A Low-Temperature Casting and Strontium Modification Synergistic Process for Controlling Primary Silicon Size in Aluminum Ingots

By combining low-temperature casting with strontium modification, the primary silicon phase was refined and evenly distributed, solving the problem of coarse primary silicon in aluminum ingot production, improving the mechanical and processing properties of aluminum ingots, and making them suitable for industrial applications.

CN123102977APending Publication Date: 2026-11-17LONGDA ALUMINUM (WUHAN) CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611145491.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing aluminum ingot production processes, the primary silicon phase tends to be coarse, leading to reduced plasticity and toughness of the aluminum ingot. Furthermore, existing single processes cannot achieve stable and efficient control of the primary silicon size, which limits the application of aluminum-silicon alloys in high-end structural components.

Method used

By employing a synergistic process of low-temperature casting and strontium modification, the growth of the primary silicon phase is suppressed by low-temperature casting, while strontium modification is used to regulate the nucleation and growth direction of the silicon phase, thereby achieving a comprehensive control effect of multiple nucleations, slow growth, and fine morphology.

Benefits of technology

Aluminum ingots with small and uniformly distributed primary silicon were obtained, which significantly improved the mechanical and processing properties of the aluminum ingots, reduced cracking and delamination defects, and made them suitable for industrial mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102977A_ABST
    Figure CN123102977A_ABST
Patent Text Reader

Abstract

This invention discloses a low-temperature casting and strontium modification synergistic process for controlling the size of primary silicon in aluminum ingots, belonging to the field of aluminum ingot production technology. Through the synergistic effect of strontium modification and low-temperature casting, the nucleation and growth process of primary silicon in the aluminum-silicon alloy melt is regulated, achieving refinement of the size and rounding of the primary silicon morphology in the aluminum ingot. The advantages of low-temperature casting in this invention are: reducing the superheat of the melt casting (10-40℃ lower than conventional casting temperature), which shortens the residence time of the melt at high temperatures, reducing the diffusion distance and rate of silicon atoms, thus inhibiting the growth and coarsening of the primary silicon phase from the root; and creating better nucleation conditions at the lower casting temperature, promoting the generation of a large number of primary silicon nuclei in the melt, increasing the number of nuclei, and thus achieving "multi-nucleation," laying the foundation for subsequent refinement of primary silicon. Simultaneously, low-temperature casting reduces the temperature difference between the melt and the mold, reducing internal stress in the casting and decreasing the generation of defects such as cracks.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of aluminum ingot production technology, and particularly relates to a low-temperature casting and strontium modification synergistic process for controlling the initial silicon size of aluminum ingots. Background Technology

[0002] Aluminum-silicon alloys are among the most widely used cast aluminum alloys in the industrial field due to their low density, excellent casting performance, outstanding wear resistance, and moderate cost. The primary silicon phase, as the key second phase in aluminum-silicon alloys, directly determines the subsequent processing performance of the aluminum ingot (such as rolling, extrusion, and forging) and the mechanical properties of the final product (such as strength, plasticity, and toughness) through its size, morphology, and distribution. In conventional casting processes, due to high melt superheat and insufficient nucleation conditions, the primary silicon phase tends to preferentially grow, forming coarse blocky, lamellar, or needle-like structures. These coarse silicon phases easily cause stress concentration within the alloy, significantly reducing its plasticity and toughness, and may also lead to defects such as cracking and delamination during subsequent processing, severely limiting the application of aluminum-silicon alloys in high-end structural components.

[0003] Currently, traditional methods for refining primary silicon in aluminum ingots in the industry mainly include phosphorus modification, strontium modification, rapid solidification, electromagnetic stirring, and the addition of refining agents. However, each of these single processes has significant limitations and makes it difficult to achieve stable and efficient control of the size of primary silicon. Phosphorus modification process: It has a certain refining effect on primary silicon, but its improvement effect on eutectic silicon is limited. Moreover, phosphorus is prone to antagonistic reaction with the subsequently added strontium to form refractory compounds, which affects the modification effect. At the same time, the amount of phosphorus added is not easy to control, and excessive amount can easily lead to increased alloy brittleness. Conventional casting process: The casting temperature is generally too high (720~750℃), the melt is overheated, the silicon atom diffusion rate is fast, and the primary silicon phase tends to grow and coarsen quickly after nucleation, making it difficult to obtain a fine and uniform structure. Strontium modification process alone: ​​The main function of strontium is to refine eutectic silicon. Its effect on refining primary silicon is weak. When used alone, it cannot effectively solve the problem of coarse primary silicon and is prone to uneven modification and rapid degradation. Rapid solidification and electromagnetic stirring process: high equipment investment cost, complex operation, difficult to adapt to industrial mass production, and limited effect on refining primary silicon in high silicon aluminum alloys.

