Welding control method and apparatus for pulsed MIG welding of aluminum alloy battery casings

By employing a preset pulse waveform and reverse movement of the welding torch in pulsed MIG welding of aluminum alloy battery casings, welding defects were solved, and the sealing performance and structural reliability of the battery casings were improved.

CN123103114APending Publication Date: 2026-11-17ZHEJIANG CHINALCO AUTOMOBILE LIGHTWEIGHT TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611579627.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the prior art, aluminum alloy battery casings are prone to forming and metallurgical defects during pulsed MIG welding, such as arc crater shrinkage, hot cracks, and insufficient weld tail height, which affect the sealing performance and structural reliability of the battery casing.

Method used

The pulsed MIG welding process is adopted, which controls the welding current by preset pulse waveform and gradually reduces the peak current and pulse frequency as the welding approaches the end point. Combined with the reverse movement of the welding torch and delayed arc interruption, a smooth transition of welding heat input and compensation filling of the molten pool are achieved.

Benefits of technology

It significantly improves the sealing reliability and structural safety of aluminum alloy battery casing welding, reduces defects such as arc crater shrinkage and hot cracking, and ensures the continuity and integrity of weld formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103114A_ABST
    Figure CN123103114A_ABST
Patent Text Reader

Abstract

This application provides a welding control method and apparatus for pulsed MIG welding of aluminum alloy battery casings. It includes: employing a pulsed MIG welding process, controlling the welding current according to a preset pulse waveform, controlling the welding torch to move along the weld direction at a first speed, and maintaining a constant wire feed speed to weld the aluminum alloy battery casing; when the welding progresses to a first preset distance from the weld endpoint, gradually reducing the peak current until the weld endpoint is reached; after detecting that the weld endpoint has been reached, reducing the pulse frequency to a preset frequency, and simultaneously controlling the welding torch to move in the opposite direction to weld to a second preset distance; after detecting that the welding torch has moved to the second preset distance, maintaining wire feed for a first preset time, then controlling the welding torch to extinguish the arc and stopping wire feed to complete the welding. This solves the problem of related technologies using a single current decay to terminate welding, which carries the risk of welding defects and thus affects the structural reliability of the battery casing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of pulsed MIG welding technology for aluminum alloy battery casings, and more specifically, to a welding control method, apparatus, storage medium, and welding robot for pulsed MIG welding of aluminum alloy battery casings. Background Technology

[0002] Aluminum alloy battery casings are widely used in power batteries and energy storage systems for new energy vehicles. These casings are typically made of 6xxx series aluminum alloy sheets, with a thickness generally ranging from 1.5 to 3.0 mm. Due to the metallurgical properties of aluminum alloys, such as high thermal conductivity, large coefficient of linear expansion, high solidification shrinkage, and strong susceptibility to hot cracking, forming and metallurgical defects are easily generated during pulsed MIG welding, especially in the arc-end stage of the weld.

[0003] During the arc-ending phase of welding, the welding heat input typically transitions rapidly from a stable welding state to an arc-extinguishing state. This sudden decrease in heat supply to the molten pool reduces its support capacity, causing the liquid metal to solidify before it has been adequately compensated for. Simultaneously, the tensile stress generated by solidification shrinkage concentrates in the center of the crater, easily inducing defects such as crater shrinkage cavities, hot cracks, and localized collapse. Furthermore, insufficient weld reinforcement or discontinuous weld formation at the tail end can adversely affect the sealing performance and structural reliability of the battery casing.

[0004] In related technologies, arc termination control is typically achieved by simply reducing the current or directly cutting off the arc. This type of method terminates the welding by only reducing the current, without systematically regulating the reduction of heat input, the volume compensation of liquid metal, and the evolution of solidification stress. This leads to a sudden drop in the heat supply of the molten pool and insufficient support capacity during the arc termination phase, which in turn causes forming and metallurgical defects such as arc crater shrinkage, hot cracks, local collapse, and insufficient weld tail height, seriously affecting the sealing performance and structural reliability of the battery casing.

[0005] In summary, the relevant technology achieves welding termination through a single current decay, which poses a risk of welding defects and could affect the structural reliability of the battery casing. Summary of the Invention

[0006] The main objective of this application is to provide a welding control method, apparatus, storage medium, and welding robot for pulsed MIG welding of aluminum alloy battery casings, so as to at least solve the problem that related technologies achieve welding termination through a single current decay, which poses a risk of welding defects and thus affects the structural reliability of the battery casing.

[0007] To achieve the above objectives, according to one aspect of this application, a welding control method for pulsed MIG welding of aluminum alloy battery casings is provided, comprising: employing a pulsed MIG welding process, controlling the welding current according to a preset pulse waveform, controlling the welding torch to move along the weld direction at a first speed, and welding the aluminum alloy battery casing at a constant wire feed speed, wherein the preset pulse waveform includes a peak current, a base current, and a pulse frequency; when the welding progresses to a first preset distance from the weld end point, controlling the peak current in the preset pulse waveform to gradually decrease according to a preset current attenuation strategy until the weld end point is reached; after detecting that the weld end point has been reached, reducing the pulse frequency to a preset frequency, simultaneously controlling the welding torch to move in the opposite direction to weld to a second preset distance, and when the welding torch is detected to have moved to the second preset distance, maintaining wire feed to a first preset duration, controlling the welding torch to cut off the arc and stopping wire feed to complete the welding.

