A method for preparing high-strength and tough layered austenitic steel with layered dislocation density and grain size distribution.
By controlling the difference in laser power between layers to alternately print coarse and fine grain layers, the problem of optimizing the impact toughness of layered austenitic steel in the prior art has been solved, achieving a synergistic improvement in high strength and high toughness. By constructing a heterogeneous structure through grain size and dislocation density gradient, the impact resistance of the material has been enhanced.
Patent Information
- Application Number
- CN202611408592.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies have failed to effectively optimize impact toughness when preparing layered austenitic steel. They lack quantitative research on the relationship between interlayer energy density difference and microstructure properties, making it impossible to optimize Charpy impact toughness and difficult to balance strength and toughness.
By controlling the difference in laser power between layers, coarse and fine grain layers are printed alternately. High and low energy densities are used for alternating scanning to form a gradient in grain size and dislocation density, thereby constructing a heterostructure and achieving differentiation in grain epitaxial growth and dislocation density, thus promoting multiple toughening mechanisms.
It significantly improves the impact toughness and tensile properties of the material, achieving a synergistic improvement in high strength and high toughness. The combined effect of crack propagation path deflection and twin-induced plasticity enhances the material's impact resistance.
Smart Images

Figure CN123103014A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal additive manufacturing technology, and more specifically relates to a method for preparing high-strength and tough layered austenitic steel with layered distribution of dislocation density and grain size. Background Technology
[0002] Laser powder bed fusion (L-PBF) technology enables customized control of the microstructure of metal components through layer-by-layer printing. During the L-PBF forming process, 316L austenitic stainless steel forms a unique cellular dislocation structure and grain boundary element segregation, resulting in grain boundary strengthening and dislocation strengthening effects. This technology has already achieved breakthroughs in applications such as medical implants and complex aerospace components.
[0003] Some existing technologies involve the preparation of heterogeneous austenitic stainless steel by controlling the interlayer printing process parameters. For example, some schemes construct a sandwich structure and differentiate the energy density of the core and edge regions to obtain a heterogeneous structure with different grain size gradients. The uniform elongation is increased from 33% to 44% by utilizing the heterogeneous deformation-induced (HDI) strengthening effect. In other schemes, a high-power interlayer rotation process is used to prepare a fine-grained structure, while a low-power non-rotation process promotes grain epitaxial growth to obtain a coarse-grained structure. The two processes are combined alternately to obtain a layered structure.
[0004] However, existing technologies mostly focus on controlling the grain size and layered microstructure, and optimizing tensile properties. The optimization and control of impact toughness remains a gap. There is a lack of quantitative research on the relationship between interlayer energy density difference and microstructure properties, making it impossible to determine the optimal process parameter window. The influence of layered microstructure on crack propagation behavior under impact loads is unclear, and Charpy impact toughness optimization cannot be achieved. Therefore, it is urgent to establish a quantitative relationship between interlayer power difference, microstructure, and mechanical properties, and to develop a layered 316L stainless steel preparation technology that combines excellent impact toughness and tensile properties. Summary of the Invention
[0005] The purpose of this invention is to provide a method for preparing high-strength and high-toughness layered austenitic steel with layered dislocation density and grain size distribution, and more specifically, to provide a method for preparing austenitic steel with layered dislocation density and grain size distribution by controlling the interlayer laser power difference, so as to solve the problems existing in the prior art.
[0006] To achieve the above objectives, the present invention provides the following solution: One of the technical solutions of this invention is to provide a method for preparing high-strength and high-toughness layered austenitic steel with layered distribution of dislocation density and grain size, the steps of which include: Alternating coarse-grained and fine-grained layers are designed in the construction direction, and laser powder melting is used for alternating printing to prepare high-strength and tough layered austenitic steel with layered distribution of dislocation density and grain size. The thickness of a single layer of the coarse-grained or fine-grained layer is an integer multiple of the thickness of a single powder layer.