[0004] Therefore, developing a casting process that is simple, cost-controllable, adaptable to industrial production, and capable of achieving dual regulation of primary silicon nucleation and growth through synergistic effects to stably obtain a fine and uniform microstructure, overcoming the limitations of existing single processes, and improving the quality of aluminum ingots and subsequent processing performance, has significant engineering application value and market prospects. Summary of the Invention

[0005] This invention aims to overcome the shortcomings of existing technologies and provide a low-temperature casting and strontium modification synergistic process for controlling the size of primary silicon in aluminum ingots. The core idea is to suppress the growth of the primary silicon phase through low-temperature casting, and to regulate the nucleation and growth direction of the silicon phase through strontium modification. The two work together to achieve a comprehensive control effect of "multiple nucleation, slow growth, and fine morphology", ultimately obtaining aluminum ingots with small primary silicon size, uniform distribution, and excellent mechanical properties.

[0006] The present invention adopts the following technical solution: a low-temperature casting and strontium modification synergistic process for controlling the size of primary silicon in aluminum ingots. Through the synergistic effect of strontium modification and low-temperature casting, the nucleation and growth process of primary silicon in aluminum-silicon alloy melt is regulated, thereby achieving the refinement of the size and the rounding of the morphology of primary silicon in aluminum ingots. In the synergistic effect, low-temperature casting is used to inhibit the growth of primary silicon phase and promote the generation of a large number of primary silicon crystal nuclei, while strontium modification is used to adsorb onto the primary silicon growth interface, change its growth direction, and inhibit its preferential growth.

[0007] Furthermore, the process also includes raw material pretreatment, smelting, refining and degassing, and solidification and cooling steps, with each step being sequentially connected to ensure synergistic effects.

[0008] Furthermore, the melting temperature is 720–760°C, and after the raw materials are completely melted, the mixture is stirred evenly and the oxide slag is removed.

[0009] Furthermore, the refining and degassing process employs argon or nitrogen gas at a flow rate of 0.5–1.0 m³ / s. 3 / h, refining time 10-15 min, let stand and skim off the residue again.

[0010] Furthermore, the strontium modification treatment is carried out at 710–730°C, using an Al-10Sr master alloy, with a strontium addition amount of 0.02–0.06 wt%.

[0011] Furthermore, after the strontium is added, the mixture is stirred for 3-5 minutes and kept at a temperature for 10-20 minutes to complete the deterioration. During the deterioration process, an inert gas is used for protection to prevent the strontium from burning out.

[0012] Furthermore, the low-temperature casting temperature is 660–710℃, the casting speed is 0.5–1.0 m / s, and a stable low-flow-rate filling method is adopted.

[0013] Furthermore, the mold is preheated to 110-130°C before casting, with the lower temperature range for metal molds and the higher temperature range for sand molds.

[0014] Furthermore, after casting, the aluminum ingot solidifies naturally in the mold. After solidification, it is cooled to room temperature at a controlled temperature of 5-10℃ / h.

[0015] Furthermore, the primary silicon in the aluminum ingots prepared by this process has an average size of ≤20 μm and is uniformly distributed in granular or short rod shapes; the aluminum-silicon alloy includes conventional aluminum-silicon alloys and high-silicon aluminum alloys, specifically one or more of A356, ADC12, and Al-20Si.

[0016] I. The advantages of low-temperature casting in this invention: It reduces the superheat of the melt during casting (by 10-40°C compared to conventional casting temperatures). On one hand, this shortens the residence time of the melt at high temperatures, reducing the diffusion distance and rate of silicon atoms, thus inhibiting the growth and coarsening of the primary silicon phase at its source. On the other hand, the lower casting temperature creates better nucleation conditions, promoting the formation of a large number of primary silicon nuclei in the melt, increasing the number of nuclei, and thus achieving "multi-nucleation," laying the foundation for subsequent refinement of the primary silicon. Simultaneously, low-temperature casting reduces the temperature difference between the melt and the mold, lowering the internal stress of the casting and reducing the occurrence of defects such as cracks.

