A wear-resistant hob cutter ring, its preparation method and application

By employing a composite process of annular and spherical reinforcing blanks in the cutter ring of a tunnel boring machine, combined with micron and nano titanium carbide particles, a wear-resistant skeleton is constructed, solving the problem of insufficient wear resistance and toughness of the cutter ring, and achieving the effects of extending cutter life and reducing cost.

CN123102972APending Publication Date: 2026-11-17GUANGDONG INST OF NEW MATERIALS +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611323818.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing cutterhead materials for tunnel boring machines cannot simultaneously achieve both wear resistance and toughness, resulting in short service life, high replacement frequency, and seriously affecting tunneling efficiency and maintenance costs.

Method used

A composite process of pre-formed billet and casting-infiltration is adopted. A honeycomb structure is constructed by splicing ring-reinforced billets and combining spherical reinforced billets. Combined with micron and nano titanium carbide particles, a wear-resistant skeleton is formed, which enhances the toughness and wear resistance of the material.

Benefits of technology

It extends the service life of the cutter ring, reduces the replacement frequency, improves tunneling efficiency, and reduces operation and maintenance costs. It has a simple manufacturing process and cost advantages, making it suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102972A_ABST
    Figure CN123102972A_ABST
Patent Text Reader

Abstract

This invention relates to a wear-resistant hobbing cutter ring, its preparation method, and its application, belonging to the field of tunnel boring machine manufacturing technology. The preparation method of the wear-resistant hobbing cutter ring provided by this invention includes pre-forming a blank and casting / infiltration molding. The wear-resistant hobbing cutter ring provided by this invention includes an annular reinforcing blank, a spherical reinforcing blank, and a matrix. The annular reinforcing blank is obtained by pressing and sintering TiC particles with a particle size of 1-10 μm. Multiple hexagonal through holes are formed on the annular reinforcing blank, and spherical reinforcing blanks made of carbon powder, titanium powder, and alloy powder are placed inside the through holes. The wear-resistant hobbing cutter ring provided by this invention has the characteristics of excellent wear resistance, simple manufacturing process, and controllable cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of tunnel boring machine manufacturing technology, and in particular to a wear-resistant cutterhead ring, its manufacturing method, and its application. Background Technology

[0002] Tunnel boring machines (TBMs) are core equipment for tunnel excavation in the transportation construction sector. Their highly mechanized and automated construction characteristics effectively improve tunneling efficiency. Currently, the cutterhead materials for TBM cutters both domestically and internationally commonly use Cr8Mo2VSi and Cr... 12 Conventional steel materials such as Mo1V1 are used. However, due to the limitations of conventional steel materials, current tunnel boring machine (TBM) cutterheads inherently suffer from a shortcoming: they cannot simultaneously achieve both wear resistance and toughness. During the tunneling and rock-breaking process, the cutterheads are subjected to high static pressure, dynamic impact loads, and continuous shear friction, making them prone to wear, chipping, and fatigue damage. This results in short cutterhead lifespan, frequent replacements, severely restricting tunneling efficiency and significantly increasing maintenance costs.

[0003] The surface hardness, overall toughness, and wear resistance of the cutterhead ring directly determine the service life and tunneling stability of the cutterhead. Therefore, developing a cutterhead ring for tunnel boring machines with excellent wear resistance, simple manufacturing process, and controllable cost, as well as its manufacturing process, is of great significance for improving tunneling efficiency and reducing engineering costs. Summary of the Invention

[0004] The purpose of this invention is to overcome the shortcomings of the prior art and provide a wear-resistant hobbing cutter ring, its preparation method, and its application.

[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows: In a first aspect, the present invention provides a method for preparing a wear-resistant hobbing cutter ring, specifically comprising the following steps: S1. Provide an annular reinforcing blank with the same diameter as the blade edge of the blade ring, wherein the annular reinforcing blank has a plurality of hexagonal through holes; S2. Titanium powder (Ti), carbon powder (C) and alloy steel powder are mixed evenly and then pressed into spherical reinforced blanks; S3. Place the annular reinforcing blank in the sand mold cavity, place the spherical reinforcing blank in the hexagonal through hole, and after casting, cooling, and sand removal, obtain the wear-resistant hobbing cutter ring.