[0007] Furthermore, the thickness of the single powder layer is 20-40 μm, preferably 30 μm.
[0008] Furthermore, the fine-grained layer is printed using high energy density.
[0009] Optionally, the high energy density process parameters are: laser spot diameter 35-40μm, inert gas protective atmosphere (oxygen content ≤100ppm), laser power 200W, scanning speed 900mm / s, scanning spacing 0.06mm, and interlayer rotation angle 67°.
[0010] The combination of the above parameters together constitutes the high volumetric energy density of 123 J / mm². 3 .
[0011] Furthermore, the coarse-grained layer is printed using low energy density.
[0012] Optionally, the low energy density process parameters are: laser spot diameter 35-40μm, inert gas protective atmosphere (oxygen content ≤100ppm), laser power 130-160W (preferably 140W), scanning speed 900mm / s, scanning spacing 0.06mm, and interlayer rotation angle 67°.
[0013] The combination of the above parameters together results in a low volumetric energy density of 86-99 J / mm². 3 .
[0014] In this invention, the interlayer power difference ΔP between the fine-grained layer and the coarse-grained layer is 40-70W, preferably 50-65W, and more preferably 60W.
[0015] This invention achieves grain size gradient control through interlayer power difference. Under low power conditions, the melt pool depth is small, the overlap area is small, and the number of remelted fragments is low, promoting epitaxial growth and forming a coarse-grained layer. Under high power conditions, the overlap area of the melt pool increases, the number of remelted fragments increases, and the increased content of nano-oxides provides heterogeneous nucleation sites, inhibiting epitaxial growth and forming a fine-grained layer. It also achieves dislocation density differentiation; during low-power printing, the rapid cooling rate and thermal shrinkage stress concentration lead to an increased dislocation density of 1.2 × 10⁻⁶. 14 m -2 High-power printing enhances the remelting effect, and dynamic recovery and recrystallization eliminate some dislocations, reducing the dislocation density to 1×10⁻⁶. 14 m -2It achieved cell structure size regulation, with cell structure size of 700-750nm in the high-power region and 500-550nm in the low-power region.
[0016] Furthermore, the raw materials for the coarse-grained layer and the fine-grained layer are gas-atomized 316L stainless steel powder, H13 steel powder, or 18Ni300 martensitic aging steel.
[0017] Furthermore, the ratio of the thickness of the coarse-grained layer to the thickness of the fine-grained layer is 1:1-3.
[0018] The second technical solution of the present invention provides a high-strength and tough layered austenitic steel with layered distribution of dislocation density and grain size obtained by the above preparation method.
[0019] The third technical solution of the present invention provides an application of high-strength and tough layered austenitic steel with the above-mentioned layered distribution of dislocation density and grain size in complex components such as injection molds and aerospace.
[0020] The present invention discloses the following technical effects: This invention achieves the ordered construction of material microstructure at the microscale by precisely controlling the interlayer laser power difference, resulting in significant beneficial effects. Specifically, by employing an alternating high and low power scanning strategy, the thermal behavior and solidification process of the molten pool are directly controlled: high power input (e.g., 200W) forms a deeper molten pool, enhancing the interlayer remelting effect. This not only increases the number of heterogeneous nucleation sites, effectively suppressing grain epitaxial growth and thus refining the grains, but also promotes dynamic recovery and recrystallization, reduces dislocation density, and generates larger cellular structures (700-750nm); while low power input forms a shallow molten pool, where epitaxial growth dominates, which is conducive to the formation of coarse grains. The rapid cooling leads to thermal stress concentration, significantly increasing the dislocation density and forming smaller cellular structures (500-550nm). This power modulation-based synergistic control ultimately creates clear grain size gradients (alternating between coarse and fine grain layers), dislocation density gradients (alternating between high and low density regions), and cellular structure size gradients in the material. These gradient structures jointly induce multiple strengthening and toughening mechanisms such as back stress reinforcement and crack propagation path deflection. As a result, while ensuring high strength, the plasticity and impact toughness of the material are greatly improved, successfully breaking through the bottleneck of the difficulty in synergistically improving the strength and toughness of homogeneous materials.