[0017] II. The synergistic effect of strontium modification in this invention: Strontium, as a highly efficient eutectic silicon modifier, works synergistically with low-temperature casting in this process to not only refine the eutectic silicon but also assist in refining the primary silicon. Its mechanism of action is as follows: Strontium atoms preferentially adsorb onto the growth interface of the primary silicon phase in the melt, occupying preferred growth positions and altering the growth direction of the silicon phase. This inhibits rapid growth of the silicon phase along a specific direction, transforming the primary silicon phase from its original coarse, blocky, or lamellar form into fine, granular, or short rod-like shapes. Simultaneously, strontium reduces the surface tension of the melt, promoting the dispersion of primary silicon nuclei and preventing their aggregation and growth, further enhancing the refinement effect of the primary silicon. Attached Figure Description

[0018] Figure 1 This is a metallographic image showing the size of the initial silicon in the Sr-containing process of this invention; Figure 2 For the present invention Figure 1 Enlarged schematic diagram of the structure at point A in the diagram; Figure 3 Metallographic image of the nascent silicon size without Sr process according to the present invention; Figure 4 Metallographic image of the nascent silicon size without Sr process according to the present invention; Figure 5 For the present invention Figure 3 Enlarged schematic diagram of the structure at point B in the diagram; Figure 6 For the present invention Figure 3 Enlarged schematic diagram of the structure at point C; Figure 7 For the present invention Figure 3 Enlarged schematic diagram of the structure at point D; Figure 8 For the present invention Figure 4Enlarged schematic diagram of the structure at point E in the diagram; Figure 9 For the present invention Figure 4 Enlarged schematic diagram of the structure at point F; Figure 10 For the present invention Figure 4 Enlarged schematic diagram of the structure at point G in the diagram; Figure 11 Metallographic image of the initial silicon size in the low-temperature casting process of the present invention at 660 degrees Celsius. Figure 12 For the present invention Figure 11 Enlarged schematic diagram of the structure at point H in the diagram; Figure 13 Metallographic image of the initial silicon size in the low-temperature casting process of the present invention at 700 degrees Celsius; Figure 14 For the present invention Figure 13 Enlarged schematic diagram of the structure at point I; Figure 15 This is a metallographic image showing the size of the nascent silicon in the shrinkage region of this invention. Figure 16 For the present invention Figure 15 A magnified schematic diagram of the structure at point J. Detailed Implementation

[0019] Please see Figure 1-16 The present invention will now be described in detail with reference to the accompanying drawings and embodiments: The low-temperature casting and strontium modification synergistic process for controlling the initial silicon size of aluminum ingots described in this invention is applicable to the production of various aluminum-silicon alloys (including Al-Si-Mg system, Al-Si-Cu system, high-silicon aluminum alloys, etc.) aluminum ingots. The specific steps are as follows, with clear operating requirements, parameter control and precautions for each step to ensure that the process is feasible and replicable.

[0020] S1. Raw Material Preparation and Pretreatment: Select aluminum-silicon alloy raw materials conforming to GB / T 1173-2013 standards (such as A356, ADC12, Al-20Si, etc.). Accurately proportion aluminum ingots, silicon ingots, and other alloying elements (such as magnesium, copper, manganese, etc.) according to the target aluminum ingot composition. The purity of the raw materials must meet the following requirements: aluminum content ≥ 99.7%, silicon content controlled according to the alloy grade requirements, and impurity element content (such as iron, zinc, lead) ≤ 0.5%. During pretreatment, clean the oxide scale, oil, rust, etc., from the surface of the raw materials. This can be done by sanding, alkaline washing (5%~10% NaOH solution, temperature 60~80℃, soaking for 5~10 minutes), followed by water washing and drying to avoid impurities being introduced into the melt, affecting the quality of the aluminum ingot and the modification effect. Simultaneously, prepare an aluminum-strontium master alloy (Al-10Sr master alloy recommended, purity ≥ 99.5%), broken into small pieces of 5~10mm for rapid melting and uniform dispersion.