[0008] Optionally, controlling the welding torch to move in the opposite direction to weld to a second preset distance includes: controlling the welding torch to move in the opposite direction at a second speed to weld to the second preset distance, wherein the second speed is less than the first speed.

[0009] Optionally, controlling the peak current in the preset pulse waveform to gradually decrease according to a preset current attenuation strategy includes: performing step-by-step attenuation or continuous attenuation processing on the peak current in the preset pulse waveform at a preset attenuation rate.

[0010] Optionally, controlling the arc interruption of the welding torch and stopping the wire feeding includes: controlling the arc interruption of the welding torch and stopping the wire feeding when a second preset duration is reached.

[0011] Optionally, the peak current at the end of the weld is 50% to 70% of the peak current in the preset pulse waveform.

[0012] Optionally, the first preset distance is 3mm to 10mm.

[0013] Optionally, the second preset distance is 2mm to 5mm.

[0014] According to another aspect of this application, a welding control device for pulsed MIG welding of aluminum alloy battery casings is provided, comprising: a first control unit, configured to use pulsed MIG welding process, control the welding current according to a preset pulse waveform, and control the welding torch to move along the weld direction at a first speed and a constant wire feed speed to weld the aluminum alloy battery casing, wherein the preset pulse waveform includes a peak current, a base current, and a pulse frequency; a second control unit, configured to control the peak current in the preset pulse waveform to gradually decrease according to a preset current attenuation strategy when the welding progresses to a first preset distance from the weld end point, until the welding reaches the weld end point; and a third control unit, configured to reduce the pulse frequency to a preset frequency after detecting that the welding has reached the weld end point, simultaneously control the welding torch to move in the opposite direction to weld to a second preset distance, and, upon detecting that the welding torch has moved to the second preset distance, maintain wire feed to a first preset duration, control the welding torch to cut off the arc and stop wire feed to complete the welding.

[0015] According to another aspect of this application, a computer-readable storage medium is provided, the computer-readable storage medium including a stored program, wherein, when the program is executed, it controls the device where the computer-readable storage medium is located to perform any of the described welding control methods for pulsed MIG welding of aluminum alloy battery casings.

[0016] According to another aspect of this application, a welding robot is provided, comprising: one or more processors, a memory, and one or more programs, wherein the one or more programs are stored in the memory and configured to be executed by the one or more processors, the one or more programs including a welding control method for performing any of the described pulsed MIG welding methods for aluminum alloy battery casings.

[0017] By applying the technical solution of this application, a smooth transition from a stable to a terminated state of welding heat input is achieved by gradually reducing the peak current at a first preset distance, avoiding a sudden and drastic contraction of the molten pool volume and reserving a process window for subsequent compensation. Secondly, after detecting the weld endpoint, by reducing the pulse frequency and combining it with the welding torch moving in the opposite direction by a second preset distance, the metal accumulation effect generated by the reverse movement and the stability of the low-frequency arc are utilized to promote the molten metal to flow back and fill the crater area under the action of surface tension and arc force, effectively compensating for the metal loss at the end. Finally, by maintaining wire feeding to a first preset duration before extinguishing the arc, the molten pool still has the ability to replenish liquid metal in the early stage of solidification, achieving welding compensation and significantly improving the density and forming continuity of the crater area, thereby greatly improving the sealing reliability and structural safety of the battery casing welding. This solves the problem of related technologies that use a single current decay to terminate welding, which poses a risk of welding defects and thus affects the structural reliability of the battery casing. Attached Figure Description

[0018] The accompanying drawings, which form part of this application, are used to provide a further understanding of this application. The illustrative embodiments and descriptions of this application are used to explain this application and do not constitute an undue limitation of this application. In the drawings:

[0019] Figure 1 A hardware structure block diagram of a mobile terminal for performing a welding control method for pulsed MIG welding of aluminum alloy battery casings, according to an embodiment of this application, is shown.

[0020] Figure 2 A schematic flowchart of a welding control method for pulsed MIG welding of aluminum alloy battery casings according to an embodiment of this application is shown.

[0021] Figure 3 A schematic diagram of a specific welding control method for pulsed MIG welding of aluminum alloy battery casings according to an embodiment of this application is shown;

[0022] Figure 4 A top view schematic diagram of the welding torch retraction trajectory provided according to an embodiment of this application is shown;

[0023] Figure 5 A schematic diagram of the welding process current waveform provided according to an embodiment of this application is shown;

[0024] Figure 6 A comparative schematic diagram of the crater filling effect provided according to an embodiment of this application is shown;

[0025] Figure 7 A structural block diagram of a welding control device for pulsed MIG welding of aluminum alloy battery casings, according to an embodiment of this application, is shown. Detailed Implementation

[0026] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. This application will now be described in detail with reference to the accompanying drawings and embodiments.

[0027] To enable those skilled in the art to better understand the present application, the technical solutions in the embodiments of the present application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present application, and not all embodiments. Based on the embodiments in the present application, all other embodiments obtained by those of ordinary skill in the art without creative effort should fall within the scope of protection of the present application.

[0028] It should be noted that the terms "first," "second," etc., in the specification, claims, and accompanying drawings of this application are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate for the embodiments of this application described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion; for example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.

[0029] As described in the background section, related technologies terminate welding by a single current decay, which carries the risk of welding defects and thus affects the structural reliability of the battery casing. To address the issue of welding defects caused by terminating welding by a single current decay, which in turn affects the structural reliability of the battery casing, embodiments of this application provide a welding control method, apparatus, storage medium, and welding robot for pulsed MIG welding of aluminum alloy battery casings.

