A device and method for controlling the interface composition and flash of dissimilar metal inertial friction welding
By using TIG arc additive manufacturing and high-frequency ultrasonic vibration technology, the problems of flash waste and brittle phase formation in inertial friction welding of dissimilar metals have been solved, realizing material recycling and high-performance joints, simplifying the process and reducing costs.
Patent Information
- Application Number
- CN202611627907.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-21
- Publication Date
- 2026-11-17
AI Technical Summary
Dissimilar metal inertial friction welding suffers from problems such as flash removal disrupting flow lines and wasting materials, uneven plastic flow on both sides, formation of brittle intermetallic compound layers at the interface, microcracks and warping deformation caused by thermal stress and residual stress, and disconnect between welding and post-weld treatment, resulting in complex processes, high costs, and a lack of integrated collaborative control capabilities.
The TIG arc additive welding method is used to deposit metal, suppressing the formation of brittle intermetallic compounds. The flash is extruded using a V-groove and a metal-ceramic layer, and high-frequency ultrasonic vibration is introduced to achieve effective utilization of flash metal, integrated pre- and post-weld treatment, refinement of joint structure, and elimination of residual stress.
It enables the utilization of flash resources, inhibits the formation of brittle phases, eliminates residual stress, improves the fatigue resistance of joints, simplifies the device structure, reduces costs, and ensures high-precision positioning of weld seams.
Smart Images

Figure CN123103232A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of dissimilar metal joining manufacturing technology, and more particularly to a device and method for controlling the interface composition and flash of dissimilar metal inertial friction welding. Background Technology
[0002] With the rapid development of modern equipment manufacturing towards lightweight, high specific strength, and corrosion resistance, dissimilar metal connection structures are increasingly widely used in aerospace, shipbuilding and marine engineering, and rail transportation. Dissimilar metal connections achieve synergistic optimization of high strength, lightweight, corrosion resistance, heat resistance, and economy through the complementary properties of the materials. However, due to the significant differences in physical and chemical metallurgical properties between dissimilar metals, it is difficult to achieve high-quality connections using conventional fusion welding methods. The differences in melting point and thermal conductivity between dissimilar metals result in extremely uneven heat input distribution during fusion welding, easily leading to incomplete fusion or coarse grains in overheated areas. Furthermore, dissimilar metals have limited miscibility in the liquid state and are almost insoluble in the solid state, readily forming continuous intermetallic compound layers at the interface during welding cooling. These brittle phases have vastly different properties from the matrix, easily causing crack formation and being a major cause of joint fracture.
[0003] Currently, inertial friction welding (IFW), as a solid-state joining technology, is widely used for the butt welding of tubular components. This technology stores kinetic energy through a flywheel, generating intense frictional heat in a short time, placing the interface metals in a thermoplastic state, and then achieving connection through upsetting force. Although IFW effectively avoids the formation of a molten pool and reduces porosity defects, dissimilar metal IFW still faces the following significant technical bottlenecks: First, a large amount of flash is generated during IFW. The traditional method is to remove it by turning after the workpiece cools, which not only wastes expensive alloy materials but also increases the cost and cycle of subsequent machining. Furthermore, turning to remove flash can disrupt the original flow lines of the weld and potentially introduce microcrack sources. Second, the strength, plasticity, and thermal conductivity of dissimilar metals differ significantly, and the plastic flow behavior of the two metals differs significantly during welding, leading to significant differences in the radial extrusion of the two metals. Third, despite being a solid-state welding process, under the influence of high frictional temperature and plastic deformation, the dissimilar metals at the interface still undergo intense diffusion, forming a high concentration of brittle intermetallic compound phases. The brittle phase crystal structure is complex with many slip planes, making it difficult to release stress through plastic deformation under external force, which seriously reduces the impact toughness and fatigue life of the joint. Fourth, the linear expansion coefficients of dissimilar metals differ significantly. During the rapid cooling stage after friction welding, due to the inconsistent shrinkage rates, huge thermal stress is generated at the interface. The brittle intermetallic compound layer is sandwiched between two matrices with different deformation shrinkage and bears extremely high internal tensile stress, which can easily exceed its fracture strength and directly generate microcracks during the cooling process. Fifth, the huge thermal stress during welding can cause the joint to warp and deform, forming extremely high residual tensile stress at the fragile interface. The residual stress concentrates in the intermetallic compound layer, which can easily initiate microcracks and then rapidly propagate along the continuous intermetallic compound interface, eventually leading to the brittle and sudden fracture of the joint.