[0021] S2, Raw Material Melting: The pretreated aluminum-silicon alloy raw material is placed into a resistance melting furnace or induction melting furnace. The heating device is turned on, and the temperature is slowly increased to 720~760℃ (adjusted according to the alloy grade: 720~740℃ for conventional Al-Si alloys, 740~760℃ for high-silicon aluminum alloys). After the raw material is completely melted, mechanical stirring is performed using a graphite stirring rod. The stirring speed is controlled at 30~50 r / min, and the stirring time is 5~8 min to ensure uniform melt composition and avoid local component segregation. During stirring, oxide slag on the surface of the melt is removed promptly (using a graphite slag scraper to gently remove it, avoiding excessive stirring of the melt which could lead to secondary oxidation).

[0022] S3, Refining, Degassing, and Slag Removal: The purpose of refining is to remove gases (mainly hydrogen) and fine inclusions from the melt, ensuring its purity and laying the foundation for subsequent modification and casting. An inert gas refining method is used (argon or nitrogen, purity ≥99.99%). The refining tube is inserted into the bottom of the melt (50-100mm from the furnace bottom), and inert gas is introduced, with the gas flow rate controlled at 0.5-1.0m³ / h. 3 The refining time is 10-15 minutes per hour. During refining, the refining tube is moved slowly to ensure that all areas of the melt are fully refined. After refining, the gas supply is stopped, and the melt is allowed to stand for 5-8 minutes to allow fine inclusions and bubbles to rise to the surface. The oxide slag is then removed again to ensure that the melt is free of obvious inclusions and bubbles. If a higher purity of the melt is required, a small amount of refining agent (such as hexachloroethane, at a concentration of 0.1%-0.2% of the melt mass) can be added to the inert gas to enhance the degassing and slag removal effect.

[0023] S4, Strontium Modification Treatment: After refining, the melt temperature is steadily reduced to 710~730℃ (too high a temperature will cause strontium loss and reduce the modification effect; too low a temperature will make it difficult for the aluminum-strontium master alloy to melt and disperse unevenly). Then, the pretreated aluminum-strontium master alloy is slowly added to the melt, with the amount added controlled according to the target strontium content (the strontium addition amount is 0.02~0.06wt% of the alloy melt mass, recommended 0.03~0.04wt%, which can be finely adjusted according to the alloy composition: for high-silicon aluminum alloys, it can be appropriately increased to 0.04~0.06wt%). After addition, stir with a graphite stirring rod for 3~5 minutes at a stirring speed of 40~60 r / min to ensure that the aluminum-strontium master alloy is completely melted and the strontium element is evenly dispersed in the melt. After stirring, maintain the melt temperature at 710~730℃ and hold for 10~20 minutes (insufficient holding time will lead to incomplete modification, while excessive holding time will cause strontium to degrade easily, affecting the modification effect), thus completing the strontium modification treatment. During the modification process, the atmosphere inside the furnace must be strictly controlled to prevent air from entering. Inert gas protection (such as argon, flow rate 0.2~0.3 m³ / h) can be used. 3 / h), to prevent strontium from being oxidized and burned off.

[0024] S5, Low-Temperature Casting: After the modification and heat preservation are completed, the melt temperature is steadily reduced to 660~710℃ (the casting temperature needs to be adjusted according to the alloy grade and mold type: 680~695℃ for conventional Al-Si alloys, 695~710℃ for high-silicon aluminum alloys; for metal mold casting, the temperature can be appropriately reduced by 5~10℃, and for sand mold casting, the temperature can be appropriately increased by 5~10℃) for low-temperature casting. Before casting, the mold needs to be pretreated: the metal mold needs to be preheated to 150~250℃ (if the preheating temperature is too low, the melt cools too quickly, which can easily cause cold shuts and cracks; if the temperature is too high, it can easily lead to the growth of primary silicon). The preheating method can be electric heating or hot air heating to ensure uniform mold temperature; the sand mold needs to be dried to a moisture content of ≤0.5% to avoid the generation of gas during casting and the formation of porosity defects.

[0025] During casting, a low-flow-rate, steady filling method should be adopted, with the casting speed controlled between 0.5 and 1.0 m / s. Excessive flow rate should be avoided to prevent slag entrapment, secondary oxidation, or impact on the mold, which could affect the uniformity of the aluminum ingot's microstructure. During casting, the flow state of the melt must be continuously observed, and the casting speed adjusted promptly to ensure the mold is fully filled without overflow or slag entrapment. After casting, a riser should be reserved at the top of the mold for feeding purposes, reducing shrinkage cavities and porosity defects inside the aluminum ingot.

