additional locking device is needed. The radial split modules 2 can achieve self-locking by pressing them against the central mold core 1. The radial gaps between adjacent radial split modules 2 form a diversion channel 3. The radial split modules 2 move radially away from the central mold core 1 and disperse, opening the diversion channel 3. The radial split modules 2 move radially towards the central mold core 1 and close, closing the diversion channel 3. This realizes the control of opening or closing the diversion channel 3. This forming method divides the entire forging process of the disc forging into three stages of loading forging: free forging upsetting rough billet, pre-forging diversion and load reduction filling, and final forging finishing. In each forging stage, the process waste material in the spoke area of ​​the disc pre-forging is guided to be discharged in an orderly manner from the diversion channel by controlling the real-time closing or opening of the diversion channel 3 of the lower die during the pre-forging process, thus avoiding the continuous accumulation of metal in the cavity and the sudden increase in load. This forming method makes the forming force of each forging stage significantly lower than that of a single overall final forging, and the peak load is effectively distributed, thereby achieving the overall die forging of Φ1600mm titanium alloy forgings within the capacity range of an 800MN press.Using the multi-stage step-by-step load reduction forming method for Φ1600mm titanium alloy forgings of this invention, the step-by-step load reduction decomposes a load exceeding 1000MN into multiple stage loads not exceeding 800MN, with a maximum load reduction of over 45%, significantly reducing the forming load. Φ1600mm titanium alloy disc forging can be completed on an 800MN press. Utilizing the radial component of the axial pressing pressure of the upper die during forging, each radially segmented module 2 is pressed tightly against the peripheral wall of the central die core 1. The radially segmented modules 2 and the central die core 1 achieve self-locking. The greater the forging pressing pressure, the stronger the locking force, preventing the radially segmented modules 2 from separating and generating flash burrs during final forging. The force-bearing area of ​​the die in each forming step is precisely matched with the projected area of ​​the corresponding forging blank, and the self-locking force increases with the forging pressure. The forging pressure is adaptive, achieving a synergistic adaptive effect; the wedge angle of the mating inclined surface between the radial split module 2 and the central die core 1 is less than the friction self-locking angle, ensuring self-locking stability; the flow of the billet from the center to the rim is controlled by the spacing of the radial split modules 2, suppressing folding and incomplete filling, and precisely controlling the metal flow; each radial split module 2 can be replaced independently, and local wear only requires replacement of the corresponding worn parts, reducing die maintenance costs by more than 60%, thus reducing die costs and maintenance difficulty; multiple forgings with small deformation are beneficial to the dynamic recrystallization and grain refinement of titanium alloys, improving the uniformity of the structure and the microstructure properties of forgings; it is suitable for titanium alloys such as TC4, TC17, and TA15, and can also be extended to large disc parts of difficult-to-deform materials such as high-temperature alloys and ultra-high-strength steels, demonstrating strong adaptability.

[0024] As one possible implementation method, such as Figure 2 As shown, the angle between the axis of the frustum-shaped central mold core 1 and the generatrix is ​​α, where 5°≤α≤20°.

[0025] The angle between the axis of the central die core 1 and the generatrix is ​​determined according to the load-bearing requirements of the lower die and the tonnage of the forging. For example, if the angle α between the axis of the central die core 1 and the generatrix is ​​5°, 10°, 15° or 20°, it ensures that there is sufficient radial force on the central die core 1, avoids the separation of the radial split module 2 from the central die core 1 during the axial pressing of the final forging die, ensures that the flow channel 3 of the lower die is closed, thereby avoiding the generation of flash and burrs, and at the same time avoiding excessive radial force, excessive compression of the central die core 1, and damage.

[0026] As one possible implementation method, such as Figure 2 As shown, the angle between the axis of the central mold core 1 and the generatrix is ​​10°≤α≤15°.

[0027] If the angle α between the axis of the central mold core 1 and the generatrix is ​​10°, 11°, 12°, 13°, 14°, or 15°, it has a good self-locking effect and protects the central mold core 1.

[0028] As one possible implementation method, such as Figure 2 , Figure 3 , Figure 4 As shown, the number of radial split modules 2 is 4 to 6.

[0029] The number of radial split modules 2 can be determined as 4, 5 or 6 depending on the actual size, geometric characteristics and load requirements of the forging. If the forging size is small and the shape is simple, 4 radial split modules 2 are selected. If the forging size is large and the shape is complex, 6 radial split modules 2 are selected. As the number of radial split modules 2 increases, the number of diversion channels 3 increases.