[0004] To address these issues, the industry has attempted transitions using methods such as adding intermediate layers or explosive welding, but these processes are complex and costly. Existing technologies often separate welding and post-weld treatment into two independent steps. This fragmented process fails to utilize the residual heat effect of the welding thermal cycle, resulting in low stress relief efficiency. Therefore, there is a pressing need to develop a novel composite manufacturing process and apparatus that integrates welding, forming, modification, and stress relief. Summary of the Invention
[0005] In view of the above-mentioned problems in existing heterogeneous metal inertial friction welding, such as flash removal disrupting flow lines and wasting materials, uneven plastic flow on both sides, formation of brittle intermetallic compound layers at the interface, microcracks and warping deformation caused by thermal stress and residual stress, and the disconnect between welding and post-weld treatment, complex process and high cost, and lack of integrated collaborative control capability, this paper provides a device and method for controlling the interface composition and flash of heterogeneous metal inertial friction welding.
[0006] This invention mainly utilizes TIG arc additive welding to deposit metal and suppress the formation of brittle intermetallic compounds. It uses TIG arc preheating, inertial friction welding to achieve solid-phase connection, and V-groove and metal-ceramic layer extrusion to accommodate flash. At the same time, high-frequency ultrasonic vibration is introduced to achieve effective utilization of flash metal, integrated pre-weld and post-weld treatment, refinement of joint structure, suppression of brittle phases, and elimination of residual stress.
[0007] The technical means employed in this invention are as follows: A device for controlling the interface composition and flash of dissimilar metals inertial friction welding, comprising: The frame and the power drive system, rotary clamping system, upsetting feed system and composite welding execution system arranged sequentially along the workpiece axis; The power drive system includes a servo motor, a drive shaft, a clutch, and a flywheel. The output end of the servo motor is connected to the drive shaft, the drive shaft is connected to the main shaft through the clutch, and the flywheel is fixedly mounted on the main shaft. The rotary clamping system includes a rotary chuck and a first clamping jaw disposed on the rotary chuck. The rotary chuck is fixedly connected to the spindle. A metal-ceramic layer is embedded at the front end of the first clamping jaw, and an annular groove is provided on the inner wall of the metal-ceramic layer. The upsetting feed system includes a movable worktable, a servo hydraulic cylinder, and a second clamping jaw disposed on the movable worktable. The output end of the servo hydraulic cylinder is connected to the movable worktable and is used to drive the movable worktable to move axially. The composite welding execution system includes a free-walking mechanism, a TIG welding torch, a wire feeder, and a high-frequency ultrasonic vibration device. The free-walking mechanism is mounted on the frame, the TIG welding torch is mounted on the free-walking mechanism, and the high-frequency ultrasonic vibration device is mounted on the movable worktable. Furthermore, the first clamping jaw integrates a temperature sensor and an annular induction heater. The temperature sensor is electrically connected to the annular induction heater and is used for closed-loop control of preheating and slow cooling of the workpiece. The second clamping jaw has an integrated stress measuring device for detecting the clamping force and upsetting force on the workpiece.
[0008] Furthermore, the upsetting feed system also includes a mandrel, one end of which is rotatably connected to the flywheel, and the other end of which passes sequentially through the hollow housing of the servo hydraulic cylinder and the movable worktable before being fixedly connected to the frame.
[0009] Furthermore, the TIG welding torch includes a welding torch body and an attitude adjustment assembly mounted on the welding torch body. The attitude adjustment assembly includes a vertical telescopic mechanism and a pivot hinge mechanism. The vertical telescopic mechanism is used to drive the welding torch body to extend and retract in the vertical direction, and the pivot hinge mechanism is used to drive the welding torch body to adjust the pitch angle around a pivot.
[0010] Furthermore, the amplitude transformer of the high-frequency ultrasonic vibration device is connected to an ultrasonic impact head at its end.
[0011] This invention also provides a method for controlling the interface composition and flash of dissimilar metal inertial friction welding, comprising the following steps: Step 1: Machin the mating end face of the rotating side workpiece into a bevel, keep the mating end face of the upsetting side workpiece flat, and assemble the two workpieces coaxially onto the mandrel; Step 2: The clutch engages, the servo motor drives the rotating workpiece to rotate, and the TIG welding torch performs arc additive manufacturing at the bevel of the rotating workpiece to form a deposited metal layer. Step 3: The clutch disengages, the flywheel drives the rotating side workpiece to rotate at high speed, the servo hydraulic cylinder pushes the upsetting side workpiece to move towards the rotating side workpiece for contact friction, and at the same time, the TIG welding torch preheats the upsetting side workpiece, and the resulting flash is squeezed and filled to the root of the bevel. Step 4: Turn on the high-frequency ultrasonic vibration device to input high-frequency mechanical vibration energy into the welding area.