[0026] S6. Solidification and Cooling: After casting, allow the aluminum ingot to solidify naturally in the mold. The solidification time is adjusted according to the ingot size: small ingots (≤5kg) solidify for 20-30 minutes, medium ingots (5-20kg) for 30-60 minutes, and large ingots (≥20kg) for 60-120 minutes. Ensure complete solidification to avoid premature demolding, which could lead to deformation and cracking. After solidification, use natural cooling or controlled-temperature cooling (5-10℃ / h) to cool the ingot to room temperature (25-35℃). During cooling, avoid rapid cooling of the ingot surface; cover the surface with insulating cotton to reduce the temperature difference between the inside and outside and lower internal stress. After cooling to room temperature, demold, remove the riser and flash to obtain the finished aluminum ingot.

[0027] S7. Finished Product Inspection and Subsequent Processing: Finished aluminum ingots must undergo rigorous inspection. The size and morphology of primary silicon are observed using a metallographic microscope to ensure that the average size of the primary silicon is ≤20μm, and that it is in the form of fine particles or short rods, with uniform distribution. The hardness of the aluminum ingots is tested using a hardness tester (Brinell hardness HB≥50), and the mechanical properties are tested using a tensile testing machine (tensile strength ≥180MPa, elongation ≥8%). Simultaneously, the chemical composition of the aluminum ingots is tested to ensure that the strontium content and other alloying element content meet design requirements, with no significant impurities exceeding the standard. For aluminum ingots that fail the inspection, they can be remelted, the process parameters adjusted, and then recast. Qualified aluminum ingots can be further processed (such as rolling or extrusion) or stored in a warehouse.

[0028] Casting temperature: 660~710℃. Adjustment criteria: Conventional Al-Si alloys (such as A356, ADC12) have lower melting points and can use 680~695℃; high-silicon aluminum alloys (such as Al-20Si) have higher melting points and require 695~710℃; metal molds have fast thermal conductivity, so the casting temperature can be reduced by 5~10℃ to avoid defects caused by excessive cooling; sand molds have slow thermal conductivity, so the casting temperature can be increased by 5~10℃ to ensure sufficient filling.

[0029] Strontium content: 0.02~0.06wt%. Adjustment basis: For conventional Al-Si alloys, 0.03~0.04wt% is recommended to meet the dual refinement requirements of primary silicon and eutectic silicon; for high-silicon aluminum alloys, the primary silicon content is high and needs to be appropriately increased to 0.04~0.06wt% to enhance the modification effect; if the strontium content is below 0.02wt%, the modification is insufficient and the primary silicon will still be coarse; if it is above 0.06wt%, strontium compound inclusions are easily generated, reducing the alloy's plasticity.

[0030] Tempering time: 10~20min. Adjustment criteria: A holding time of 10~15min is suitable for small melts (≤500kg) to ensure uniform dispersion of strontium and sufficient tempering; a holding time of 15~20min is suitable for large melts (≥500kg) to avoid insufficient tempering in some areas; if the holding time is too long (>20min), strontium will degrade and the tempering effect will decrease; if the holding time is too short (<10min), strontium will not be completely dispersed and the tempering will be uneven.

[0031] Preheating temperature of the casting mold: 110~130℃. Adjustment basis: metal mold preheating temperature 150~200℃, sand mold preheating temperature 200~250℃; the larger the aluminum ingot size, the preheating temperature of the casting mold can be appropriately increased by 5~10℃ to reduce internal stress; the smaller the aluminum ingot size, the preheating temperature can be appropriately decreased by 5~10℃ to accelerate the solidification rate and inhibit silicon phase growth.

[0032] Melting temperature: 720~760℃. Adjustment basis: conventional Al-Si alloys 720~740℃, high silicon aluminum alloys 740~760℃; if the melting temperature is too high, it will increase the risk of melt oxidation and gas absorption, and accelerate the diffusion of silicon atoms, which is not conducive to subsequent refinement; if the temperature is too low, the raw materials are difficult to melt completely, and compositional segregation is likely to occur.

[0033] The following is the experimental data: Experimental parameter design:

[0034] Experimental results statistics:

[0035] Significant refinement effect of primary silicon: The average size of primary silicon in aluminum-silicon alloy ingots is reduced from 35~50μm in conventional processes to ≤20μm, and some can reach 10~15μm. The standard deviation of size distribution is ≤5μm, which is significantly better than single low temperature casting (average size of primary silicon 25~35μm) or single strontium modification process (average size of primary silicon 30~40μm).