[0021] The layered austenitic steel prepared by this invention exhibits a significant improvement in toughness under impact loading. This beneficial effect stems from the synergistic effect of a multi-stage toughening mechanism: during crack propagation, the strain incompatibility between the coarse-grained and fine-grained layers induces geometrically necessary dislocation accumulation at the interface, generating back stress and thus relaxing the stress concentration at the crack tip. Simultaneously, the significant grain size difference between the layers forces repeated deflection of the crack path, significantly increasing the energy required for crack propagation. Furthermore, due to its larger grain size, the coarse-grained layer has a lower twinning critical shear stress, making it more prone to activating the twinning-induced plasticity (TWIP) effect during impact, further coordinating plastic deformation and releasing localized stress. The combined effect of back stress strengthening, crack deflection, and the TWIP effect simultaneously and significantly improves the crack propagation work and impact toughness of the material.
[0022] Compared with existing homogeneous and layered microstructure preparation techniques, this invention achieves synergistic optimization of microstructure and properties through interlayer power control, resulting in the following significant advantages: First, this method successfully solves the problem of balancing strength and toughness. At an interlayer power difference ΔP = 60W, while maintaining high strength (tensile strength ≥ 620MPa), the elongation and crack propagation energy are increased by 12.14% and 11.45% respectively compared to homogeneous microstructures, and the Charpy V-notch impact toughness is ≥ 280J, achieving a synergistic improvement in strength and toughness. Second, the layered structure significantly improves impact resistance. The crack propagation path is deflected due to the microstructure difference, and the propagation energy can be increased by up to 23.26% (ΔP = 70W), while the stress concentration factor at the crack tip is reduced by 15-20%, thus greatly enhancing the material's ability to resist dynamic loads. Furthermore, this invention possesses excellent microstructure designability; by adjusting the power difference, the grain size gradient (15-30μm) and dislocation density distribution (3-12×10⁻⁶) can be precisely controlled. 14 m -2 The design integrates structure and performance by defining the layer thickness ratio (1:1-3). Finally, the process window is clear and reliable, establishing a quantitative mapping relationship between interlayer power difference, grain size difference, and mechanical properties. The optimal process range for strength and toughness matching (ΔP=50-65W) is determined, providing clear process guidance and reliable basis for the engineering application of high-performance layered stainless steel. Attached Figure Description
[0023] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 The images show the pore distribution of samples prepared under different interlayer power differences (ΔP) in Examples 1-3, where (a) is Example 1, (b) is Example 2, and (c) is Example 3.
[0024] Figure 2 The images show optical microscope images of the molten pool morphology of samples prepared under different interlayer power differences (ΔP) in Examples 1-3, where (a) is Example 1, (b) is Example 2, and (c) is Example 3.
[0025] Figure 3 The EBSD inverse pole figure (IPF) and Kernel average orientation difference (KAM) diagrams of the samples prepared in Examples 2 and 3 are shown, where (a) is the IPF diagram of Example 2, (b) is the KAM diagram of Example 2, (c) is the IPF diagram of Example 3, and (d) is the KAM diagram of Example 3.
[0026] Figure 4 The images show the SEM images of the melt pool distribution and the cellular structure of selected points in the sample of Example 3. (a) is the SEM image of the melt pool distribution, and (b) and (c) are the SEM images of the cellular structure of selected points in (a).
[0027] Figure 5 The effect of interlayer power regulation on mechanical properties is shown in (a) for engineering stress-strain curve and (b) for impact load-displacement curve.
[0028] Figure 6 The stress-strain curve of the sample in Comparative Example 1 is shown.
[0029] Figure 7 The impact load-displacement curve is shown for the sample in Comparative Example 1.