[0030] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings in the embodiments of the present invention.

[0031] The methods and embodiments provided in this application can be executed on a mobile terminal, computer terminal, or similar computing device. Taking running on a mobile terminal as an example, Figure 1 This is a hardware structure block diagram of a mobile terminal for a welding control method used in pulse MIG welding of aluminum alloy battery casings, according to an embodiment of the present invention. Figure 1 As shown, a mobile terminal may include one or more ( Figure 1 Only one is shown in the diagram. A processor 102 (which may include, but is not limited to, a microprocessor MCU or a programmable logic device FPGA, etc.) and a memory 104 for storing data are also shown. The mobile terminal may further include a transmission device 106 for communication functions and an input / output device 108. Those skilled in the art will understand that... Figure 1 The structure shown is for illustrative purposes only and does not limit the structure of the mobile terminal described above. For example, the mobile terminal may also include components that are more... Figure 1 The more or fewer components shown, or having the same Figure 1 The different configurations shown.

[0032] The memory 104 can be used to store computer programs, such as application software programs and modules, like the computer program corresponding to the welding control method for pulsed MIG welding of aluminum alloy battery casings in this embodiment of the invention. The processor 102 executes various functional applications and data processing by running the computer program stored in the memory 104, thereby implementing the above-described method. The memory 104 may include high-speed random access memory and may also include non-volatile memory, such as one or more magnetic storage devices, flash memory, or other non-volatile solid-state memory. In some instances, the memory 104 may further include memory remotely located relative to the processor 102, and these remote memories can be connected to the mobile terminal via a network. Examples of the aforementioned networks include, but are not limited to, the Internet, corporate intranets, local area networks, mobile communication networks, and combinations thereof. The transmission device 106 is used to receive or send data via a network. Specific examples of the aforementioned networks may include wireless networks provided by the mobile terminal's communication provider. In one example, the transmission device 106 includes a Network Interface Controller (NIC), which can be connected to other network devices via a base station to communicate with the Internet. In one example, the transmission device 106 may be a radio frequency (RF) module, which is used to communicate with the Internet wirelessly.

[0033] This embodiment provides a welding control method for pulsed MIG welding of aluminum alloy battery casings, which runs on a mobile terminal, computer terminal, or similar computing device. It should be noted that the steps shown in the flowchart in the accompanying drawings can be executed in a computer system such as a set of computer-executable instructions. Also, although the logical order is shown in the flowchart, in some cases, the steps shown or described can be executed in a different order than that shown here.

[0034] Figure 2 This is a flowchart of a welding control method for pulsed MIG welding of aluminum alloy battery casings according to an embodiment of this application. Figure 2 As shown, the method includes the following steps:

[0035] Step S201: Using pulsed MIG welding process, the welding current is controlled according to the preset pulse waveform, and the welding torch is controlled to move along the weld direction at a first speed and the wire feeding speed is constant to weld the aluminum alloy battery casing. The preset pulse waveform includes peak current, base current and pulse frequency.

[0036] The first speed is the normal welding speed of the pulsed MIG welding process, which can be set according to welding requirements.

[0037] Step S202: When the welding progresses to the first preset distance from the end of the weld, the peak current in the preset pulse waveform is gradually reduced according to the preset current attenuation strategy until the welding reaches the end of the weld.

[0038] Specifically, the peak current at the end of the weld is 50% to 70% of the peak current in the preset pulse waveform.

[0039] Step S203: After detecting that the welding has reached the end point of the weld, the pulse frequency is reduced to a preset frequency, and the welding torch is controlled to move in the opposite direction to weld to a second preset distance. When the welding torch is detected to have moved to the second preset distance, the wire feeding is maintained for a first preset duration, and then the arc of the welding torch is cut off and the wire feeding is stopped to complete the welding.

[0040] The first preset distance can be set to 3mm to 10mm, and the second preset distance can be set to 2mm to 5mm, wherein the second preset distance is less than the first preset distance;

[0041] Specifically, the first preset duration can be set to 0.1s to 0.3s, ensuring the molten pool remains in a metal-supplying state before arc termination, guaranteeing sufficient filling conditions in the crater area. Subsequently, delayed arc termination control is implemented within a time range of 0.1s to 0.5s, allowing the arc energy to gradually decay and achieve stable arc extinguishing, while simultaneously stopping wire feeding. This delayed control method ensures the molten pool maintains short-term liquid compensation capability during the initial solidification stage, thereby achieving controlled solidification and filling of the crater area, effectively reducing the risk of welding defects such as crater shrinkage, end depression, and hot cracking.

[0042] In this embodiment, by applying steps S201, S202, and S203, a smooth transition from a stable to a terminated state of welding heat input is achieved by gradually reducing the peak current at the first preset distance. This avoids sudden and drastic shrinkage of the molten pool volume and reserves a process window for subsequent compensation. Secondly, after detecting the weld endpoint, by reducing the pulse frequency and combining it with the welding torch moving in the opposite direction by a second preset distance, the metal accumulation effect generated by the reverse movement and the stability of the low-frequency arc are utilized to encourage the molten metal to flow back and fill the crater area under the action of surface tension and arc force, effectively compensating for the metal loss at the end. Finally, by maintaining wire feeding to the first preset duration before extinguishing the arc, the molten pool still has the ability to replenish liquid metal in the early stages of solidification, achieving welding compensation and significantly improving the density and continuity of the crater area, thereby greatly improving the sealing reliability and structural safety of the battery casing welding. This solves the problem of related technologies that use a single current decay to terminate welding, which carries the risk of welding defects and thus affects the structural reliability of the battery casing.