[0036] The morphology of silicon phase is significantly improved: the primary silicon is transformed from the coarse block, strip, and needle-like shape of conventional processes into fine, rounded granules or short rods, with no obvious coarse silicon phase aggregation, greatly improving the uniformity of the structure and reducing stress concentration points.

[0037] Significantly improved alloy mechanical properties: Compared with conventional processes, the Brinell hardness of aluminum ingots is increased by 15%~25% (from the conventional 40~50HB to 50~65HB), tensile strength is increased by 10%~20% (from the conventional 160~180MPa to 180~210MPa), elongation is increased by 20%~30% (from the conventional 6~8% to 8~10%), and the cracking and delamination defect rate during subsequent processing is reduced by more than 80%.

[0038] No new complex equipment is required, and it can be adapted to existing casting production lines. The amount of aluminum-strontium master alloy added is small, and the cost increase is ≤5%. Moreover, the process parameters are easy to control, making it suitable for industrial mass production. Production efficiency and finished product qualification rate are both improved to over 95% (compared to 80-85% for conventional processes).

[0039] It is compatible with various aluminum-silicon alloys, including conventional Al-Si-Mg series, Al-Si-Cu series alloys and high-silicon aluminum alloys, and can be used for the production of aluminum ingots of different sizes and for different purposes, offering high flexibility.

[0040] Example 1: A356 aluminum alloy ingot (conventional Al-Si-Mg system, used for automotive parts) 1. Raw material preparation and pretreatment: Select A356 aluminum alloy raw material (composition: Si 6.5~7.5wt%, Mg 0.3~0.45wt%, Al balance), clean the surface oxide scale and oil stains, and crush the aluminum strontium master alloy (Al-10Sr) to 5~10mm.

[0041] 2. Melting: Put the A356 raw material into the induction melting furnace, heat it to 730℃, and after it is completely melted, stir it with a graphite stirring rod for 6 minutes to remove the surface oxide slag.

[0042] 3. Refining and degassing: Introduce argon gas (99.99% purity) at a flow rate of 0.8 m³ / s. 3 / h, refine for 12 minutes, let stand for 6 minutes, and skim off the residue again.

[0043] 4. Strontium modification: Reduce the melt temperature to 720℃, add Al-10Sr master alloy with 0.035wt% strontium, stir for 4 min, hold for 15 min, and protect with argon gas.

[0044] 5. Low-temperature casting: Reduce the melt temperature to 660℃, preheat the metal mold to 180℃, and cast steadily at a speed of 0.8m / s, leaving risers.

[0045] 6. Solidification and cooling: Solidify naturally for 30 minutes, cool to room temperature, then demold and remove risers and flash.

[0046] 7. Test results: The average size of the nascent silicon is 15μm, which is fine and uniformly distributed; the Brinell hardness is 58HB, the tensile strength is 200MPa, and the elongation is 9.5%; the finished product qualification rate is 96%, with no obvious defects.

[0047] Example 2: ADC12 aluminum alloy ingot (conventional Al-Si-Cu system, used for mechanical structural parts) 1. Raw material preparation and pretreatment: Select ADC12 aluminum alloy raw material (composition: Si 9.6~12.0wt%, Cu 1.5~3.5wt%, Al balance), wash with alkali to remove oil and dry, and crush aluminum strontium master alloy (Al-10Sr) to 5~10mm.

[0048] 2. Melting: Put the mixture into a resistance melting furnace, heat it to 740℃, and after it is completely melted, stir for 5 minutes and remove the oxide slag.

[0049] 3. Refining and degassing: Introduce nitrogen (99.99% purity) at a flow rate of 0.6 m³ / h. 3 Add 0.15wt% hexachloroethane refining agent per hour, refine for 10 minutes, let stand for 5 minutes, and remove slag.

[0050] 4. Strontium modification: When the melt temperature drops to 725℃, add Al-10Sr master alloy with a strontium addition of 0.04wt%, stir for 3min, hold for 18min, and protect with nitrogen.

[0051] 5. Low-temperature casting: The melt temperature is reduced to 695℃, the sand mold is preheated to 220℃, and the casting is carried out at a speed of 0.6m / s, with risers reserved.

[0052] 6. Solidification and cooling: Solidify naturally for 40 minutes, cover with insulation cotton and cool to room temperature, then demold.