[0030] Figure 8 This is an optical microscope image of the molten pool morphology for Comparative Example 1.
[0031] Figure 9 This is an optical microscope image of the molten pool morphology of the sample in Comparative Example 2.
[0032] Figure 10 The tensile fracture morphology of the sample in Comparative Example 2 is shown. Detailed Implementation
[0033] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0034] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Any stated value or intermediate value within a stated range, as well as each smaller range between any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0035] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.
[0036] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be readily apparent to those skilled in the art. This specification and embodiments are merely exemplary.
[0037] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.
[0038] Unless otherwise specified, all raw materials and reagents involved in the specific embodiments of this invention are commercially available products.
[0039] Unless otherwise specified, room temperature and normal temperature in the specific embodiments of this invention refer to 20-30℃.
[0040] It should be noted that any aspects not described in detail in this invention are conventional practices in the field and are not the focus of this invention.
[0041] In a specific embodiment of the present invention, the raw materials for the coarse-grained layer and the fine-grained layer are illustrated by gas-atomized 316L stainless steel powder. The composition is shown in Table 1, with a particle size D50 of 35 μm, a maximum particle size ≤ 75 μm, and vacuum drying at 120°C for 6 hours.
[0042] Table 1 In a specific embodiment of the present invention, the laser powder bed fusion equipment selected is the JHL100E+ type L-PBF equipment, with a laser spot diameter of 37.7μm, a substrate of 316L stainless steel, and an oxygen content of ≤100ppm in the forming chamber.
[0043] Example 1 The preparation steps for high-strength and high-toughness layered austenitic steel with layered dislocation density and grain size distribution include (interlayer power difference ΔP = 50W): S1. Establish a layered model, and alternately stack fine-grained layers and coarse-grained layers, with a single layer thickness of 480μm; S2, Fine Crystal Layer: Laser power 200W, scanning speed 900mm / s, scanning spacing 0.06mm, single powder layer thickness 0.03mm, interlayer rotation 67°, 16 layers printed; S3, Coarse Crystal Layer: Laser power 150W, scanning speed 900mm / s, scanning spacing 0.06mm, single powder layer thickness 0.03mm, interlayer rotation 67°, 16 layers printed; S4. Repeat the above alternating printing process to the sample height to obtain a high-strength and tough layered austenitic steel with layered distribution of dislocation density and grain size.
[0044] Example 2 Compared with Example 1, the only difference is that the printing laser power of the coarse grain layer in step S3 is 140W, and the interlayer power difference ΔP = 60W.
[0045] Example 3 Compared with Example 1, the only difference is that the printing laser power of the coarse grain layer in step S3 is 130W, and the interlayer power difference ΔP = 70W.
[0046] Example 4 Compared with Example 1, the only difference is that the printing laser power of the coarse grain layer in step S3 is 160W, and the interlayer power difference ΔP = 40W.
[0047] Comparative Example 1 Preparation of homogeneous tissue samples: Compared with Example 1, the only difference is that the laser power of the coarse-grained layer was adjusted to 200W, and the product obtained was a homogeneous tissue sample.
[0048] The preparation steps of L-PBF homogeneous austenitic steel include: S1. Establish a block sample printing model, and use the same printing preparation process for the entire model; S2. Process parameter settings: laser power 200W, scanning speed 900mm / s, scanning interval 0.06mm, single powder layer thickness 0.03mm, interlayer rotation 67°, printing until model completion.
[0049] Comparative Example 2 The only difference from Example 1 is that the laser power for printing the coarse grain layer in step S3 is 120W.
[0050] Test case Figure 1 The images show the pore distribution of samples prepared under different interlayer power differences (ΔP) in Examples 1-3, where (a) is Example 1, (b) is Example 2, and (c) is Example 3.
[0051] Figure 2 The images show optical microscope images of the molten pool morphology of samples prepared under different interlayer power differences (ΔP) in Examples 1-3, where (a) is Example 1, (b) is Example 2, and (c) is Example 3.