[0006] Preferably, the annular reinforcing blank is formed by splicing together multiple arc-shaped reinforcing blanks in the circumferential direction, and each arc-shaped reinforcing blank has a hexagonal through hole.

[0007] Preferably, the hexagonal through holes are arranged in an array on the annular reinforced blank.

[0008] Preferably, the arc-shaped reinforced preform is obtained by mixing titanium carbide (TiC) powder with a binder, followed by pressing and sintering.

[0009] The technical solution of this invention constructs a wear-resistant cutter ring through a composite process of pre-formed blank and casting-infiltration molding. The annular reinforcing blank is formed by splicing multiple arc-shaped reinforcing blanks, which not only reduces the forming difficulty of the annular reinforcing blank, but also allows the gaps between the arc-shaped reinforcing blanks to release thermal stress, prevent crack propagation, and extend the service life of the annular reinforcing blank as a wear-resistant skeleton. The array of dispersed through-hole structures on the annular reinforcing blank forms a honeycomb structure, uniformly distributing the tunneling load, absorbing impact energy, and reducing stress concentration. Spherical reinforcing blanks are placed within the through-hole structure, further inhibiting crack propagation. Even after the through-hole structure and the spherical reinforcing blanks are assembled, gaps remain, preserving channels for the deep penetration of the molten metal, allowing the reinforcing blank and the alloy steel matrix to have a "pinning" effect, preventing peeling off of the composite zone.

[0010] Preferably, in step S1, the cross-section of the hexagonal through hole is a regular hexagon.

[0011] Preferably, the side length of the regular hexagon is 5-15 mm; more preferably, the side length of the regular hexagon is 8-12 mm.

[0012] Preferably, in step S2, the radius of the spherical reinforced blank is equal to the side length of the regular hexagon.

[0013] In the technical solution of this invention, the dimensions of the spherical reinforcing blank must be compatible with the dimensions of the regular hexagonal channel of the arc-shaped reinforcing blank. When the dimensions are too small, the spherical reinforcing blank is prone to displacement inside the regular hexagonal channel, making effective fixation difficult; when the dimensions are too large, the spherical reinforcing blank cannot be assembled into the regular hexagonal channel, causing assembly difficulties. By designing a compatibility between the two dimensions, it is possible to ensure that the spherical reinforcing blank is stably housed within the hexagonal channel, preventing displacement and detachment of the spherical reinforcing blank during casting and ensuring the integrity of the composite reinforcement structure.

[0014] Preferably, in step S1, the thickness of the annular reinforced blank is 15-30 mm.

[0015] Preferably, the distance between the outer surface of the annular reinforced blank on the side away from the center and the impact surface of the hobbing cutter ring is 3-5 mm.

[0016] Preferably, the particle size Dv50 of the titanium carbide powder is 1-10 μm.

[0017] Preferably, in step S2, the particle size Dv50 of the titanium powder is 10-20 μm, the particle size Dv50 of the carbon powder is 5-10 μm, and the particle size Dv50 of the alloy steel powder is 20-50 μm.

[0018] Preferably, in step S2, the weight ratio of carbon powder, titanium powder and alloy steel powder is 68-72:17-18:10-15; more preferably, the total weight of carbon powder and titanium powder is 85-90 parts, and the total weight of alloy steel powder is 10-15 parts.

[0019] Preferably, the weight ratio of carbon powder to titanium powder is 4:1.

[0020] The inventors discovered that the micron-sized titanium carbide particles in the arc-shaped reinforced billet are used to construct the main load-bearing skeleton and improve wear resistance; the carbon powder and metal powder in the spherical reinforced billet will induce an in-situ reaction under high temperature melt, and titanium carbide particles with a particle size Dv50 of 200-800nm ​​will precipitate between the micron-sized titanium carbide skeleton, thus optimizing the interfacial compatibility between the micron-sized titanium carbide particles and the alloy steel matrix.