[0053] 7. Test results: The average size of the nascent silicon is 18μm, in the shape of short rods, and uniformly distributed; Brinell hardness is 62HB, tensile strength is 205MPa, elongation is 8.5%; finished product qualification rate is 95.5%.

[0054] Example 3: Al-20Si high-silicon aluminum alloy ingot (for wear-resistant parts) 1. Raw material preparation and pretreatment: Select Al-20Si high silicon aluminum alloy raw material (Si 20wt%, Al balance), clean surface impurities, and crush aluminum strontium master alloy (Al-10Sr) to 5~10mm.

[0055] 2. Melting: Put the mixture into an induction melting furnace, heat it to 750℃, and after it is completely melted, stir for 8 minutes to ensure that the silicon element is evenly dispersed and remove the oxide slag.

[0056] 3. Refining and degassing: Introduce argon gas at a flow rate of 1.0 m³ / s. 3 / h, refine for 15min, let stand for 8min, skim off the residue.

[0057] 4. Strontium modification: When the melt temperature drops to 730℃, add Al-10Sr master alloy with a strontium addition of 0.05wt%, stir for 5min, hold for 20min, and protect with argon gas.

[0058] 5. Low-temperature casting: The melt temperature is reduced to 705℃, the metal mold is preheated to 200℃, and the metal is cast at a speed of 0.7m / s, with risers reserved.

[0059] 6. Solidification and cooling: Solidify naturally for 60 minutes, then cool to room temperature under controlled temperature and demold.

[0060] 7. Test results: The average size of the nascent silicon is 20μm, which is fine and granular with no coarse silicon phase; the Brinell hardness is 65HB, the tensile strength is 195MPa, and the elongation is 8%; the finished product qualification rate is 95%, and the wear resistance is improved by 20% compared with the conventional process.

Claims

1. A low-temperature casting and strontium modification synergistic process for controlling the initial silicon size of aluminum ingots, characterized in that, By combining strontium modification with low-temperature casting, the nucleation and growth process of primary silicon in the aluminum-silicon alloy melt is regulated, thereby refining the size and rounding the morphology of primary silicon in the aluminum ingot. In the synergistic effect, low-temperature casting is used to suppress the growth of primary silicon phase and promote the generation of a large number of primary silicon nuclei, while strontium modification is used to adsorb onto the primary silicon growth interface, change its growth direction, and suppress its preferential growth.

2. The collaborative process according to claim 1, characterized in that: The process also includes raw material pretreatment, smelting, refining and degassing, and solidification and cooling steps, with each step connected in an orderly manner to ensure synergistic effects.

3. The collaborative process according to claim 2, characterized in that: The melting temperature is 720-760℃. After the raw materials are completely melted, the mixture is stirred evenly and the oxide slag is removed.

4. The collaborative process according to claim 3, characterized in that: The refining and degassing process uses argon or nitrogen gas at a flow rate of 0.5–1.0 m³ / s. 3 / h, refining time 10-15 min, let stand and skim off the residue again.

5. The collaborative process according to claim 4, characterized in that: The strontium modification treatment was carried out at 710–730 °C, using an Al-10Sr master alloy, with a strontium addition amount of 0.02–0.06 wt%.

6. The collaborative process according to claim 5, characterized in that: After adding strontium, stir for 3-5 minutes and keep warm for 10-20 minutes to complete the deterioration. Inert gas is used to protect the strontium during the deterioration process to prevent it from burning out.

7. The collaborative process according to claim 6, characterized in that: The low-temperature casting temperature is 660–710℃, the casting speed is 0.5–1.0 m / s, and a stable low-flow-rate filling method is adopted.

8. The collaborative process according to claim 7, characterized in that: Before casting, the mold is preheated to 110-130℃, with the lower temperature range for metal molds and the higher temperature range for sand molds.

9. The collaborative process according to claim 8, characterized in that: After casting, the aluminum ingot solidifies naturally in the mold. After solidification, it is cooled to room temperature at a controlled temperature of 5-10℃ / h.

10. The collaborative process according to any one of claims 1-9, characterized in that: The aluminum ingots prepared by this process have an average primary silicon size of ≤20 μm, which is uniformly distributed in granular or short rod shape; the aluminum-silicon alloy includes conventional aluminum-silicon alloys and high-silicon aluminum alloys, specifically one or more of A356, ADC12, and Al-20Si.