A laser filler wire welding device and welding method for 430 ferritic stainless steel NiCr-3

By using a vibration drive and optimizing welding parameters in laser filler wire welding of 430 ferritic stainless steel, the problems of Nb segregation and hot cracking of NiCr-3 welding wire under rapid solidification conditions were solved, and the stability and toughness of the weld were improved.

CN123103183APending Publication Date: 2026-11-17SHANXI TAIGANG STAINLESS STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611443476.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the laser welding process of 430 ferritic stainless steel, NiCr-3 welding wire is prone to Nb segregation and hot cracking under rapid solidification conditions, which leads to cracking or breakage of the weld during subsequent cold rolling. Existing technologies lack effective control methods.

Method used

A laser filler wire welding device for 430 ferritic stainless steel NiCr-3 was adopted. The device uses a vibration drive to generate a lateral micro-oscillation at the end of the welding wire, and controls the wire landing point, the molten pool mixing state and heat input. Combined with BSE and EDS detection, the welding parameters were optimized to reduce the risk of Nb segregation.

Benefits of technology

It effectively reduces Nb segregation between the weld centerline and dendrites, avoids the propagation of post-weld hot cracks, and ensures the stability and toughness of the weld during cold rolling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103183A_ABST
    Figure CN123103183A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of stainless steel laser welding technology, and provides a laser filler wire welding device and method for 430 ferritic stainless steel NiCr-3. The device includes a laser welding head, a shielding gas nozzle, a wire guide nozzle, and a vibration drive component. The laser welding head is positioned above the weld seam of the stainless steel base material to emit laser light. A shielding gas nozzle is located on one side of the laser irradiation end, and a wire guide nozzle is located on the other side. The vibration drive component is fixed to the outside of the wire guide nozzle by a connecting clamp. Laser filler wire welding is performed using NiCr-3 or ERNiCr-3 type welding wire, and the welding process is controlled by the fusion ratio and feed rate. The wire quantity control keeps the base metal dilution rate and nominal Nb content of the weld within a controllable range; the wire landing point is controlled at the front to the middle of the molten pool; heat input is controlled; and a vibration drive is used to generate medium-frequency, small-amplitude lateral micro-vibration at the end of the wire to enhance local disturbance in the molten pool and break up continuous Nb-rich paths. This invention treats welding material selection, Nb input, molten pool mixing, solidification segregation, hot cracking, and cold rolling results as a control closed loop, thereby improving the welding effect of 430 ferritic stainless steel, reducing Nb segregation index, reducing solidification cracking, and improving cold rolling throughput with high reduction rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of stainless steel laser welding technology, and relates to NiCr-3 laser filler wire welding of 430 ferritic stainless steel plates and strips, specifically a NiCr-3 laser filler wire welding device and welding method for 430 ferritic stainless steel. Background Technology

[0002] 430 ferritic stainless steel is a low-Ni or essentially Ni-free Cr-based stainless steel, widely used in sheet and strip products where corrosion resistance, surface quality, and cost are critical. For annealed and pickled 430 stainless steel sheet and strip, head and tail welding or process continuation welding are often required during production, and the welded joint may continue to undergo a significant proportion of cold rolling deformation. For example, in the production of 430 stainless steel sheet and strip with a thickness of about 5mm, the weld area needs to withstand about 60% to 75% of the subsequent cold rolling reduction.

[0003] Under these conditions, the quality of the weld cannot be judged solely by its post-weld appearance and conventional connection strength; it must also meet the following requirements:

[0004] (1) The weld metal should have sufficient plasticity and toughness;

[0005] (2) The weld and heat-affected zone should not have excessively high hardness peak values;

[0006] (3) There should be good deformation compatibility between the weld, fusion line and base material;

[0007] (4) There should be no through-cracks or continuous weak segregation after welding;

[0008] (5) Cracking and breakage should not occur along the weld centerline, between dendrites or in the fusion zone during subsequent cold rolling.