[0030] As one possible implementation, the height-to-diameter ratio of the titanium alloy billet is 0.8 to 1.2.

[0031] Titanium alloy billets can be made from bar stock. According to the principle of deformation distribution of titanium alloy billets, if the height-to-diameter ratio is too large, the billet is prone to bending and instability during free forging and upsetting, and the billet may fold or tilt. If the height-to-diameter ratio is too small, the radial resistance during free forging and upsetting is large, the deformation resistance is large, the forming load is increased, and the deformation is uneven. The height-to-diameter ratio of titanium alloy billets is 0.8 to 1.2. If the height-to-diameter ratio is 0.8 to 0.9, or 1.0, or 1.1 or 1.2, the titanium alloy billet can be freely forged evenly and stably upsetting, avoiding forming defects.

[0032] As one possible implementation, the titanium alloy billet is TC4, TC17, or TA15.

[0033] The forming method is suitable for forming TC4, TC17, or TA15 disc forgings. It can also be used for high-temperature alloys with a heat recovery temperature of 900°-1000° or ultra-high-strength steel with a heat recovery temperature of 850°-1150°.

[0034] As one possible implementation method, such as Figure 1 As shown, the free forging upsetting heating temperature of the titanium alloy billet, the pre-forging heating temperature of the upsetting billet, and the final forging heating temperature of the disc pre-forging are all T. β -40℃, where T β This is the β phase transformation point of the titanium alloy.

[0035] Titanium alloy billets, upsetting billets, and disc forgings are heated to T. β -40℃ reduces the deformation resistance of titanium alloy billets, upsetting billets, and disc forgings, improving the load reduction effect. This ensures that the titanium alloy can flow smoothly along the diversion channel 3 and fill the cavity, while avoiding premature filling of the cavity and a sharp increase in load due to excessive fluidity. Forging in the α-phase and β-phase two-phase regions avoids excessive grain coarsening in the forgings, improves the fracture toughness and fatigue strength of the forgings, and the forged disc forging blank 4 meets the stringent requirements of aerospace load-bearing components.

[0036] Implementation Case: For the forming of TC4 titanium alloy fan discs, the projected diameter of the fan disc is 1650mm, the maximum thickness is 120mm, and the minimum thickness is 65mm.

[0037] According to the principle of deformation distribution, the Φ500mm×1086mm bar stock is upheaded into a Φ646mm×650mm billet with a height-to-diameter ratio of approximately 1.0.

[0038] Step 1: The first step is to assemble the upper mold into a flat anvil mold, and then place the billet into the heating furnace and heat it to T. β At -40℃, the flow channel 3 of the lower mold is closed, the billet is placed in the center of the cavity of the lower mold, and the flat anvil presses down at a speed of 2-5 mm / s. The billet is freely upset into an upset billet with an axial pressure load of about 160 MN and the load is stable.

[0039] Step Two: In the second step, replace the upper die with the final forging die, and place the upsetting billet into the heating furnace and heat it to T. β At -40℃, the flow channel 3 of the lower die is opened, the cavity diameter of the lower die increases, the upsetting billet is placed in the center of the cavity of the lower die, the final forging die is pressed down, the upsetting billet is die-forged into a disc pre-forging part, the process residue in the spoke area of ​​the disc pre-forging part is discharged downward along the opened flow channel 3 until the rim cavity of the lower die is filled, the process residue discharged into the flow channel 3 forms branches, and the peak load is about 685MN.

[0040] Step 3: The third step involves placing the pre-forged disc into a heating furnace and heating it to T. β At -40℃, the flow channel 3 of the lower die is closed, the cavity diameter of the lower die is restored, the disc pre-forging is placed in the center of the cavity of the lower die, the branches abut against the top surface of the lower die, the final forging die is pressed down, the disc pre-forging is die-forged into a disc forging blank 4 until the flash appears, the process residue (branches) discharged through the flow channel 3 is pressed back into the cavity of the lower die and fused with the disc pre-forging body, the peak load is about 685MN.

[0041] The peak forming load in this implementation case was 685MN, which is 45% lower than that of traditional one-time final forging.

[0042] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.