[0043] In the specific implementation process, controlling the welding torch to move in the opposite direction to weld to the second preset distance includes: controlling the welding torch to move in the opposite direction at a second speed to weld to the second preset distance, wherein the second speed is less than the first speed.

[0044] The second speed can be set to 30% to 70% of the first speed.

[0045] In this embodiment, the speed relationship of the welding torch's reverse movement is defined, i.e., the second speed is less than the first speed. This parameter setting plays a crucial role in optimizing the crater filling quality. The lower reverse welding speed (second speed) directly leads to an increase in heat input per unit length and a longer molten pool existence time. In aluminum alloy welding, the molten pool cooling rate is closely related to solidification behavior. A slower moving speed allows the arc to heat the crater area for a longer time, helping to maintain the liquid state of the molten pool and reduce the local cooling rate gradient. This not only facilitates the escape of gases and the floating of inclusions in the molten pool, reducing porosity and slag inclusion defects; more importantly, the slow retraction movement allows the molten metal sufficient time to redistribute and fill the central depression of the crater under the influence of gravity, surface tension, and arc plasma flow. Compared to high-speed retraction, which may cause metal spatter or uneven filling, low-speed retraction can form a fuller and smoother crater shape, effectively eliminating the problem of insufficient tail height, ensuring the geometric consistency of the weld end, and meeting the requirements of the battery casing for high-precision sealing joints.

[0046] Specifically, controlling the peak current in the preset pulse waveform to gradually decrease according to the preset current attenuation strategy includes: performing step-by-step attenuation or continuous attenuation processing on the peak current in the preset pulse waveform at a preset attenuation rate.

[0047] In this embodiment, the attenuation strategy for the peak current is specifically defined, encompassing either stepped or continuous attenuation, to achieve refined and stable heat input control. Traditional direct arc termination or linear attenuation often leads to thermal shock, while stepped or continuous attenuation strategies allow the control system to dynamically adjust energy output based on the real-time state of the molten pool. Stepped attenuation, through discrete current steps, enables the molten pool to adapt to energy changes at each stage, avoiding thermal stress concentration; continuous attenuation provides a smoother energy transition curve, further eliminating molten pool fluctuations caused by sudden changes in heat input. This refined current control not only effectively suppresses rapid solidification and volume shrinkage of the molten pool caused by a sharp drop in heat input during the arc termination stage, but also makes the droplet transition smoother, reducing metal spatter during the arc termination process. By precisely controlling the descent slope of the peak current, the temperature field distribution in the crater region can be optimized, allowing the solidification front to advance smoothly from the weld tail to the interior, thereby significantly reducing solidification shrinkage stress, suppressing the generation of microcracks, and improving the uniformity and mechanical properties of the weld metal.

[0048] More specifically, controlling the arc interruption of the welding torch and stopping the wire feeding includes: controlling the arc interruption of the welding torch and stopping the wire feeding when the second preset duration is reached.

[0049] In this embodiment, immediately extinguishing the arc after the welding torch retracts causes rapid crusting on the surface of the molten pool, while the remaining liquid portion inside develops shrinkage cavities due to the inability to receive subsequent metal replenishment. By setting a second preset duration (preferably 0.1s-0.5s), the system can maintain continuous wire feeding before the arc extinguishes, utilizing this delay effect to inject additional filler metal into the crater area. Simultaneously, the delay allows the molten pool to undergo brief self-smoothing using residual heat after arc extinguishing, reducing depressions caused by surface tension. This coordinated control over the time dimension fundamentally eliminates crater shrinkage defects, improves the density of the weld end, and is crucial for preventing battery electrolyte leakage or external corrosion intrusion, thereby ensuring the lifespan of the new energy battery casing.

[0050] To enable those skilled in the art to better understand the technical solution of this application, the implementation process of the welding control method for pulse MIG welding of aluminum alloy battery casings will be described in detail below with reference to specific embodiments.

[0051] To address the problems of sudden drop in heat input, insufficient molten pool volume compensation, and stress concentration due to solidification shrinkage in the existing pulsed MIG welding arc termination stage, this embodiment relates to a specific welding control method for pulsed MIG welding of aluminum alloy battery casings. By constructing a phased control model, a heat input gradient reduction stage, a spatial volume compensation stage, and a timing arc termination control stage are sequentially set in the welding terminal area to achieve systematic control of the arc termination process.

[0052] Specifically, this invention achieves a smooth transition of the molten pool heat input from a stable welding state to a termination state by implementing peak current gradient reduction control during the arc termination phase; it also achieves volume compensation of liquid metal in the arc crater area by forming a local metal accumulation zone through the spatial retraction movement of the welding torch; and it alleviates the concentration of solidification shrinkage stress by adjusting the solidification rhythm of the molten pool and reducing the cooling rate gradient through delayed arc termination control.

[0053] Through the aforementioned multi-dimensional collaborative control mechanism, this embodiment can effectively suppress defects such as arc crater shrinkage, hot cracks, and tail collapse, thereby improving the forming stability and sealing reliability of the weld end of the thin-walled aluminum alloy battery casing.