[0009] Traditional 309 type austenitic stainless steel welding materials can be used in some ferritic stainless steel welding scenarios. However, in the case of laser welding of 430 ferritic stainless steel followed by large deformation cold rolling, 309 type welds are prone to problems such as local high hardness, thickness-direction microstructure differences, and deformation incoordination. Existing sample evidence shows that 309 welds exhibit significant cracking under cupping and cold deformation conditions. The transverse hardness increases to approximately 345 HV0.3 from the base material's approximately 180 to 220 HV0.3, and the localized thickness-direction hardness can reach approximately 347.5 HV0.3, indicating a significant hardness peak and the risk of local strain concentration.

[0010] NiCr-3 or ERNiCr-3 type nickel-based welding wires have good plasticity, toughness and adaptability to dissimilar metal welding. When used for laser filler wire welding of 430 ferritic stainless steel, they can improve the plasticity of the weld and the coordination of cold deformation. Comparative samples have shown that NiCr-3 welds do not exhibit the same severe cracking phenomenon as 309 welds after cupping. Therefore, it is necessary to replace 309 type welding materials in engineering.

[0011] However, NiCr-3 type welding wires typically contain about 2% to 3% Nb. For example, Thermanit Nicro 82 welding wire's quality certificate shows an Nb content of about 2.63 wt.%, while the Nb content in the 430 base metal is only about 0.0021 wt.%. The Nb content differs by more than a thousand times. Under the conditions of small weld pool, rapid cooling, and short solidification time in laser filler welding, the Nb introduced by the welding wire is prone to segregation between dendrites, at the weld centerline, or in the final solidification zone, forming Nb-rich phases, low-melting-point terminal liquid films, or semi-continuous Nb-rich fragile paths, which can induce solidification hot cracks. These post-weld hot cracks may continue to propagate during subsequent cupping or approximately 70% cold rolling processes, becoming a significant source of risk for weld cracking or breakage.

[0012] Therefore, the core contradiction in laser filler wire welding of 430 ferritic stainless steel NiCr-3 lies in the fact that NiCr-3 is beneficial for improving plasticity, toughness and deformation coordination, but its Nb content brings the risk of Nb segregation and hot cracking under rapid solidification conditions. Existing technologies lack a control method that addresses this contradiction and unifies the welding material route, Nb input amount, wire drop point, molten pool disturbance and cold rolling adaptability evaluation.

[0013] In laser filler wire welding of 430 ferritic stainless steel NiCr-3, simply increasing or decreasing the laser heat input cannot simultaneously resolve the following contradictions: too low a heat input may lead to insufficient fusion and inadequate mixing, while too high a heat input may cause grain coarsening, decreased deformation coordination, or uncontrolled weld formation; simply reducing the wire feed rate can reduce Nb input, but may weaken the ductility and toughness advantages of NiCr-3 weld; simply adjusting the welding material can change the weld microstructure, but cannot actively break up the continuous Nb-rich pathways in the final solidification zone.

[0014] Therefore, a specialized method is needed that takes "using NiCr-3 to improve the ductility and toughness of the weld" as a premise, and simultaneously adjusts "Nb input amount, welding wire entry position into the molten pool, molten pool mixing state, and Nb-rich continuity at the solidification end". Summary of the Invention

[0015] The purpose of this invention is to provide a laser filler wire welding device and welding method for 430 ferritic stainless steel NiCr-3, in order to solve the problems of insufficient deformation coordination of 309 type welding materials under large deformation cold rolling conditions, the easy generation of Nb segregation and solidification hot cracks in NiCr-3 Nb-containing welding wire under rapid solidification conditions of laser welding, and the expansion of post-weld hot cracks in subsequent cold rolling leading to weld cracking or breakage.

[0016] The technical solution adopted by the present invention to achieve the above objectives is as follows:

[0017] A laser wire-filling welding device for 430 ferritic stainless steel NiCr-3 includes a laser welding head, a protective gas nozzle, a wire guide nozzle, and a vibration drive component. The laser welding head is positioned above the weld seam of the stainless steel base material to emit laser light. A protective gas nozzle is provided on one side of the laser irradiation end, and a wire guide nozzle is provided on the other side. The vibration drive component is fixed to the outside of the wire guide nozzle by a connecting clamp.