[0021] To achieve the aforementioned structural features and technical effects, the spherical reinforced blank in this invention is obtained by uniformly mixing titanium powder (Ti), carbon powder (C), and alloy steel powder and then pressing it; the arc-shaped reinforced blank is obtained by mixing titanium carbide (TiC) powder with a binder and then pressing and sintering it.

[0022] Preferably, the adhesive preparation includes inorganic adhesives or organic adhesives.

[0023] Preferably, the inorganic binder includes at least one of silicates, phosphates, and aluminates.

[0024] Preferably, the organic binder includes at least one of epoxy system, silicone system, and acrylic system.

[0025] Preferably, the TiC particles in the prepared arc-shaped reinforced blank are 85-90 parts by weight, and the binder is 10-15 parts by weight.

[0026] Preferably, the axial pressure of the arc-shaped reinforced blank is 30-50KN, and the holding time is 10-15s.

[0027] Preferably, the sintering temperature of the arc-shaped reinforced blank is 200-300℃, and the sintering time is 1-1.5h.

[0028] Preferably, the crush resistance of the arc-shaped reinforced blank is 25-30 MPa.

[0029] Preferably, in step S2, the axial pressure of the spherical reinforced blank is 10-20KN, and the holding time is 5-10s.

[0030] Preferably, in step S3, the distance between the outer surface of the annular reinforced blank on the side away from the center and the inner surface of the sand mold is 5-7 mm.

[0031] Preferably, in step S3, the casting temperature is 1450-1600℃.

[0032] Preferably, in step S3, the casting melt is an alloy steel melt.

[0033] Secondly, the present invention provides a wear-resistant hob ring prepared by the above-described method for preparing wear-resistant hob rings.

[0034] Preferably, the wear-resistant hobbing cutter ring includes a cutter ring root and a cutter ring cutting edge. The cutter ring cutting edge includes an annular reinforcing blank, a spherical reinforcing blank, and an alloy steel matrix. The cutter ring root includes an alloy steel matrix.

[0035] This invention employs a differentiated design, with the wear-resistant hobbing cutter ring consisting of a root and a cutting edge along the radial direction. A composite reinforcement structure is constructed for the severely worn cutting edge to improve its hardness and wear resistance, resist wear during tunneling, and extend the service life of the cutter ring. An alloy steel matrix is ​​used at the root of the cutter ring to retain the strength, toughness, machinability, and cost advantages of alloy steel.

[0036] Thirdly, the present invention provides the application of the above-mentioned wear-resistant roller cutter ring in a tunnel boring machine.

[0037] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. The technical solution of this invention constructs a wear-resistant cutter ring through a composite process of pre-formed blank and casting-infiltration molding. The annular reinforcing blank is formed by splicing multiple arc-shaped reinforcing blanks, which not only reduces the forming difficulty of the annular reinforcing blank, but also allows the gaps between the arc-shaped reinforcing blanks to release thermal stress, prevent crack propagation, and extend the service life of the annular reinforcing blank as a wear-resistant skeleton. The arrayed and dispersed through-hole structure on the annular reinforcing blank forms a honeycomb structure, uniformly distributing the tunneling load, absorbing impact energy, and reducing stress concentration. Spherical reinforcing blanks are placed within the through-hole structure, further inhibiting crack propagation. Even after the through-hole structure and the spherical reinforcing blanks are assembled, gaps remain, preserving channels for the deep penetration of the molten metal, allowing the reinforcing blank and the alloy steel matrix to achieve a "pinning" effect, preventing peeling off of the composite zone.

[0038] 2. The manufacturing process provided by this invention is simple, controllable, highly efficient, and cost-effective, making it suitable for mass production. Furthermore, this technology has broad applicability, allowing for customized design and manufacturing of cutterheads for tunnel boring machines in different operating environments, sizes, and models, demonstrating excellent industrial application prospects and promotional value.

[0039] 3. In the present invention, the wear-resistant hob cutter ring consists of a root and a cutting edge in the radial direction. A composite structure is constructed in the cutting edge to enhance the wear resistance of the cutting edge, improve the hob's ability to resist friction, cutting, extrusion and wear during hard rock excavation, extend its service life and reduce the replacement frequency. At the same time, the alloy steel matrix of the cutter ring root is retained to meet the wear resistance requirements while taking into account the structural toughness and production cost.