[0054] Figure 3 A schematic diagram illustrating the specific welding control method for pulsed MIG welding of aluminum alloy battery casings, as shown below. Figure 3 As shown, the specific steps include the following:

[0055] S1, Main Welding Stage:

[0056] Aluminum alloy battery casings are welded using pulsed MIG welding. During the main welding process, the welding current is output stably according to a preset pulse waveform, which includes peak current, base current, and pulse frequency. The peak current is used to achieve full melting and metallurgical bonding of the base material, while the base current is used to maintain stable arc combustion and continuous molten pool existence. Simultaneously, with constant wire feeding speed and stable welding travel speed, the molten pool is kept in a continuous and stable flow and solidification equilibrium state, thereby forming a uniform and continuously formed weld body structure.

[0057] S2, Gradual Filling Stage:

[0058] When the welding process progresses to a preset distance from the weld end, it enters the slow-descent filling stage, preferably 3mm to 10mm. During this stage, the peak current is gradually controlled by stepwise or continuous attenuation to reduce it to a set proportional range, while the base current remains stable to maintain arc continuity and uninterrupted wire feeding and melting. Simultaneously, by extending the pulse period or reducing the pulse frequency, the heat input per unit time is gradually reduced, thereby achieving controlled shrinkage of the molten pool volume and a smooth transition of heat input, avoiding molten pool collapse, depressions, or unstable formation at the weld end due to sudden changes in heat input.

[0059] S3, Retreat Compensation Phase:

[0060] Figure 4 This is a schematic diagram of the welding torch retraction trajectory, as shown below. Figure 4 As shown, when welding reaches the end of the weld, while maintaining continuous arc burning and wire feeding, the welding torch retracts 2mm to 5mm in the opposite direction of the weld. During the retraction process, a low-frequency pulsed current mode is used to reduce arc disturbance intensity and enhance molten pool stability. Simultaneously, the retraction speed is controlled at 30% to 70% of the main welding speed, creating a controlled heat input zone for repair welding in the retraction area. During this process, the molten droplets continuously transfer and are redistributed to the end molten pool area under the combined action of arc force, gravity, and surface tension, thereby metallurgically compensating for and filling the crater area, making up for end metal loss, and reducing the probability of shrinkage cavities and solidification defects.

[0061] S4, Delayed Arc Breaking Phase:

[0062] After the retraction compensation is completed, wire feeding is maintained for 0.1s to 0.3s to ensure the molten pool remains in a metal-supplying state before arc extinguishing, guaranteeing sufficient filling conditions in the crater area. Subsequently, delayed arc extinguishing control is implemented within a time range of 0.1s to 0.5s, allowing the arc energy to gradually decay and achieve stable arc extinguishing, while simultaneously stopping wire feeding. This delayed control method ensures the molten pool maintains short-term liquid compensation capability during the initial solidification stage, thereby achieving controlled solidification and filling of the crater area, effectively reducing the risk of welding defects such as crater shrinkage, end depression, and hot cracking.

[0063] Figure 5 This is a schematic diagram of the current waveform during the welding process. The welding current control in steps S1, S2, S3, and S4 is as follows: Figure 5 As shown.

[0064] in addition, Figure 6 This diagram illustrates the comparison of crater filling effects. The welding results of this solution (crater compensation control) and related technologies (direct arc interruption) are shown below. Figure 6 As shown.

[0065] Compared with relevant welding solutions, the implementation scheme of this application specifically achieves the following beneficial effects:

[0066] 1) By setting a slow-fall filling stage, the peak current and pulse parameters are gradually attenuated, so that the welding heat input can be continuously and smoothly transitioned, avoiding the rapid shrinkage of the molten pool volume at the end of the weld due to sudden changes in heat input, thereby effectively suppressing the instantaneous collapse of the molten pool and the generation of end depression defects.

[0067] 2) By introducing a retraction compensation stage, the welding torch is reversed under the conditions of continuous arc burning and continuous wire feeding, so that the molten metal is transported back to the arc crater area under the action of arc force and surface tension, forming a local metal enrichment and compensation accumulation zone, thereby significantly increasing the metal filling amount in the arc crater area.

[0068] 3) Through the synergistic effect of gradual transition and shrinkage compensation, the stress gradient in the solidification process of the weld end area is effectively released, reducing the concentration of residual tensile stress caused by uneven solidification and shrinkage, thereby reducing the tendency of hot cracks and solidification cracks to occur.

[0069] 4) By improving the integrity and density of the metal filling at the weld tail, the forming quality and surface continuity of the weld end are significantly improved, thereby enhancing the overall sealing reliability and structural service safety of the aluminum alloy battery casing.

[0070] 5) By coordinating the control of current attenuation, welding torch retraction path and arc interruption delay, multi-parameter coupled stable regulation of the arc termination process is achieved, thereby improving the stability, consistency and process repeatability of the welding process.

[0071] This application provides specific welding examples, taking a 6xxx series aluminum alloy battery casing as an example. The plate thickness is 2mm, and the welding is performed using pulsed MIG welding process, specifically including the following:

[0072] During the main welding stage, the peak current is set to 180A, the base current is 60A, and the pulse frequency is 120Hz to ensure stable penetration and continuous weld formation.

[0073] During the slow-filling stage, the process begins approximately 5 mm from the end of the weld. The peak current is reduced in a cycle-by-cycle manner, decreasing by about 5% per pulse cycle until the peak current decays to about 60% of the main welding peak current. The base current remains constant to maintain stable arc combustion and continuous wire feeding and melting process, thereby achieving a smooth decay of the heat input to the molten pool.