[0018] Furthermore, the vibration drive component adopts a mechanical eccentric vibrator, piezoelectric vibrator, electromagnetic vibrator or equivalent vibration source, and is installed at the end of the wire guide near the molten pool through a connecting clamp, so that the end of the welding wire will produce a slight lateral swing when vibrating.

[0019] A laser filler wire welding method for 430 ferritic stainless steel NiCr-3 includes the following steps:

[0020] S1. Place the 430 ferritic stainless steel strip base material to be welded under the laser welding head, and feed NiCr-3 welding wire through the wire guide nozzle. The Nb content of the welding wire is 2.0 wt.% to 3.0 wt.%.

[0021] S2. Set the laser power, welding speed, wire feed speed, defocusing amount, spot diameter and shielding gas parameters, and control the nominal line energy, wire feed volume per unit length, base metal dilution rate and nominal Nb content of weld to be within the preset window;

[0022] The parameters of the preset window are as follows: nominal line energy controlled between 0.25 and 0.45 kJ / mm, wire feed volume per unit weld length controlled between 1.40 and 2.05 mm³ / mm, base metal dilution rate controlled between 35% and 60%, and nominal Nb content of the weld controlled between 1.05 and 1.75 wt.%.

[0023] S3. Set the wire tilt angle, extension length and landing position so that the wire melts into the molten pool from the front edge to the middle, and avoids concentrated melting into the last solidification zone at the tail.

[0024] S4. Start the vibration drive to drive the wire guide tip to vibrate laterally, so that the end of the welding wire forms a medium-frequency small-amplitude lateral oscillation; the vibration frequency is 120 to 260 Hz, and the amplitude of the welding wire end is 0.06 to 0.14 mm.

[0025] S5. Perform laser filler wire welding to form a welded joint between NiCr-3 welding wire and 430 base material, which is mainly nickel-based weld and diluted by the base material.

[0026] S6. Perform PT, metallographic, BSE, EDS and hardness tests on the weld after welding, focusing on the weld centerline, crack path, interdendritic space and the final solidification zone.

[0027] S7. Determine whether the Nb segregation and hot cracking indicators meet the preset requirements; if not, proceed to process adjustment S8; if they meet the requirements, proceed to S9 to perform cupping or cold rolling verification on the sample.

[0028] The adjustment process S8 includes: when the centerline has a clear Nb-rich band, the PT shows abnormalities, or the risk of cold rolling cracking increases, the wire landing point is preferentially adjusted towards the leading edge of the molten pool, the wire feeding speed is reduced by 10% to 20%, the base material dilution rate is adjusted to 45% to 50%, or the vibration frequency is adjusted to 180 to 220 Hz and the end amplitude is adjusted to 0.08 to 0.12 mm; when the weld formation is unstable, the reinforcement height fluctuates, or spatter increases, the amplitude is reduced, the wire extension length is shortened, or the landing point is moved back from the leading edge to the front middle.

[0029] The S9 verification of the sample cupping or cold rolling is as follows: the cold rolling reduction can be three levels of verification: 30%, 50% and 70%, and the focus is on observing whether the crack extends along the weld centerline, the Nb-rich area or the existing hot crack.

[0030] S10. When the post-weld hot cracking, Nb segregation, and cold rolling cracking all meet the target range, the curing process window is set.

[0031] Furthermore, the diameter of the welding wire is 0.8 to 1.2 mm, preferably 0.9 mm.

[0032] Furthermore, the laser power is 8 to 14 kW, preferably 12 kW; the welding speed is 1.8 to 2.8 m / min, preferably 2.2 m / min; the wire feed speed is 5.0 to 7.0 m / min, preferably 6.5 m / min; the defocusing amount is -1.0 to +1.0 mm; and the spot diameter is 0.4 to 0.8 mm.