[0040] 4. The present invention uses a wear-resistant composite material developed by the inventors. By introducing micron-sized titanium carbide particles externally and generating nano-sized titanium carbide particles in situ, a multi-scale titanium carbide particle structure is constructed in the blade ring. Among them, the micron-sized titanium carbide particles form the load-bearing skeleton, and the nano-sized titanium carbide particles optimize the interface compatibility. Attached Figure Description

[0041] Figure 1 This is a partial structural schematic diagram of the wear-resistant hob ring of the present invention; In the figure: the cutting edge of the cutter ring includes a spherical reinforcing blank 3, an arc-shaped reinforcing blank 2 and an alloy steel matrix 1, and the root of the cutter ring includes an alloy steel matrix 1; Figure 2 This is a schematic diagram of the wear-resistant hobbing cutter ring prepared in Example 3; In the figure: the wear-resistant hob cutter ring includes the cutter ring root 4 and the cutter ring cutting edge 5.

[0042] Figure 3 The image shows the SEM morphology of the cutting edge of the wear-resistant hob prepared in Example 3. Detailed Implementation

[0043] To better illustrate the purpose, technical solution, and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0044] Unless otherwise specified, all other materials and reagents used in the examples are commercially available.

[0045] Example 1 S1. TiC particles with a particle size Dv50 of 2μm are pressed into shape under an axial pressure of 30KN and a holding time of 15s. The particles are then sintered at a temperature of 300℃ to obtain an arc-shaped reinforced blank with a thickness of 15mm. Multiple arc-shaped reinforced blanks are spliced ​​together circumferentially to form an annular reinforced blank with the same diameter as the blade edge. Multiple hexagonal through holes are opened on the annular reinforced blank, and the side length of the regular hexagon of the through hole cross-section is 5mm. The TiC particles are 85 parts by weight, and the binder is 15 parts by weight.

[0046] S2. Ti powder with a particle size Dv50 of 10μm, C powder with a particle size Dv50 of 5μm and alloy steel powder with a particle size Dv50 of 20μm are mixed evenly in proportion and then pressed into a spherical reinforced billet under an axial pressure of 10KN and a holding time of 10s. The total weight of Ti powder and C powder is 85 parts, and the weight of alloy steel powder is 15 parts. The weight ratio of Ti powder to C powder is 4:1.

[0047] S3. Place the annular reinforcing blank in the sand mold cavity, with the distance between the side of the annular reinforcing blank away from the center and the inner surface of the sand mold being 5mm. Place the spherical reinforcing blank in the hexagonal through hole. After casting, cooling, and sand removal at a casting temperature of 1500℃, the wear-resistant hobbing cutter ring is obtained.

[0048] Example 2 S1. TiC particles with a particle size Dv50 of 10μm are pressed into shape under an axial pressure of 40KN and a holding time of 12s. The particles are then sintered at a temperature of 250℃ to obtain an arc-shaped reinforced blank with a thickness of 30mm. Multiple arc-shaped reinforced blanks are spliced ​​together in the circumferential direction to form an annular reinforced blank with the same diameter as the blade edge. Multiple hexagonal through holes are opened on the annular reinforced blank, and the side length of the regular hexagon of the through hole cross-section is 15mm. The TiC particles are 88 parts by weight, and the binder is 12 parts by weight.

[0049] S2. Ti powder with a particle size Dv50 of 20μm, C powder with a particle size Dv50 of 10μm and alloy steel powder with a particle size Dv50 of 50μm are mixed evenly in proportion and then pressed into a spherical reinforced billet under an axial pressure of 15KN and a holding time of 8s. The total weight of Ti powder and C powder is 90 parts, and the weight of alloy steel powder is 10 parts. The weight ratio of Ti powder to C powder is 4:1.

[0050] S3. Place the annular reinforcing blank in the sand mold cavity, with the distance between the side of the annular reinforcing blank away from the center and the inner surface of the sand mold being 7mm. Place the spherical reinforcing blank in the hexagonal through hole. After casting, cooling, and sand removal at a casting temperature of 1500℃, the wear-resistant hobbing cutter ring is obtained.