[0012] Furthermore, the bevel is a double-sided V-shaped bevel with an angle of 30°-60°; In step three, the flash, guided by the metal-ceramic layer, is squeezed and filled into the root region of the double-sided V-shaped bevel.
[0013] Furthermore, in step two, the welding current is 50A-200A, the welding voltage is 5V-15V, the arc length is 1mm-4mm, the wire feed speed is 2mm / s-5mm / s, and a deposited metal layer with a thickness of 5mm-20mm is formed. In step three, the flywheel speed is 500rpm-3000rpm, the feed speed of the workpiece on the upsetting side is 5mm / s-50mm / s, the friction pressure is 20MPa-200MPa, and the upsetting pressure is 50MPa-400MPa.
[0014] Furthermore, the material of the rotating side workpiece is titanium alloy, the material of the upsetting side workpiece is steel, and the welding wire used in step two is one of copper-based welding wire, nickel-based welding wire, molybdenum-based welding wire, zirconium-based welding wire, silver-based welding wire, or high-entropy alloy welding wire.
[0015] Furthermore, in step four, the frequency of the high-frequency ultrasonic vibration device is 5kHz-50kHz, and the amplitude output range is 20μm-100μm.
[0016] Compared with the prior art, the present invention has the following advantages: 1. Resource utilization of flash. By designing the V-shaped bevel on the workpiece mating end face on the rotating side, the TIG arc preheating design, and the metal-ceramic layer to accommodate flash, the heat input distribution and metal flow are controlled. The originally harmful friction welding flash is used as filler material, realizing the recycling of materials, reducing machining allowance, and improving material utilization.
[0017] 2. Active suppression of brittle phases. By introducing active elements through arc additive manufacturing, compounds with better toughness are preferentially generated through metallurgical reactions. This fundamentally changes the chemical composition distribution at the interface, effectively suppressing the formation of binary brittle phases, blocking the formation of continuous brittle layers, and allowing them to be dispersed in the matrix.
[0018] 3. Stress relief mechanism. Preheating is achieved through a built-in heater and TIG arc, which reduces the temperature gradient of the thermal cycle and reduces thermal stress from the source. At the same time, high-frequency ultrasonic impact is used to introduce high-amplitude residual compressive stress immediately after welding to offset tensile stress and significantly improve the fatigue resistance of the joint.
[0019] 4. Simplified device structure and guaranteed coaxiality. Through the clutch switching mechanism, the workpiece can utilize the rotation function of the same spindle system in various modes such as arc additive manufacturing, inertial friction welding, and arc preheating. The arc welding torch only needs to perform linear motion, eliminating the need for complex ring guide rails, thus reducing equipment manufacturing costs. Furthermore, the workpiece is always clamped and rotated by the same spindle system, eliminating the need for secondary clamping or realignment, ensuring extremely high repeatability of weld position positioning, and truly realizing in-situ repair and modification. Attached Figure Description
[0020] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0021] Figure 1 This is a schematic front sectional view of the overall structure of the device of the present invention; Figure 2 for Figure 1 Enlarged view of a portion of the image; Figure 3 This is a schematic diagram of the overall structure of the device of the present invention at point A, viewed from the right. Figure 4This is a schematic diagram illustrating the principle of arc additive manufacturing. Figure 5 A schematic diagram illustrating the principles of inertial friction welding, arc preheating, and flash removal; Figure 6 This is a schematic diagram of the microstructure obtained by the apparatus and method of the present invention.