[0033] Furthermore, the parameters of the preset window are further preferably: nominal line energy controlled at 0.30 to 0.36 kJ / mm, wire feeding volume per unit weld length controlled at 1.55 to 1.90 mm3 / mm, and base material dilution rate controlled at 40% to 55%.

[0034] Furthermore, the welding wire tilt angle is preferably 15° to 30°; the welding wire extension length is 8 to 13 mm, preferably 8 to 10 mm; the welding wire deviates laterally from the weld centerline by no more than 0.20 mm, and the offset of the landing point relative to the center of the laser spot along the welding forward direction is -0.20 to +0.80 mm, preferably +0.20 to +0.60 mm.

[0035] Furthermore, the Nb segregation index target is 1.0 to 2.2.

[0036] The beneficial effects of this invention are:

[0037] This invention retains the advantages of NiCr-3 welding wire in improving the ductility, toughness, and deformation coordination of 430 ferritic stainless steel welds, while controlling the risk of Nb-rich segregation through Nb input, wire drop point, and wire vibration disturbance, thus avoiding simply replacing NiCr-3 with 309 or completely rejecting the NiCr-3 approach.

[0038] This invention controls the landing point of the welding wire to the front to the middle of the molten pool, so that the welding wire has a longer molten pool mixing time after melting. By using the medium-frequency small amplitude lateral vibration of the wire guide tip, the end of the welding wire is made to swing slightly and disturb the local molten pool. This can break the originally continuous or semi-continuous Nb-rich path into a point or short strip distribution, reducing the continuous Nb-rich path between the weld centerline and dendrites.

[0039] This invention reduces the risk of post-weld solidification hot cracking by reducing the Nb-rich low-melting-point terminal liquid film or the fragile path between continuous dendrites. After adopting the preferred process of this invention, no continuous linear appearance was observed in the PT, and no through-weld centerline cracking occurred after 70% cold rolling.

[0040] This invention does not judge quality solely by weld appearance, but establishes a closed loop between BSE, EDS spot scan, EDS, Nb segregation index, centerline segregation width, peak hardness, and cold rolling verification, thereby guiding process window iteration and serving as a basis for on-site quality evaluation.

[0041] The welding device of the present invention uses a wire guide nozzle or wire feeding tube near the vibration drive component, and achieves vibration drive through mechanical eccentricity, electromagnetic or piezoelectric vibration. It does not require a complex ultrasonic cavitation system. Its preferred vibration frequency and amplitude are within the range that can be easily achieved and detected by conventional mechanical systems, which is convenient for modification of existing laser wire filler welding equipment. Attached Figure Description

[0042] Figure 1 This is a schematic diagram of the structure of the laser filler wire welding device of the present invention;

[0043] In the diagram: 1. Laser welding head; 2. Shielding gas nozzle; 3. Wire guide nozzle; 4. Vibration drive component; 5. Stainless steel base material; 6. Laser; 7. NiCr-3 welding wire; 8. Connecting clamp.

[0044] Figure 2 This is a schematic flowchart of the welding method of the present invention;

[0045] Figure 3 This is a summary table of welding process results for Embodiment 1 of the present invention;

[0046] Figure 4 This is a summary table of the welding process verification results of Embodiment 2 of the present invention;

[0047] Figure 5 This is a block diagram of the overall technical roadmap of the present invention.

[0048] Figure 6 This is a schematic diagram of the evaluation of weld structure before the process improvement of this invention;

[0049] Figure 7 This is a schematic diagram illustrating the evaluation of weld structure after the process improvement of this invention. Detailed Implementation

[0050] The present invention will be further described below with reference to the embodiments and accompanying drawings:

[0051] A laser filler wire welding device for 430 ferritic stainless steel NiCr-3, such as Figure 1 As shown, the device includes a laser welding head 1, a protective gas nozzle 2, a wire guide nozzle 3, and a vibration drive component 4. The laser welding head 1 is positioned above the weld seam of the stainless steel base material 5 to emit a laser 6. A protective gas nozzle 2 is positioned on one side of the laser 6 irradiation end, and a wire guide nozzle 3 is positioned on the other side. The wire guide nozzle 3 is used to attach NiCr-3 welding wire 7. The vibration drive component 4 is fixed to the outside of the wire guide nozzle 3 by a connecting clamp 8. The vibration drive component 4 adopts a mechanical eccentric vibrator, a piezoelectric vibrator, an electromagnetic vibrator, or an equivalent vibration source. It is installed at the end of the wire guide nozzle 3 near the molten pool by the connecting clamp 8, and the end of the welding wire will produce a slight lateral swing during vibration.