[0051] Example 3 S1. TiC particles with a particle size Dv50 of 5μm are pressed into shape under an axial pressure of 50KN and a holding time of 10s. The mixture is then sintered at a temperature of 200℃ to obtain an arc-shaped reinforced blank with a thickness of 20mm. Multiple arc-shaped reinforced blanks are spliced ​​together circumferentially to form an annular reinforced blank with the same diameter as the blade edge. Multiple hexagonal through holes are opened on the annular reinforced blank, and the side length of the regular hexagon of the through hole cross-section is 10mm. The weight parts of TiC particles are 90 parts, and the weight parts of binder are 10 parts.

[0052] S2. Ti powder with a particle size Dv50 of 15μm, C powder with a particle size Dv50 of 8μm and alloy steel powder with a particle size Dv50 of 30μm are mixed evenly in proportion and then pressed into a spherical reinforced billet under an axial pressure of 20KN and a holding time of 5s. The total weight of Ti powder and C powder is 90 parts, and the weight of alloy steel powder is 10 parts. The weight ratio of Ti powder to C powder is 4:1.

[0053] S3. Place the annular reinforcing blank in the sand mold cavity, with the distance between the side of the annular reinforcing blank away from the center and the inner surface of the sand mold being 6mm. Place the spherical reinforcing blank in the hexagonal through hole. After casting, cooling, and sand removal at a casting temperature of 1600℃, the wear-resistant hobbing cutter ring is obtained.

[0054] Comparative Example 1 Compared with Example 3, except that no spherical reinforced preform was prepared, the other preparation methods, components and weight parts are completely the same.

[0055] Comparative Example 2 Compared with Example 3, except that the spherical reinforced blank was not prepared and the annular reinforced blank was not provided with hexagonal through holes, the other preparation methods, components and weight parts are completely the same.

[0056] Comparative Example 3 Compared with Example 3, except that the distance between the side of the annular reinforced blank away from the center and the inner surface of the sand mold is 0 mm, the other preparation methods, components and weight parts are completely the same.

[0057] Performance testing: The wear-resistant hobbing cutter rings prepared in the examples and comparative examples were tested.

[0058] (1) The test method for the volume fraction of titanium carbide particles refers to GB / T 18876.3-2008 "Standard test method for determination of metallographic structure, inclusion content and grade in steel and other metals by automatic image analysis - Part 3 Image analysis and stereoscopic determination of titanium carbide grade in steel". (2) The Rockwell hardness test method refers to GB / T 230.1-2018 "Metallic materials Rockwell hardness test - Part 1: Test method"; (3) The test method for impact toughness refers to GB / T 229-2020 "Charpy Pendulum Impact Test Method for Metallic Materials", and the notch type is unnotched; (4) The test method for wear resistance is in accordance with T / CFA 010604-3-2016 "Test Method for Impact Abrasive Wear of Steel Materials". The conventional H13 alloy steel matrix sample is used as the performance comparison benchmark to calculate the relative wear resistance ratio.

[0059] The test results of the above embodiments and comparative examples are shown in Table 1.

[0060] Table 1 As shown in Table 1, the comprehensive mechanical properties of the wear-resistant hobbing cutter rings prepared in Examples 1-3 are all superior to those in Comparative Examples 1-3. The total volume fraction of titanium carbide particles is 80-90%, the Rockwell hardness is 60-65 HRC, the impact toughness is 33-35 J, and the relative wear resistance is 3-4 times that of the H13 matrix. Among them, Example 3 is a preferred embodiment of the present invention; thus, it is confirmed that the wear-resistant hobbing cutter rings prepared using the raw material particle size, ratio, and process parameters defined in the present invention can have both hardness and wear resistance; the wear-resistant composite material prepared within the preferred parameter range can further improve its hardness and wear resistance.

[0061] Comparative Example 1 did not prepare a spherical reinforced blank, which weakened the ability to suppress cracks. In addition, there were only single-scale titanium carbide particles inside the cutter ring, and the volume fraction of titanium carbide particles was reduced. Therefore, the hardness and relative wear resistance of the cutter ring decreased significantly.