[0074] During the retraction compensation stage, when welding reaches the end position of the weld, under the conditions of continuous arc burning and continuous wire feeding, the welding torch retracts 3mm in the opposite direction of the weld. During the retraction process, the welding speed is adjusted to 50% of the main welding speed. At the same time, a low-frequency pulse current mode is adopted to reduce arc disturbance and enhance the stability of the molten pool, so that the molten metal flows back to the arc crater area under the combined action of arc force, gravity and surface tension and achieves compensation filling.

[0075] During the arc-breaking control phase, the wire feeding system continues to supply wire 0.2 seconds in advance before arc breaking to ensure that there is still a source of metal supply at the end of the molten pool. Then, after a 0.3-second delay, the arc energy is gradually reduced and the arc is broken. At the same time, the wire feeding is stopped, so that the molten pool can maintain a liquid-filled state for a short time and complete controlled solidification.

[0076] The weld quality inspection results showed that shrinkage defects in the arc crater area were significantly reduced, the continuity of weld end formation was significantly improved, no hot cracks or obvious solidification cracks were observed, and the stability of welding quality was improved.

[0077] This application also provides a welding control device for pulsed MIG welding of aluminum alloy battery casings. It should be noted that the welding control device for pulsed MIG welding of aluminum alloy battery casings in this application can be used to execute the welding control method for pulsed MIG welding of aluminum alloy battery casings provided in this application. This device is used to implement the above embodiments and preferred embodiments; details already described will not be repeated. As used below, the term "module" can refer to a combination of software and / or hardware that performs a predetermined function. Although the device described in the following embodiments is preferably implemented in software, hardware implementation, or a combination of software and hardware, is also possible and contemplated.

[0078] The following describes the welding control device for pulsed MIG welding of aluminum alloy battery casings provided in the embodiments of this application.

[0079] Figure 7 This is a schematic diagram of a welding control device for pulsed MIG welding of aluminum alloy battery casings according to an embodiment of this application. Figure 7 As shown, the device includes:

[0080] The first control unit 71 is used to weld the aluminum alloy battery casing by using pulsed MIG welding process, controlling the welding current according to a preset pulse waveform, and controlling the welding torch to move along the weld direction at a first speed and a constant wire feeding speed. The preset pulse waveform includes peak current, base current and pulse frequency.

[0081] The second control unit 72 is used to control the peak current in the preset pulse waveform to gradually decrease according to the preset current attenuation strategy when the welding is advanced to a first preset distance from the end of the weld, until the welding reaches the end of the weld.

[0082] The third control unit 73 is used to reduce the pulse frequency to a preset frequency after detecting that the welding has reached the end of the weld, and at the same time control the welding torch to move in the opposite direction to weld to a second preset distance. When the welding torch is detected to have moved to the second preset distance, the control unit maintains wire feeding for a first preset time, and then controls the welding torch to cut off the arc and stop wire feeding to complete the welding.

[0083] The first preset distance can be set to 3mm to 10mm, and the second preset distance can be set to 2mm to 5mm, with the second preset distance being less than the first preset distance.

[0084] Specifically, the peak current at the end of the weld is 50% to 70% of the peak current in the preset pulse waveform.

[0085] In this embodiment, by gradually reducing the peak current at the first preset distance, a smooth transition from a stable to a terminated state of welding heat input is achieved, avoiding sudden and drastic shrinkage of the molten pool volume and reserving a process window for subsequent compensation. Secondly, after detecting the weld endpoint, by reducing the pulse frequency and combining it with the welding torch moving in the opposite direction by a second preset distance, the metal accumulation effect generated by the reverse movement and the stability of the low-frequency arc are utilized to promote the molten metal to flow back and fill the crater area under the action of surface tension and arc force, effectively compensating for the end-point metal loss. Finally, by maintaining wire feeding to the first preset duration before extinguishing the arc, the molten pool still has the ability to replenish liquid metal in the early stages of solidification, achieving welding compensation and significantly improving the density and forming continuity of the crater area, thereby greatly improving the sealing reliability and structural safety of the battery casing welding. This solves the problem of related technologies that use a single current decay to terminate welding, which carries the risk of welding defects and thus affects the structural reliability of the battery casing.

[0086] As an optional solution, the third control unit includes a first control module for controlling the welding torch to move in the opposite direction at a second speed to weld to the second preset distance, wherein the second speed is less than the first speed.

[0087] In one alternative, the second control unit includes a processing module for performing stepwise or continuous attenuation processing on the peak current in the preset pulse waveform at a preset attenuation rate.

[0088] In one alternative, the third control unit further includes a second control module for controlling the welding torch to cut off the arc and stop wire feeding when a second preset time is reached.

[0089] The aforementioned welding control device for pulsed MIG welding of aluminum alloy battery casings includes a processor and a memory. The first control unit, second control unit, third control unit, etc., are all stored as program units in the memory, and the processor executes these program units to achieve their respective functions. All of the above modules reside in the same processor; alternatively, the modules may be located in different processors in any combination.

[0090] The processor contains a core, which retrieves the corresponding program unit from memory. One or more cores can be configured. By adjusting the core parameters, issues can be addressed. However, some technologies use a single current decay to terminate welding, which carries the risk of welding defects and could affect the structural reliability of the battery casing.

[0091] The memory may include non-permanent memory in computer-readable media, such as random access memory (RAM) and / or non-volatile memory, such as read-only memory (ROM) or flash RAM, and the memory includes at least one memory chip.

[0092] This invention provides a computer-readable storage medium including a stored program, wherein, when the program is executed, it controls the device containing the computer-readable storage medium to perform the welding control method for pulsed MIG welding of aluminum alloy battery casings.