[0052] This vibration method does not require strong ultrasonic cavitation or large-amplitude wire swing as necessary conditions. Instead, it uses medium-frequency small-amplitude mechanical wire vibrator to cause a small periodic change in the position of the welding wire melting in order to disturb the liquid phase flow in the final solidification zone without destroying the stability of the weld formation, and to break the continuous Nb-rich path into point-like, short strip-like or discontinuous distribution.

[0053] The welding method using the above-mentioned welding equipment, such as Figure 2 As shown, it includes the following steps:

[0054] S1. Confirmation of Base Material and Welding Material: Place the 3-8mm thick 430 ferritic stainless steel strip base material 5 to be welded below the laser welding head 1. Install NiCr-3 laser filler wire on the wire guide tip 3. The diameter of the welding wire is 0.8-1.2 mm, preferably 0.9 mm; the Nb content of the welding wire is 2.0wt.% to 3.0wt.%, preferably about 2.63wt.%.

[0055] S2. Set laser and wire feeding references: Set laser power, welding speed, wire feeding speed, defocusing amount, spot diameter and shielding gas parameters, and control nominal line energy, wire feeding volume per unit length, base metal dilution rate and nominal Nb content of weld within the preset window.

[0056] The parameters of the preset window are: nominal wire energy controlled between 0.25 and 0.45 kJ / mm, wire feed volume per unit weld length controlled between 1.40 and 2.05 mm³ / mm, base metal dilution rate controlled between 35% and 60%, and nominal Nb content of the weld controlled between 1.05 and 1.75 wt.%; more preferably: nominal wire energy controlled between 0.30 and 0.36 kJ / mm, wire feed volume per unit weld length controlled between 1.55 and 1.90 mm³ / mm, and base metal dilution rate controlled between 40% and 55%;

[0057] The laser power is 8 to 14 kW, preferably 12 kW; the welding speed is 1.8 to 2.8 m / min, preferably 2.2 m / min; the wire feed speed is 5.0 to 7.0 m / min, preferably 6.5 m / min; the defocusing amount is -1.0 to +1.0 mm, and the spot diameter is 0.4 to 0.8 mm.

[0058] S3. Set the wire landing point: Set the wire tilt angle, extension length and landing point position so that the wire melts into the molten pool from the front edge to the middle front and avoids concentrated melting into the last solidification zone at the tail.

[0059] The preferred angle of the welding wire is 15° to 30°; the extension length of the welding wire is 8 to 13 mm, preferably 8 to 10 mm; the lateral deviation of the welding wire from the center line of the weld is no more than 0.20 mm, and the offset of the point of impact of the welding wire relative to the center of the laser spot along the welding direction is -0.20 to +0.80 mm, preferably +0.20 to +0.60 mm.

[0060] S4. Start the transverse vibration of the wire guide tip: Start the vibration drive 4 to drive the wire guide tip 3 to vibrate laterally, so that the end of the welding wire forms a medium-frequency small amplitude transverse oscillation; the vibration frequency is 120 to 260 Hz, and the amplitude of the welding wire end is 0.06 to 0.14 mm.

[0061] S5. Perform laser filler wire welding to form a welded joint between NiCr-3 welding wire and 430 base material, which is mainly nickel-based weld and diluted by the base material.

[0062] S6. Post-weld crack and microstructure detection: Perform PT, metallographic, BSE, EDS and hardness tests on the weld after welding, focusing on the weld centerline, crack path, interdendritic space and the final solidification zone.