[0062] In Comparative Example 2, no hexagonal through-holes were provided, meaning the annular reinforced blank was a solid and dense structure. In the absence of a spherical reinforced blank as a precursor, the solid structure could not effectively absorb impact energy, resulting in significant local stress concentration. At the same time, the dense structure of the solid blank and the insufficient melt infiltration channels led to a large number of defects such as pores, shrinkage porosity, and shrinkage cavities at the cutting edge of the cutter ring, further deteriorating the overall mechanical properties of the cutter ring, with the most significant decrease in impact toughness.

[0063] In Comparative Example 3, the distance between the side of the annular reinforced billet away from the center and the inner surface of the sand mold is 0 mm. The insufficient gap makes it difficult for the high-temperature alloy steel melt to spread and penetrate fully, resulting in a large number of defects such as pores, shrinkage porosity, and shrinkage cavities in the cutting edge area. This leads to poor bonding quality between TiC particles and the alloy steel matrix and low interfacial bonding strength, causing the annular reinforced billet to easily fall off as a whole under load and impact.

[0064] Figure 3 This is a SEM image of the cutting edge of the wear-resistant hob ring prepared in Example 3. Figure 3 A continuous matrix phase is visible, in which two types of reinforcing particles are uniformly distributed: one type consists of micron-sized TiC particles introduced through physical mixing, which provide skeletal support; the other type consists of in-situ generated nano-sized TiC particles that are dispersedly distributed. The particles show no significant agglomeration and are tightly embedded within the matrix, exhibiting good interfacial bonding without cracks or pores. The micron-sized particles construct the structural framework, while the uniformly dispersed nano-sized particles provide reinforcement; the two work synergistically to exert complementary effects in scale and distribution, significantly improving the overall performance of the material.

[0065] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.

Claims

1. A method for preparing a wear-resistant hobbing cutter ring, characterized in that, Includes the following steps: S1. Provide an annular reinforcing blank with the same diameter as the blade edge of the blade ring, wherein the annular reinforcing blank has a plurality of hexagonal through holes; S2. Press titanium powder, carbon powder and alloy steel powder into spherical reinforced blanks; S3. Place the annular reinforcing blank in the sand mold cavity, place the spherical reinforcing blank in the hexagonal through hole, and after casting, cooling, and sand removal, obtain the wear-resistant hobbing cutter ring.

2. The method for preparing the wear-resistant hobbing cutter ring as described in claim 1, characterized in that, The annular reinforced blank is formed by splicing together multiple arc-shaped reinforced blanks along the circumference, and each arc-shaped reinforced blank has a hexagonal through hole.

3. The method for preparing the wear-resistant hob ring as described in claim 1, characterized in that, The hexagonal through holes are arranged in an array on the annular reinforced blank.

4. The method for preparing the wear-resistant hobbing cutter ring as described in claim 2, characterized in that, The arc-shaped reinforced preform is obtained by mixing titanium carbide powder with a binder, followed by pressing and sintering. The particle size Dv50 of the titanium carbide powder is 1-10 μm.

5. The method for preparing the wear-resistant hob ring as described in claim 1, characterized in that, In step S2, the particle size Dv50 of the titanium powder is 10-20 μm, the particle size Dv50 of the carbon powder is 5-10 μm, and the particle size Dv50 of the alloy steel powder is 20-50 μm.

6. The method for preparing the wear-resistant hob ring as described in claim 1, characterized in that, In step S1, the cross-section of the hexagonal through hole is a regular hexagon, and the side length of the regular hexagon is 5-15mm; In step S2, the radius of the spherical reinforced blank is equal to the side length of the regular hexagon.

7. The method for preparing the wear-resistant hob ring as described in claim 1, characterized in that, In step S1, the thickness of the annular reinforced blank is 15-30 mm.

8. The method for preparing the wear-resistant hobbing cutter ring as described in claim 1, characterized in that, In step S2, the weight ratio of carbon powder, titanium powder and alloy steel powder is 68-72:17-18:10-15.

9. A wear-resistant hob ring prepared by the method described in any one of claims 1-8.

10. The application of the wear-resistant cutterhead ring as described in claim 9 in a tunnel boring machine.