[0052] Figure 3 The EBSD inverse pole figure (IPF) and Kernel average orientation difference (KAM) diagrams of the samples prepared in Examples 2 and 3 are shown, where (a) is the IPF diagram of Example 2, (b) is the KAM diagram of Example 2, (c) is the IPF diagram of Example 3, and (d) is the KAM diagram of Example 3.
[0053] Figure 4 The images show the SEM images of the melt pool distribution and the cellular structure of selected points in the sample of Example 3. (a) is the SEM image of the melt pool distribution, and (b) and (c) are the SEM images of the cellular structure of selected points in (a).
[0054] Depend on Figures 1-4 It can be seen that, Figure 1 The image shows the density and defect distribution. Samples prepared under different interlayer power differences (200W-150W (Example 1), 200W-140W (Example 2), 200W-130W (Example 3)) all exhibited extremely high internal density (≥99.5%), with very few and dispersed pores. This indicates that changing the interlayer printing power does not deteriorate the molding quality, ensuring the basic macroscopic properties of the material. Macroscopic morphology of the molten pool (…) Figure 2 and Figure 4 As shown in (a) of the diagram, the alternating light and dark layered features along the construction direction (BD) become more pronounced as the interlayer power difference increases. Figure 4 (a) clearly shows the difference in melt pool depth under alternating high and low power conditions; the melt pool depth in the 200W high-power region is significantly greater than that in the 130W low-power region. The high-power melt pool has a stronger remelting effect on the previous layer, with a melt pool depth of approximately 200 μm, while the melt pool depth in the low-power region is only about 60 μm. This depth difference is the core reason for the formation of heterogeneous layered structures. Microstructure evolution ( Figure 3 ): EBSD test ( Figure 3 Figures (a) and (c) show that the samples exhibit a clear coarse-to-fine grain stratification. In the 200W-130W (Example 3) samples, the grain size in the coarse-grained region is significantly finer than at a single power level (reduced from 151.08 μm to 61.57 μm), which is attributed to the thermal cycling of adjacent high-power layers promoting grain fragmentation. KAM diagram ( Figure 3 (b) and (d) in the figure reflect the difference in dislocation density distribution. The darker colored areas correspond to the low-power printing areas, showing higher residual strain and dislocation aggregation, which provides the material with additional strain hardening capability. Substructural features ( Figure 4 In (b) and (c) of the image: High-magnification SEM observation revealed that the interior of the molten pool consists of a fine cellular structure. The average size of the cellular structure at 200 W power is approximately 724 nm, while at 130 W power, due to the faster cooling rate, the cellular structure is further refined to 544 nm. This submicron-sized cellular structure and the solute segregation within it are important contributing factors to the improved material strength.
[0055] Prepare sheet-like specimens according to GB / T 228.1 standard, and test them on an MTS-200kN testing machine at 10... -3 s -1 Strain rate test for tensile properties.
[0056] Charpy V-notch specimens with a notch depth of 2 mm and a diameter of 3 mm × 10 mm × 55 mm were prepared according to GB / T 229 standard. The impact toughness was tested using an Instron 9450 drop hammer impact tester.
[0057] Figure 5 The effect of interlayer power regulation on mechanical properties is shown in (a) for engineering stress-strain curve and (b) for impact load-displacement curve.
[0058] Figure 6 The stress-strain curve of the sample in Comparative Example 1 is shown.
[0059] Figure 7 The impact load-displacement curve is shown for the sample in Comparative Example 1.