[0093] Specifically, the welding control method for pulsed MIG welding of aluminum alloy battery casings includes:

[0094] Step S201: Using pulsed MIG welding process, the welding current is controlled according to the preset pulse waveform, and the welding torch is controlled to move along the weld direction at a first speed and the wire feeding speed is constant to weld the aluminum alloy battery casing. The preset pulse waveform includes peak current, base current and pulse frequency.

[0095] Step S202: When the welding progresses to the first preset distance from the end of the weld, the peak current in the preset pulse waveform is gradually reduced according to the preset current attenuation strategy until the welding reaches the end of the weld.

[0096] Step S203: After detecting that the welding has reached the end point of the weld, the pulse frequency is reduced to a preset frequency, and the welding torch is controlled to move in the opposite direction to weld to a second preset distance. When the welding torch is detected to have moved to the second preset distance, the wire feeding is maintained for a first preset duration, and then the arc of the welding torch is cut off and the wire feeding is stopped to complete the welding.

[0097] This invention provides a processor for running a program, wherein the program executes the welding control method for pulsed MIG welding of aluminum alloy battery casings.

[0098] Specifically, the welding control method for pulsed MIG welding of aluminum alloy battery casings includes:

[0099] Step S201: Using pulsed MIG welding process, the welding current is controlled according to the preset pulse waveform, and the welding torch is controlled to move along the weld direction at a first speed and the wire feeding speed is constant to weld the aluminum alloy battery casing. The preset pulse waveform includes peak current, base current and pulse frequency.

[0100] Step S202: When the welding progresses to the first preset distance from the end of the weld, the peak current in the preset pulse waveform is gradually reduced according to the preset current attenuation strategy until the welding reaches the end of the weld.

[0101] Step S203: After detecting that the welding has reached the end point of the weld, the pulse frequency is reduced to a preset frequency, and the welding torch is controlled to move in the opposite direction to weld to a second preset distance. When the welding torch is detected to have moved to the second preset distance, the wire feeding is maintained for a first preset duration, and then the arc of the welding torch is cut off and the wire feeding is stopped to complete the welding.

[0102] This invention provides an electronic device, which includes a processor, a memory, and a program stored in the memory and executable on the processor. When the processor executes the program, it performs at least the following steps:

[0103] Step S201: Using pulsed MIG welding process, the welding current is controlled according to the preset pulse waveform, and the welding torch is controlled to move along the weld direction at a first speed and the wire feeding speed is constant to weld the aluminum alloy battery casing. The preset pulse waveform includes peak current, base current and pulse frequency.

[0104] Step S202: When the welding progresses to the first preset distance from the end of the weld, the peak current in the preset pulse waveform is gradually reduced according to the preset current attenuation strategy until the welding reaches the end of the weld.

[0105] Step S203: After detecting that the welding has reached the end point of the weld, the pulse frequency is reduced to a preset frequency, and the welding torch is controlled to move in the opposite direction to weld to a second preset distance. When the welding torch is detected to have moved to the second preset distance, the wire feeding is maintained for a first preset duration, and then the arc of the welding torch is cut off and the wire feeding is stopped to complete the welding.

[0106] The devices mentioned in this article can be servers, PCs, tablets, mobile phones, etc.

[0107] This application also provides a computer program product, which, when executed on a data processing device, is suitable for executing an initialization program having at least the following method steps:

[0108] Step S201: Using pulsed MIG welding process, the welding current is controlled according to the preset pulse waveform, and the welding torch is controlled to move along the weld direction at a first speed and the wire feeding speed is constant to weld the aluminum alloy battery casing. The preset pulse waveform includes peak current, base current and pulse frequency.

[0109] Step S202: When the welding progresses to the first preset distance from the end of the weld, the peak current in the preset pulse waveform is gradually reduced according to the preset current attenuation strategy until the welding reaches the end of the weld.

[0110] Step S203: After detecting that the welding has reached the end point of the weld, the pulse frequency is reduced to a preset frequency, and the welding torch is controlled to move in the opposite direction to weld to a second preset distance. When the welding torch is detected to have moved to the second preset distance, the wire feeding is maintained for a first preset duration, and then the arc of the welding torch is cut off and the wire feeding is stopped to complete the welding.

[0111] It is obvious to those skilled in the art that the modules or steps of the present invention described above can be implemented using general-purpose computing devices. They can be centralized on a single computing device or distributed across a network of multiple computing devices. They can be implemented using computer-executable program code, and thus can be stored in a storage device for execution by a computing device. In some cases, the steps shown or described can be performed in a different order than those described herein, or they can be fabricated as separate integrated circuit modules, or multiple modules or steps can be fabricated as a single integrated circuit module. Thus, the present invention is not limited to any particular combination of hardware and software.

[0112] Those skilled in the art will understand that embodiments of this application can be provided as methods, systems, or computer program products. Therefore, this application can take the form of a completely hardware embodiment, a completely software embodiment, or an embodiment combining software and hardware aspects. Furthermore, this application can take the form of a computer program product embodied on one or more computer-usable storage media (including, but not limited to, disk storage, CD-ROM, optical storage, etc.) containing computer-usable program code.

[0113] This application is described with reference to flowchart illustrations and / or block diagrams of methods, apparatus (systems), and computer program products according to embodiments of this application. It will be understood that each block of the flowchart illustrations and / or block diagrams, and combinations of blocks in the flowchart illustrations and / or block diagrams, can be implemented by computer program instructions. These computer program instructions can be provided to a processor of a general-purpose computer, special-purpose computer, embedded processor, or other programmable data processing apparatus to produce a machine, such that the instructions, which execute via the processor of the computer or other programmable data processing apparatus, generate instructions for implementing the flowchart... Figure 1 One or more processes and / or boxes Figure 1 A device that provides the functions specified in one or more boxes.