[0063] S7. Determine whether the Nb segregation and hot cracking indices meet the preset requirements; the target Nb segregation index is 1.2 to 2.2; if it does not meet the target, proceed to adjustment process S8; if it meets the target, proceed to S9 to perform cupping or cold rolling verification on the sample.

[0064] The adjustment process S8 includes: when the centerline has a clear Nb-rich band, the PT shows abnormalities, or the risk of cold rolling cracking increases, the wire landing point is preferentially adjusted towards the leading edge of the molten pool, the wire feeding speed is reduced by 10% to 20%, the base material dilution rate is adjusted to 45% to 50%, or the vibration frequency is adjusted to 180 to 220 Hz and the end amplitude is adjusted to 0.08 to 0.12 mm; when the weld formation is unstable, the reinforcement height fluctuates, or spatter increases, the amplitude is reduced, the wire extension length is shortened, or the landing point is moved back from the leading edge to the front middle.

[0065] The S9 verification of the sample cupping or cold rolling is as follows: the cold rolling reduction can be three levels of verification: 30%, 50% and 70%, and the focus is on observing whether the crack extends along the weld centerline, the Nb-rich area or the existing hot crack.

[0066] S10, Curing process window: When post-weld hot cracking, Nb segregation and cold rolling cracking all meet the target range, the curing process window is set.

[0067] The main calculation formulas include:

[0068] Nominal line energy Calculate using the following formula:

[0069] ;

[0070] Wire feed volume per unit weld length Calculate using the following formula:

[0071] ;

[0072] Nb input index per unit weld length Calculate using the following formula:

[0073] ;

[0074] parent material dilution rate Calculate using the following formula:

[0075] ;

[0076] nominal Nb content of weld Calculate using the following formula:

[0077] ;

[0078] Among them, when When expressed as a percentage, it should be converted to a decimal between 0 and 1 before calculation, such as NiCr-3 welding wire. Approximately 2.63 wt.%, 430 base material When the base metal dilution rate is 40%, 50%, and 55%, the nominal Nb content of the weld is approximately 1.58 wt.%, 1.32 wt.%, and 1.18 wt.%, respectively.

[0079] Nb segregation index Calculate using the following formula:

[0080] .

[0081] Example 1

[0082] A 5mm thick annealed and pickled 430 ferritic stainless steel plate was selected. NiCr-3 type nickel-based welding wire with a diameter of 0.9mm and an Nb content of approximately 2.63 wt.% was used. The laser power was set to 12kW, the welding speed to 2.2m / min, the defocusing amount to 0mm, the spot diameter to approximately 0.6mm, the shielding gas to be helium or an argon-helium mixture, the wire feed speed to 6.5m / min, the wire tilt angle to approximately 20°, and the wire extension length to approximately 10mm.

[0083] According to the above formula, the nominal line energy is about 0.327 kJ / mm, or about 327 J / mm; the wire feed volume per unit weld length is about 1.88 mm3 / mm; this process can form NiCr-3 nickel-based welds and improve the cupping deformation performance relative to 309 welds, but without coordinated control of fusion ratio, wire drop point, wire vibration and heat input, discontinuous hot cracks and Nb-rich bright white phases can still be observed at the weld centerline or between dendrites.

[0084] The results are as follows Figure 3 As shown in the table, while NiCr-3 welding wire is beneficial for improving the cold deformation compatibility of 430 welds, its Nb content can lead to interdendritic segregation and solidification hot cracking risks under rapid solidification conditions in laser welding. Therefore, subsequent embodiments, while retaining the advantages of NiCr-3 weld plasticity and toughness, synergistically optimize four dimensions: fusion ratio, wire landing point, medium-frequency small-amplitude vibrating wire, and heat input.

[0085] Example 2

[0086] Preferred process window: The base material is 430 ferritic stainless steel with a thickness of about 5 mm; the welding wire is NiCr-3 or ERNiCr-3 type welding wire with a diameter of 0.9 mm; the laser power is about 12.0 kW, the welding speed is about 2.2 m / min, and the line energy is about 327 J / mm; the wire feed speed is about 5.6 to 5.9 m / min; the base material dilution rate is about 47% to 53%; the welding wire landing point is located in the front middle of the molten pool, and x_f is about +0.30 to +0.60 mm; the transverse vibration frequency of the wire guide tip is about 200 Hz, and the actual amplitude of the welding wire end is about 0.10 mm.