[0060] Depend on Figures 5-7It can be seen that as the interlaminar power difference gradually increases, the elongation gradually increases (from 55.8% to 62.7%), and the yield strength and tensile strength also improve (yield strength increases from 532 MPa to 540 MPa, and tensile strength increases from 710 MPa to 726 MPa). However, when the interlaminar power difference reaches 70 W (Example 3), the yield strength and tensile strength of the material begin to decrease (from 532 MPa to 524 MPa), which corresponds to the displacement-load diagram in the impact test, showing a decrease in strength. This is mainly because the grain size difference of the 200 W-130 W (Example 3) sample is large, resulting in stronger stress concentration at the interface, causing premature cracking at the interface and leading to a decrease in yield strength. Among them, the tensile properties are most significantly improved when the interlaminar power difference is 60 W (Example 2), exhibiting higher work hardening ability and a 12.14% increase in elongation compared to the 200 W (Comparative Example 1) sample. This also indicates that when the grain size in the coarse-grained region of the layered structure is too large, the overall strength of the material will decrease due to the interface and the resulting stress. The maximum impact load of the 200W-130W (Example 3) sample was slightly lower than that of the 200W (Comparative Example 1) sample, while the maximum impact load of the other three groups of layered structures was higher than that of the 200W (Comparative Example 1) sample. After reaching the maximum load, the rate of decline of the curves for the 200W-130W (Example 3) and 200W-140W (Example 2) samples slowed down, indicating that the layered structure effectively hindered crack propagation. Analysis of crack initiation success and crack propagation work showed that the increase in interlayer power difference had a relatively small impact on crack initiation success, slightly higher than that of the 200W (Comparative Example 1) sample, while the effect on crack propagation work was more significant, increasing with the increase of interlayer power difference. When the interlaminar power difference increased to 70 W (Example 3), the crack propagation energy of the layered structure (21.31 J) increased by 23.26% compared to the homogeneous structure (17.28 J), and the total impact energy increased by 12.14%. Example 4 shows that when the interlaminar power is small, the strength and plasticity are slightly improved simultaneously. The yield strength (YS) of this sample is about 535 MPa, the tensile strength (UTS) reaches 715 MPa, and the elongation increases to about 57%. Compared with the 200 W constant power sample (YS ~ 530 MPa, elongation ~ 56%), under these parameters, the introduction of a heterostructure achieves a slight increase in strength while maintaining high plasticity. At the same time, the crack propagation resistance is enhanced, with the total impact energy (Et) of the sample increasing to about 28.5 J and the crack propagation energy (Ep) increasing to about 18 J, indicating that the introduction of the interlaminar power gradient effectively improves the material's ability to resist crack propagation during the fracture stage.
[0061] Engineering stress-strain curve of sample 1 (Comparative Example 1) Figure 6The results showed that its elongation was only 55.8%, and its yield strength was approximately 532 MPa. Compared with the example, the homogeneous microstructure, due to the lack of back stress strengthening and the coarse-fine grain synergistic deformation mechanism during deformation, experienced earlier saturation of work hardening capacity, resulting in significantly lower plasticity than Example 2 (elongation 62.7%). In the impact test ( Figure 7 In Comparative Example 1, the load-displacement curve of the sample showed a rapid decrease in load with increasing displacement after reaching the maximum load (approximately 5.5 kN). In contrast, the curve of the heterogeneous layered sample (e.g., 200 W-140 W (Example 2)) exhibited a smoother decrease with multiple fluctuations, indicating that the homogeneous structure has a weaker ability to impede crack propagation. Its crack propagation energy was only 17.28 J, significantly lower than that of the heterogeneous layered sample constructed through power regulation in this invention. Figure 8 The image shows an optical microscope image of the molten pool morphology in Comparative Example 1. As can be seen from the image, the molten pool of Comparative Example 1 (single 200W power) is uniformly distributed and does not exhibit obvious layered alternation characteristics. Its density was measured to be 99.7%, maintaining high forming quality, but the microstructure consists of relatively simple equiaxed crystals, lacking the regulatory effect of heterogeneous interfaces on dislocations and cracks.
[0062] Figure 9 This is an optical microscope image of the molten pool morphology of the sample in Comparative Example 2.
[0063] Figure 10 The tensile fracture morphology of the sample in Comparative Example 2 is shown.