[0114] These computer program instructions may also be stored in a computer-readable storage medium that can direct a computer or other programmable data processing device to function in a particular manner, such that the instructions stored in the computer-readable storage medium produce an article of manufacture including instruction means, which are implemented in a process Figure 1 One or more processes and / or boxes Figure 1 The function specified in one or more boxes.

[0115] These computer program instructions may also be loaded onto a computer or other programmable data processing equipment to cause a series of operational steps to be performed on the computer or other programmable equipment to produce a computer-implemented process, thereby providing instructions that execute on the computer or other programmable equipment for implementing the process. Figure 1 One or more processes and / or boxes Figure 1 The steps of the function specified in one or more boxes.

[0116] In a typical configuration, a computing device includes one or more processors (CPU), input / output interfaces, network interfaces, and memory.

[0117] Memory may include non-persistent memory in computer-readable media, such as random access memory (RAM) and / or non-volatile memory, such as read-only memory (ROM) or flash RAM. Memory is an example of computer-readable media.

[0118] Computer-readable media include both permanent and non-permanent, removable and non-removable media that can store information using any method or technology. Information can be computer-readable instructions, data structures, modules of programs, or other data. Examples of computer storage media include, but are not limited to, phase-change memory (PRAM), static random access memory (SRAM), dynamic random access memory (DRAM), other types of random access memory (RAM), read-only memory (ROM), electrically erasable programmable read-only memory (EEPROM), flash memory or other memory technologies, CD-ROM, digital versatile optical disc (DVD) or other optical storage, magnetic tape, magnetic disk storage or other magnetic storage devices, or any other non-transferable medium that can be used to store information accessible by a computing device. As defined herein, computer-readable media does not include transient computer-readable media, such as modulated data signals and carrier waves.

[0119] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0120] It should also be noted that the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus. Unless otherwise specified, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes that element.

[0121] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A welding control method for pulsed MIG welding of aluminum alloy battery casings, characterized in that, include: The aluminum alloy battery casing is welded using a pulsed MIG welding process. The welding current is controlled according to a preset pulse waveform, and the welding torch is controlled to move along the weld direction at a first speed and a constant wire feed speed. The preset pulse waveform includes peak current, base current and pulse frequency. When the welding progresses to the first preset distance from the end of the weld, the peak current in the preset pulse waveform is gradually reduced according to the preset current attenuation strategy until the welding reaches the end of the weld. After detecting that the welding has reached the end of the weld, the pulse frequency is reduced to a preset frequency, and the welding torch is controlled to move in the opposite direction to weld to a second preset distance. When the welding torch is detected to have moved to the second preset distance, the wire feed is maintained for a first preset duration, and then the arc of the welding torch is cut off and the wire feed is stopped to complete the welding.

2. The method according to claim 1, characterized in that, Controlling the welding torch to move in the reverse direction to weld to the second preset distance includes: The welding torch is controlled to move in the opposite direction at a second speed to weld to the second preset distance, wherein the second speed is less than the first speed.

3. The method according to claim 1, characterized in that, Controlling the peak current in the preset pulse waveform to gradually decrease according to a preset current attenuation strategy includes: The peak current in the preset pulse waveform is subjected to stepwise or continuous attenuation at a preset attenuation rate.

4. The method according to claim 1, characterized in that, Controlling the arc interruption of the welding torch and stopping the wire feed includes: When the second preset duration is reached, the welding torch is controlled to cut off the arc and the wire feeding is stopped.

5. The method according to claim 1, characterized in that, The peak current at the end of the weld is 50% to 70% of the peak current in the preset pulse waveform.

6. The method according to claim 1, characterized in that, The first preset distance is 3mm to 10mm.

7. The method according to claim 1, characterized in that, The second preset distance is 2mm to 5mm.

8. A welding control device for pulsed MIG welding of aluminum alloy battery casings, characterized in that, include: The first control unit is used to weld the aluminum alloy battery casing by using pulsed MIG welding process, controlling the welding current according to a preset pulse waveform, and controlling the welding torch to move along the weld direction at a first speed and a constant wire feed speed. The preset pulse waveform includes peak current, base current and pulse frequency. The second control unit is used to control the peak current in the preset pulse waveform to gradually decrease according to a preset current attenuation strategy when the welding progresses to a first preset distance from the end of the weld, until the welding reaches the end of the weld. The third control unit is used to reduce the pulse frequency to a preset frequency after detecting that the welding has reached the end of the weld, and at the same time control the welding torch to move in the opposite direction to weld to a second preset distance. When the welding torch is detected to have moved to the second preset distance, the control unit maintains wire feeding for a first preset time, and then controls the welding torch to cut off the arc and stop wire feeding to complete the welding.

9. A computer-readable storage medium, characterized in that, The computer-readable storage medium includes a stored program, wherein, when the program is executed, it controls the device containing the computer-readable storage medium to perform the welding control method for pulsed MIG welding of aluminum alloy battery casings as described in any one of claims 1 to 7.

10. A welding robot, characterized in that, include: One or more processors, a memory, and one or more programs, wherein the one or more programs are stored in the memory and configured to be executed by the one or more processors, the one or more programs including a welding control method for pulsed MIG welding of aluminum alloy battery casings as described in any one of claims 1 to 7.