[0022] In the diagram: 1. Servo motor; 2. Drive shaft; 3. Spindle; 4. Clutch; 5. Rotary chuck; 6. Flywheel; 601. Top side metal atoms; 602. Rotating side metal atoms; 603. Clad metal atoms; 604. Tough phase; 605. Brittle phase; 7. Rotating side workpiece; 8. Pressure-sensing chuck; 9. First clamping jaw; 10. Free-moving mechanism; 11. TIG welding torch; 12. Metal-ceramic layer; 13. Temperature sensor; 14. Upsetting side workpiece; 15. Second clamping jaw; 16. Moving worktable; 17. First sliding bracket; 18. Servo hydraulic cylinder; 19. Second sliding bracket; 20. Control box; 21. High-frequency ultrasonic vibration device; 22. Pressure-sensing chuck; 23. Mandrel; 24. Double-sided V-groove; 25. Clad metal layer; 26. Flash. Detailed Implementation
[0023] It should be noted that, unless otherwise specified, the embodiments and features described in the present invention can be combined with each other. The present invention will now be described in detail with reference to the accompanying drawings and embodiments.
[0024] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. The following description of at least one exemplary embodiment is merely illustrative and is in no way intended to limit the present invention or its application or use. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0025] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the scope of exemplary embodiments according to the invention. As used herein, the singular form is intended to include the plural form as well, unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.
[0026] Unless otherwise specifically stated, the relative arrangement, numerical expressions, and values of the components and steps described in these embodiments do not limit the scope of the invention. It should also be understood that, for ease of description, the dimensions of the various parts shown in the drawings are not drawn to actual scale. Techniques, methods, and devices known to those skilled in the art may not be discussed in detail, but where appropriate, such techniques, methods, and devices should be considered part of the specification. In all examples shown and discussed herein, any specific values should be interpreted as merely exemplary and not as limitations. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters in the following figures denote similar items; therefore, once an item is defined in one figure, it need not be further discussed in subsequent figures.
[0027] Example 1: As Figures 1-3 As shown, the present invention provides a device for controlling the interface composition and flash of heterogeneous metal inertial friction welding, including a frame and a power drive system, a rotary clamping system, an upsetting feed system and a composite welding execution system arranged sequentially along the workpiece axis.
[0028] like Figure 1 The power drive system includes a servo motor 1, a drive shaft 2, a clutch 4, and a flywheel 6. The output end of the servo motor 1 is connected to the drive shaft 2, which is connected to the main shaft 3 via the clutch 4. The flywheel 6 is fixedly mounted on the main shaft 3. The clutch 4 is located between the drive shaft 2 and the main shaft 3 and is used to switch between motor drive mode and flywheel inertia mode. The coaxiality of the clutch 4 is ≤0.02mm. The selected servo motor 1 has a power of 15kW-30kW; the selected main shaft 3 has a diameter of 60mm-100mm, high rigidity, and a through-hole diameter of 20mm-30mm; the selected flywheel 6 has a diameter of 300mm-400mm, a thickness of 50mm-80mm, and is made of high-strength steel that has undergone tempering treatment. The flywheel 6 is equipped with an encoder, which is used to collect the real-time rotational speed of the flywheel 6.
[0029] like Figure 1 and Figure 2The rotary clamping system includes a rotary chuck 5 and a first clamping jaw 9 mounted on the rotary chuck 5. The outer diameter of the rotary chuck 5 is 150mm-250mm. The rotary chuck 5 is fixedly connected to the spindle 3. The clamping section of the first clamping jaw 9 has a contact area width of 20mm-30mm and a clamping surface curvature of R30mm. The front end of the first clamping jaw 9 is inlaid with a high-temperature resistant metal-ceramic layer 12. The inner wall of the metal-ceramic layer 12 is machined into an annular groove to accommodate flash 26. The groove width is 8mm-12mm and the groove depth is 3mm-5mm. The first clamping jaw 9 integrates a temperature sensor 13 and an annular induction heater. The temperature sensor 13 is electrically connected to the annular induction heater for closed-loop control of preheating and slow cooling of the workpiece.
[0030] like Figure 1 and Figure 3 The upsetting feed system includes a movable worktable 16, a servo hydraulic cylinder 18, and a second clamping jaw 15 mounted on the movable worktable 16. The output end of the servo hydraulic cylinder 18 is connected to the movable worktable 16 and is used to drive the movable worktable 16 to move axially. The maximum thrust of the servo hydraulic cylinder 18 is 500kN, and the maximum stroke is 100mm.
[0031] Temperature sensor 13, ring heating inductor and stress testing device are all integrated into control box 20 for monitoring and manual operation of preheating, cooling and welding processes.