[0087] The results are as follows Figure 4 The content of the table is shown in the middle.

[0088] This invention does not improve a single parameter, but rather transforms the weld from a state of "high Nb input and continuous centerline segregation" to a state of "nominal Nb reduction, Nb-rich phase discretization, and crack path interruption" through a combination of "controlling the fusion ratio to reduce the total Nb amount, moving the welding wire drop point forward to extend the mixing time, using medium-frequency small-amplitude vibrating wire to disperse the continuous Nb-rich path, and stabilizing the molten pool mixing and solidification through the heat input window".

[0089] Overall technical route as follows Figure 5 As shown, 430 ferritic stainless steel strip is laser-filled with NiCr-3 or ERNiCr-3 type welding wire to improve plasticity and toughness. The fusion ratio and wire feed amount control the nominal Nb content of the weld. The wire landing point is moved forward to increase the mixing time of Nb in the molten pool. The final solidification zone is disturbed by medium-frequency small amplitude wire vibration. The residence time of the molten pool and the solidification rate are controlled by the heat input window. The reverse correction process window is evaluated by BSE / EDS / crack density / cold rolling results.

[0090] After welding, visual inspection and PT testing are performed first to observe whether there are longitudinal linear cracks on the weld surface. Then, samples are taken from the weld centerline, fusion line and heat-affected zone for OM metallographic, SEM fracture observation, BSE backscattering observation and EDS spot scan, line scan and mapping. Recommended elements to be tested include Nb, Ni, Fe, Cr, Mn and Si. For cross-section testing, it is recommended to select at least one cross-section each from the head stable section, middle stable section and tail stable section along the weld length. At least three fields of view near the weld centerline should be counted for each cross-section.

[0091] The following indicators should be given priority when making judgments:

[0092] Whether there is a continuous BSE bright white phase near the weld centerline and crack; whether the Nb segregation index is not greater than 1.8, preferably not greater than 1.5; whether the width of the Nb-rich band in the centerline is not greater than 25 micrometers; whether there is no through-crack in the centerline after 70% cold rolling.

[0093] Weld microstructure evaluation, such as Figure 6 and Figure 7 As shown, the Nb segregation was 3.0% before adjustment, and recovered to about 0.87% after adjustment, indicating a significant improvement in Nb segregation.

Claims

1. A 430 ferritic stainless steel NiCr-3 laser wire feed welding apparatus characterized by: It includes a laser welding head, a protective gas nozzle, a wire guide nozzle, and a vibration drive. The laser welding head is set above the weld seam of the stainless steel base material to emit laser light. A protective gas nozzle is set on one side of the laser irradiation end, and a wire guide nozzle is set on the other side. The vibration drive is fixed to the outside of the wire guide nozzle by a connecting clamp.

2. The laser filler wire welding device for 430 ferritic stainless steel NiCr-3 according to claim 1, characterized in that: The vibration drive component adopts a mechanical eccentric vibrator, piezoelectric vibrator, electromagnetic vibrator or equivalent vibration source, and is installed at the end of the wire guide near the molten pool through a connecting clamp seat. When vibrating, it causes the end of the welding wire to oscillate slightly laterally.