[0064] Depend on Figures 9-10 It can be seen that when the interlayer printing power difference further expands to 80W (i.e., 200W-120W), the molding quality and mechanical properties of the material deteriorate significantly. Melt pool morphology and defect distribution: Optical microscopy observation shows that the melt pool distribution of Comparative Example 2 sample is extremely uneven, with numerous pores and unfused defects inside. This is because the energy density of the 120W low-power component is too low to fully melt it and form a good metallurgical bond with the previous deposited layer, resulting in a significant decrease in interlayer bonding strength. Tensile fracture morphology further confirms the presence of defects; numerous large and deep irregular pores are observed on the fracture surface, exhibiting obvious brittle fracture characteristics and lacking the typical ductile fracture signs of the layered structure in the examples. Due to the presence of numerous macroscopic defects, the effective load-bearing area of Comparative Example 2 sample is significantly reduced, resulting in severe stress concentration. This leads to its strength and elongation being far lower than those of Examples 1-3. Compared to the preferred power difference range of 40W-60W in this invention, the experimental results of Comparative Example 2 show that excessive energy input fluctuations can lead to instability in the laser selective melting process, making it impossible to obtain dense and high-performance heterogeneous layered structures.
[0065] In summary, through the comparison of the above performance, the present invention has determined the optimal strength and toughness optimization process window: the optimal strength and toughness matching range is selected as 60W of interlayer power difference, which can achieve an elongation increase of ≥12% and a crack propagation energy increase of ≥11% while maintaining the strength without reduction. The optimal Charpy impact toughness optimization process window was determined: an interlayer power difference of 70 W represents the optimal match for Charpy impact toughness, achieving a crack propagation energy improvement of ≥20%. The quantitative relationship between microstructure and properties was clarified: a quantitative mapping relationship between interlayer power difference, grain size difference, and crack propagation work / elongation was established, providing a theoretical basis for the design of heterostructure materials.
[0066] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on the differences from other embodiments. The same or similar parts between the various embodiments can be referred to each other.
[0067] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a high-strength and high-toughness layered austenitic steel with layered dislocation density and grain size distribution, characterized in that the steps include... include: Alternating coarse-grained and fine-grained layers are designed in the construction direction, and laser powder melting is used for alternating printing to prepare high-strength and tough layered austenitic steel with layered distribution of dislocation density and grain size. The thickness of a single layer of the coarse-grained or fine-grained layer is an integer multiple of the thickness of a single powder layer.
2. The preparation method according to claim 1, characterized in that, The thickness of a single powder layer is 20-40 μm.
3. The preparation method according to claim 1, characterized in that, The fine-grained layer is printed using high energy density.
4. The preparation method according to claim 3, characterized in that, The high energy density process parameters are as follows: laser spot diameter 35-40μm, inert gas protective atmosphere, laser power 200W, scanning speed 900mm / s, scanning spacing 0.06mm, and interlayer rotation angle 67°.
5. The preparation method according to claim 1, characterized in that, The coarse-grained layer is printed using low energy density.
6. The preparation method according to claim 5, characterized in that, The low energy density process parameters are as follows: laser spot diameter 35-40μm, inert gas protective atmosphere, laser power 130-160W, scanning speed 900mm / s, scanning spacing 0.06mm, and interlayer rotation angle 67°.
7. The preparation method according to claim 1, characterized in that, The raw materials for the coarse-grained layer and the fine-grained layer are gas-atomized 316L stainless steel powder, H13 steel powder, or 18Ni300 maraging steel.
8. The preparation method according to claim 1, characterized in that, The ratio of the thickness of the coarse-grained layer to the thickness of the fine-grained layer is 1:1-3.
9. A high-strength and high-toughness layered austenitic steel with layered distribution of dislocation density and grain size, prepared by the preparation method according to any one of claims 1-8.
10. The application of a high-strength and high-toughness layered austenitic steel with layered dislocation density and grain size distribution as described in claim 9 in injection molds and complex aerospace components.