[0032] The second clamping jaw 15 integrates a stress measuring device to detect the clamping force and upsetting force on the workpiece. The upsetting feed system also includes a mandrel 23, which passes through the inner hole of the workpiece to support the tube wall and prevent collapse during friction upsetting. One end of the mandrel 23 is rotatably connected to the flywheel 6, and the other end passes through the hollow housing of the servo hydraulic cylinder 18 and the movable worktable 16 before being fixedly connected to the frame. The single-sided clearance between the outer diameter of the mandrel 23 and the inner diameter of the workpiece is controlled between 0.1mm and 0.5mm to accommodate tubular workpieces of different specifications.
[0033] The upsetting feed system also includes a first sliding bracket 17, and the rotary clamping system also includes a second sliding bracket 19. The first sliding bracket 17 and the second sliding bracket 19 are both fixed and coaxial. The first sliding bracket 17 is slidably engaged with the movable worktable 16, and the second sliding bracket 19 is slidably engaged with the rotary chuck 5.
[0034] like Figure 1 , Figure 4 and Figure 5The composite welding execution system includes a free-travel mechanism 10, a TIG welding torch 11, a wire feeder, and a high-frequency ultrasonic vibration device 21. The free-travel mechanism 10 is mounted on the frame and has a stroke of 300mm to cover the welding path and clearance space, with a repeatability accuracy ≤ ±0.5mm. The TIG welding torch 11 is mounted on the free-travel mechanism 10. The nozzle diameter of the TIG welding torch 11 is 10mm-12mm, and the tungsten electrode extension length is 2mm-5mm. The TIG welding torch 11 includes a torch body and a posture adjustment assembly mounted on the torch body. The posture adjustment assembly includes a vertical telescopic mechanism and a pivot hinge mechanism. The vertical telescopic mechanism drives the torch body to extend and retract vertically, and the pivot hinge mechanism drives the torch body to adjust its pitch angle around a pivot. The wire feeder is used to feed welding wire to the welding area and can be copper-based, nickel-based, molybdenum-based, zirconium-based, silver-based, or high-entropy alloy welding wire. The device also includes a gas protection device for shielding gas, which is mounted on the TIG welder but its output is not connected to the TIG welder. A high-frequency ultrasonic vibration device 21 is mounted on the movable worktable 16, with an ultrasonic impact head connected to the end of its amplitude transformer. The amplitude transformer of the high-frequency ultrasonic vibration device 21 has a length of 120mm-180mm, and its impact head radius is 4mm-6mm.
[0035] During the electric arc additive manufacturing stage and the electric arc preheating stage, the clutch 4 is engaged, and the servo motor 1 drives the workpiece 7 on the rotating side to rotate through the transmission shaft 2 and the main shaft 3. The TIG welding torch 11 is positioned by the free travel mechanism 10. During the inertial friction welding stage, the clutch 4 is disengaged, and the flywheel 6 drives the workpiece to rotate by inertia.
[0036] An annular friction pad is provided on the outer mating end face of the rotating workpiece 7, and a metal-ceramic layer 12 is provided on the side surface of the pad facing the workpiece.
[0037] The device also includes a drive assembly for driving the rotating disk to rotate. The drive assembly is mounted on the base and its output end is connected to the rotating disk.
[0038] Example 2: This embodiment provides a method for controlling the interface composition and flash of dissimilar metal inertial friction welding, specifically including the following steps: Step 1, Workpiece preparation and assembly: The mating end face of the rotating side workpiece 7 is machined into a bevel, while the mating end face of the upsetting side workpiece 14 is kept flat. The selected dissimilar metal tube has an outer diameter of 50mm-80mm, a wall thickness of 3mm-7mm, and a single-side length of 150mm-200mm. The bevel is a double-sided V-shaped bevel 24 with an angle of 30°-60°. The two workpieces are coaxially assembled on the mandrel 23, with a 30mm-100mm upsetting gap reserved. This gap provides necessary space to accommodate the plastic flash 26 generated during the subsequent friction welding stage, ensuring that the flash 26 can fully fill the root of the bevel. The heater in the clamping jaws is activated to preheat the workpiece to 300℃-500℃ and hold for 10min-20min. The rotating side workpiece 7 has high plasticity, and the dissimilar metal can be titanium alloy and high-strength steel, titanium alloy and aluminum alloy, titanium alloy and copper alloy, titanium alloy and high-temperature alloy, aluminum alloy and high-strength steel, or copper alloy and high-strength steel.