3. A laser filler wire welding method for 430 ferritic stainless steel NiCr-3, characterized in that: Includes the following steps: S1. Place the 430 ferritic stainless steel strip base material to be welded under the laser welding head, and install NiCr-3 laser filler wire on the wire guide tip. The Nb content of the welding wire is 2.0 wt.% to 3.0 wt.%. S2. Set the laser power, welding speed, wire feed speed, defocusing amount, spot diameter, and shielding gas parameters, and control the nominal laser energy, wire feed volume per unit length, base metal dilution rate, and nominal Nb content of the weld to be within a preset window; the parameters of the preset window are: nominal laser energy controlled between 0.25 and 0.45 kJ / mm, wire feed volume per unit weld length controlled between 1.40 and 2.05 mm³ / mm, base metal dilution rate controlled between 35% and 60%, and nominal Nb content of the weld controlled between 1.05 and 1.75 wt.%. S3. Set the wire tilt angle, extension length and landing position so that the wire melts into the molten pool from the front edge to the middle, and avoids concentrated melting into the last solidification zone at the tail. S4. Start the vibration drive to drive the wire guide tip to vibrate laterally, so that the end of the welding wire forms a medium-frequency small-amplitude lateral oscillation; the vibration frequency is 120 to 260 Hz, and the amplitude of the welding wire end is 0.06 to 0.14 mm. S5. Perform laser filler wire welding to form a welded joint between NiCr-3 welding wire and 430 base material, which is mainly nickel-based weld and diluted by the base material. S6. Perform PT, metallographic, BSE, EDS and hardness tests on the weld after welding, focusing on the weld centerline, crack path, interdendritic space and the final solidification zone. S7. Determine whether the Nb segregation and hot cracking indices meet the preset requirements; If the standard is not met, proceed to process adjustment S8; If the standard is met, proceed to S9 for cupping or cold rolling verification of the sample; The adjustment process S8 includes: when the centerline has a clear Nb-rich band, the PT shows abnormalities, or the risk of cold rolling cracking increases, the wire landing point is preferentially adjusted towards the leading edge of the molten pool, the wire feeding speed is reduced by 10% to 20%, the base material dilution rate is adjusted to 45% to 50%, or the vibration frequency is adjusted to 180 to 220 Hz and the end amplitude is adjusted to 0.08 to 0.12 mm; when the weld formation is unstable, the reinforcement height fluctuates, or spatter increases, the amplitude is reduced, the wire extension length is shortened, or the landing point is moved back from the leading edge to the front middle. The S9 verification of the sample cupping or cold rolling is as follows: the cold rolling reduction can be three levels of verification: 30%, 50% and 70%, and the focus is on observing whether the crack extends along the weld centerline, the Nb-rich area or the existing hot crack. S10. When the post-weld hot cracking, Nb segregation, and cold rolling cracking all meet the target range, the curing process window is set.

4. The laser filler wire welding method for 430 ferritic stainless steel NiCr-3 according to claim 3, characterized in that: The diameter of the welding wire is 0.8 to 1.2 mm, preferably 0.9 mm.

5. The laser filler wire welding method for 430 ferritic stainless steel NiCr-3 according to claim 3, characterized in that: The laser power is 8 to 14 kW, preferably 12 kW; the welding speed is 1.8 to 2.8 m / min, preferably 2.2 m / min; the wire feed speed is 5.0 to 7.0 m / min, preferably 6.5 m / min; the defocusing amount is -1.0 to +1.0 mm; and the spot diameter is 0.4 to 0.8 mm.

6. The laser filler wire welding method for 430 ferritic stainless steel NiCr-3 according to claim 3, characterized in that: The parameters of the preset window are further preferably: nominal line energy is controlled at 0.30 to 0.36 kJ / mm, wire feeding volume per unit weld length is controlled at 1.55 to 1.90 mm3 / mm, and base material dilution rate is controlled at 40% to 55%.

7. The laser filler wire welding method for 430 ferritic stainless steel NiCr-3 according to claim 3, characterized in that: The preferred angle of the welding wire is 15° to 30°; the extension length of the welding wire is 8 to 13 mm, preferably 8 to 10 mm; the lateral deviation of the welding wire from the center line of the weld is no more than 0.20 mm, and the offset of the point of impact relative to the center of the laser spot along the welding direction is -0.20 to +0.80 mm, preferably +0.20 to +0.60 mm.

8. The laser filler wire welding method for 430 ferritic stainless steel NiCr-3 according to claim 3, characterized in that: The target Nb segregation index is 1.0 to 2.2.