Claims

1. A multi-stage, step-by-step load reduction forming method for Φ1600mm grade titanium alloy forgings, characterized in that, The forming method is achieved using a split mold, which includes an upper mold and a lower mold used in conjunction. The upper mold is an integral structure, and the upper mold can be equipped with a flat anvil mold or a forging final forging mold according to the forming step requirements. The cavity of the forging final forging mold fits with the upper surface of the forging blank. The lower mold includes a frustum-shaped central mold core (1) and radial split modules (2). The central mold core (1) is fixedly set on the lower mold base, and multiple radial split modules (2) are evenly distributed around the central mold core (1) in the circumference. The radial split modules (2) are slidably set on the lower mold base in the direction away from or close to the central mold core (1). The inner surface of the radial split module (2) is an inclined surface that mates with the outer surface of the central mold core (1). When the inner surface of the radial split module (2) is in contact with the outer surface of the central mold core (1), the inner surface of the radial split module (2) is located at the top of the outer surface of the central mold core (1). The radial gap between adjacent radial split modules (2) forms a diversion channel (3). When the inner surface of the radial split module (2) is separated from the outer surface of the central mold core (1), the diversion channel (3) is opened. When the inner surface of the radial split module (2) is in contact with the outer surface of the central mold core (1), the diversion channel (3) is closed. The forming method includes the following steps: S1. Free forging and upsetting of rough billet: The upper die is assembled into a flat anvil die, and the radial split module (2) is controlled to slide towards the central die core (1) so that the inner side of the radial split module (2) is in contact with the outer side of the central die core (1), and the flow channel (3) of the lower die is closed; the titanium alloy billet is heated and placed in the center of the cavity of the lower die, and the flat anvil die is controlled to press down axially to perform free forging and upsetting of the titanium alloy billet to form an upsetting billet, and the lower end of the titanium alloy billet forms a positioning contour with the cavity of the lower die; S2. Pre-forging diversion and load reduction filling: Replace the upper die with the final forging die, control the radial split module (2) to slide away from the central die core (1), so that the inner side of the radial split module (2) is separated from the outer side of the central die core (1), the diversion channel (3) of the lower die is opened, and the cavity diameter of the lower die is increased; after the upsetting billet is reheated, it is placed in the cavity center of the lower die, and the final forging die is axially pressed down to pre-forge the upsetting billet into a disc pre-forging part. The process residue in the spoke area of ​​the disc pre-forging part is discharged outward along the opened diversion channel (3) until the rim cavity of the lower die is filled; S3. Final forging and finishing: Control the radial split module (2) to slide towards the direction close to the central mold core (1), the inner side of the radial split module (2) is in contact with the outer side of the central mold core (1), the flow channel (3) of the lower mold is closed, and the cavity diameter of the lower mold is restored to the design size of the disc forging blank (4); After the disc pre-forging is reheated, it is placed in the center of the cavity of the lower mold, and the final forging mold is axially pressed down to perform final forging of the disc pre-forging into a disc forging blank (4). The disc pre-forging continues to fill the cavity of the lower mold until the rim cavity of the lower mold is completely filled. The process residue discharged through the flow channel (3) is pressed back into the cavity of the lower mold and fused with the disc pre-forging body. When the final forging mold is pressed down to the design under-pressure amount, the final dimensional finishing of the disc forging blank (4) is completed.

2. The multi-stage step-by-step de-loading forming method for Φ1600mm grade titanium alloy forgings according to claim 1, characterized in that, The angle between the axis of the frustum-shaped central mold core (1) and the generatrix is ​​α, where 5°≤α≤20°.

3. The multi-stage step-by-step de-loading forming method for Φ1600mm grade titanium alloy forgings according to claim 2, characterized in that, The angle between the axis of the central mold core (1) and the generatrix is ​​10°≤α≤15°.

4. The multi-stage step-by-step de-loading forming method for Φ1600mm grade titanium alloy forgings according to claim 1, characterized in that, The number of radial split modules (2) is 4 to 6.

5. The multi-stage step-by-step de-loading forming method for Φ1600mm grade titanium alloy forgings according to claim 1, characterized in that, The aspect ratio of the titanium alloy billet is 0.8 to 1.

2.

6. The multi-stage step-by-step de-loading forming method for Φ1600mm grade titanium alloy forgings according to claim 1, characterized in that, The titanium alloy billet is TC4, TC17, or TA15.

7. The multi-stage step-by-step de-loading forming method for Φ1600mm grade titanium alloy forgings according to claim 1, characterized in that, The free forging upsetting heating temperature of the titanium alloy billet, the pre-forging heating temperature of the upsetting billet, and the final forging heating temperature of the disc pre-forging are all T. β -40℃, where T β This is the β phase transformation point of the titanium alloy.