[0039] Step 2, Arc Additive Manufacturing Stage: After the flywheel 6 accelerates to a rotating welding speed of 2-20 rpm, the clutch 4 engages, and the servo motor 1 drives the rotating workpiece 7 to rotate. The free-walking mechanism 10 starts, moving the TIG welding torch 11 to a position 2-4 mm from the bevel of the rotating workpiece 7. After adjusting the angle of the welding torch using the attitude adjustment component, the free-walking mechanism 10 stops. The welding current is set to 50A-200A, the welding voltage to 5V-15V, and the arc length to 1mm-4mm. The wire feeding mode is used to fill the welding wire, and the wire feeding speed is 2mm / s-5mm / s. A 5mm-20mm layer of fused metal 25 is deposited at the outer bevel of the rotating workpiece 7 using arc additive welding, alloying and preheating it. This step achieves interface alloying and toughening, providing a plastic transition layer for subsequent friction welding, and preheating the rotating workpiece 7 to eliminate local temperature differences on the workpiece surface, reduce thermal stress concentration, and provide a good thermal environment for subsequent inertial friction welding. The filler wire is one of the following: copper-based welding wire, nickel-based welding wire, molybdenum-based welding wire, zirconium-based welding wire, silver-based welding wire, or high-entropy alloy welding wire.
[0040] Step 3, Inertia Friction Welding Stage: After the flywheel 6 accelerates to the predetermined speed of 500rpm-3000rpm, the clutch 4 disengages, and the flywheel 6 drives the rotating workpiece 7 to rotate at high speed. The servo hydraulic cylinder 18 pushes the upsetting workpiece 14 to move towards the rotating workpiece 7 at a feed speed of 5mm / s-50mm / s to conduct contact friction, with the friction pressure set at 20MPa-200MPa. At the same time, the free-walking mechanism 10 is activated, moving the TIG welding torch 11 to the upsetting workpiece 14 and igniting the arc. The welding current is set to 50A-200A, the welding voltage to 4V-12V, and the arc length to 1mm-4mm to preheat the upsetting workpiece 14. Under the action of frictional heat and upsetting force, the interface metal softens and produces plastic flow. With the assistance and guidance of the metal-ceramic layer 12, the formed flash 26 is squeezed and filled into the root area of the double-sided V-groove 24. Through the transfer of cladding metal, the metal atoms 601 on the top side, 602 on the rotating side, and 603 on the cladding metal diffuse into each other to form the ductile phase 604, while the formation of the brittle phase 605 is suppressed and dispersed. After the flywheel 6 has exhausted its kinetic energy, the upsetting pressure is maintained at 50MPa-400MPa to complete the solid-phase connection.
[0041] Step 4, High-frequency ultrasound-assisted treatment stage: During inertial friction welding, the high-frequency ultrasonic vibration device 21 is activated. Ultrasonic waves are coupled into the molten pool and the solid heat-affected zone through the impact head, inputting high-frequency mechanical vibration energy. The frequency of the high-frequency ultrasonic vibration device 21 is 5kHz-50kHz, and the amplitude output range is 20μm-100μm. The acoustic flow effect is used to stir the molten pool and promote uniform diffusion of elements, the cavitation effect is used to break dendrites and refine grains, and the mechanical impact effect is used to introduce compressive stress to counteract the welding tensile stress.
[0042] Step 5, air cooling: After the TIG welding torch 11 is extinguished, the workpiece is air-cooled to room temperature.
[0043] Preferably, the base material is a titanium alloy and high-strength steel, wherein the titanium alloy tube serves as the rotating side workpiece 7, the high-strength steel tube serves as the upsetting side workpiece 14, and the filler wire is an aluminum bronze welding wire. The chemical composition of the welding wire, by weight percentage, includes: Al 7.5-8.5%, Fe ≤ 0.5%, Mn ≤ 1.0%, with the balance being Cu and unavoidable impurities. Al has a much stronger affinity for Ti than Fe. During arc additive manufacturing and inertial friction welding, Al preferentially reacts with Ti to form an AlCu2Ti ternary intermetallic compound, effectively consuming Ti atoms, blocking the formation of a continuous Ti-Fe brittle layer, and allowing it to be dispersed in the matrix.
[0044] Example 4: Taking the connection of a TC4 titanium alloy tube with an outer diameter of 60mm and a wall thickness of 5mm to a 304 stainless steel tube as an example, the specific steps are as follows: Step S1, Beveling: The butt end face of the titanium alloy tube is machined into a 60° double-sided V-shaped bevel 24 with a blunt edge of 10mm, which serves as the rotating side workpiece 7. The butt end face of the steel tube is kept flat, which serves as the upsetting side workpiece 14.
[0045] Step S2, Assembly: Fit the workpiece into the mandrel 23 and clamp it. Engage the clutch 4, and the servo motor 1 drives the workpiece to rotate at 2 rpm. Start the heater to preheat the interface area to 400℃ and hold for 15 minutes.
[0046] Step S3, Arc Additive Manufacturing: The free-moving mechanism 10 drives the TIG welding torch 11 to descend to the weld initiation point. Using the equipped attitude adjustment component, the distance between the welding torch nozzle and the workpiece surface is maintained at 2mm. The TIG welding torch 11 ignites the arc and feeds in the ER CuAl8 welding wire. The welding current is 130A, the welding voltage is 14V, the arc length is 3.5mm, and the wire feed speed is 3mm / s. The TIG welding torch 11 remains stationary or only makes slight axial linear oscillations, relying on the rotation of the workpiece to cover the entire circumference with the arc and molten pool.
[0047] Step S4, inertial friction welding: The flywheel accelerates to 2000 rpm, the clutch 4 disengages, cutting off the motor power, and the flywheel drives the main shaft 3 and the rotating workpiece 7 to rotate at high speed; simultaneously, the free-moving mechanism 10 moves the TIG welding torch 11 to the upsetting workpiece 14, maintaining a distance of 2 mm between the welding torch nozzle and the workpiece surface. After the free-moving mechanism 10 completes positioning, it stops moving, the TIG welding torch 11 is turned on, the welding current is set to 80A, the welding voltage to 10V, and the arc length to 3mm, preheating the upsetting workpiece 14; at the same time, the servo hydraulic cylinder 18 advances, the friction pressure is 30MPa, the upsetting pressure is 80MPa, the friction time is 5s, and the upsetting time is 10s. With the assistance of the metal-ceramic layer, the flash 26 completely fills the root of the V-shaped bevel of the rotating workpiece 7.
[0048] Step S5, Ultrasonic Assistance and Air Cooling: The high-frequency ultrasonic vibration device 21 impacts a point 10mm behind the weld at a frequency of 20kHz and an amplitude of 70μm. After welding, the weld is air-cooled to room temperature.
[0049] Example 5: Three sets of comparative experiments were set up to verify the effectiveness of the present invention.
[0050] Control group 1 was conventional inertial friction welding, without electric arc additive manufacturing or ultrasonic assistance. A continuous TiFe brittle layer existed at the interface, and the joint fractured at the interface during the bending test.
[0051] Control group 2 consisted of inertial friction welding with traditional TIG capping, without ultrasonic assistance, and filled with pure copper welding wire. Although it blocked part of the Ti-Fe reaction, the microstructure was coarse and contained micropores.
[0052] The experimental group used the method of the present invention to form dispersed AlCu2Ti particles at the interface, without a continuous Ti-Fe brittle intermetallic compound layer. The tensile strength and elongation after fracture of the joint can be improved, and the residual compressive stress on the surface can also be reduced.
[0053] like Figure 4 , Figure 5 and Figure 6 The working principle of the device and method of the present invention is as follows: Through the switching mechanism of clutch 4, the workpiece can utilize the rotation function of the same spindle system in various modes such as arc additive manufacturing, inertial friction welding, and arc preheating. The arc welding gun only needs to perform linear motion, eliminating the need for complex ring guide rails, which reduces equipment manufacturing costs. Furthermore, the workpiece is always clamped and rotated by the same spindle system, eliminating the need for secondary clamping or realignment, ensuring extremely high repeatability of weld position and truly realizing in-situ repair and modification.
[0054] In the arc additive manufacturing stage, a fused metal layer 25 is deposited on the V-groove of the rotating workpiece 7 using a TIG welding torch 11. By introducing active elements through arc additive manufacturing, compounds with good toughness are preferentially generated through metallurgical reactions, fundamentally changing the chemical composition distribution of the interface, achieving interface alloying and toughening, providing a plastic transition layer for subsequent friction welding, and simultaneously achieving a preheating function, reducing the temperature gradient of the thermal cycle, and reducing thermal stress from the source.
[0055] During the inertial friction welding stage, the heat input distribution and metal flow are regulated by the V-groove design of the rotating workpiece 7's mating end face, the TIG arc preheating design, and the design of the cermet layer 12 to accommodate the flash 26. With the assistance of the cermet layer 12, the flash 26 is squeezed and filled to the root of the V-groove, using the originally harmful friction welding flash 26 as filler material, realizing the resource utilization of flash 26, reducing machining allowance, and improving material utilization. Through the transfer of deposited metal, the formation of binary brittle phases is effectively suppressed, the formation of continuous brittle layers is blocked, and they are dispersed in the matrix.
[0056] In the high-frequency ultrasonic-assisted treatment stage, the molten pool is stirred by ultrasonic waves and compressive stress is introduced. High-amplitude residual compressive stress is introduced immediately after welding by high-frequency ultrasonic impact to offset tensile stress, thereby refining the joint structure, suppressing brittle phases and eliminating residual stress, and significantly improving the fatigue resistance of the joint.
[0057] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A dissimilar metal inertia friction welding interface composition and flash regulating device, characterized in that, include: The frame and the power drive system, rotary clamping system, upsetting feed system and composite welding execution system arranged sequentially along the workpiece axis; The power drive system includes a servo motor (1), a drive shaft (2), a clutch (4) and a flywheel (6). The output end of the servo motor (1) is connected to the drive shaft (2). The drive shaft (2) is connected to the main shaft (3) through the clutch (4). The flywheel (6) is fixedly mounted on the main shaft (3). The rotary clamping system includes a rotary chuck (5) and a first clamping jaw (9) disposed on the rotary chuck (5). The rotary chuck (5) is fixedly connected to the spindle (3). The front end of the first clamping jaw (9) is inlaid with a metal ceramic layer (12), and the inner wall of the metal ceramic layer (12) is provided with an annular groove. The upsetting feed system includes a movable worktable (16), a servo hydraulic cylinder (18), and a second clamping jaw (15) disposed on the movable worktable (16). The output end of the servo hydraulic cylinder (18) is connected to the movable worktable (16) and is used to drive the movable worktable (16) to move axially. The composite welding execution system includes a free-walking mechanism (10), a TIG welding torch (11), a wire feeder, and a high-frequency ultrasonic vibration device (21). The free-walking mechanism (10) is mounted on the frame, the TIG welding torch (11) is mounted on the free-walking mechanism (10), and the high-frequency ultrasonic vibration device (21) is mounted on the mobile worktable (16).
2. The dissimilar metal inertia friction welding interface composition and flash regulating device of claim 1, wherein, The first clamping jaw (9) integrates a temperature sensor (13) and an annular induction heater. The temperature sensor (13) is electrically connected to the annular induction heater and is used for closed-loop control of preheating and slow cooling of the workpiece. The second clamping jaw (15) has an integrated stress measuring device for detecting the clamping force and upsetting force on the workpiece.
3. The dissimilar metal inertia friction welding interface composition and flash regulating device of claim 1, wherein, The top forging feed system also includes a mandrel (23), one end of which is rotatably connected to the flywheel (6), and the other end of which passes through the hollow housing of the servo hydraulic cylinder (18) and the movable worktable (16) in sequence and is fixedly connected to the frame.
4. The dissimilar metal inertia friction welding interface composition and flash regulating device of claim 1, wherein, The TIG welding torch (11) includes a welding torch body and an attitude adjustment assembly mounted on the welding torch body. The attitude adjustment assembly includes a vertical telescopic mechanism and a pivot hinge mechanism. The vertical telescopic mechanism is used to drive the welding torch body to extend and retract in the vertical direction, and the pivot hinge mechanism is used to drive the welding torch body to adjust the pitch angle around the pivot.
5. The dissimilar metal inertia friction welding interface composition and flash management apparatus of claim 1, wherein, The high-frequency ultrasonic vibration device (21) has an ultrasonic impact head connected to the end of the amplitude rod.
6. A method for regulating the interface composition and flash of dissimilar metal inertia friction welding, characterized in that, The method based on the heterogeneous metal inertial friction welding interface composition and flash control device according to claim 3 includes the following steps: Step 1: The mating end face of the rotating side workpiece (7) is machined into a bevel, the mating end face of the upsetting side workpiece (14) is kept flat, and the two workpieces are coaxially assembled on the mandrel (23). Step 2: The clutch (4) engages, the servo motor (1) drives the rotating side workpiece (7) to rotate, and the TIG welding gun (11) performs arc additive manufacturing at the bevel of the rotating side workpiece (7) to form a deposited metal layer (25). Step 3: The clutch (4) disengages, the flywheel (6) drives the rotating side workpiece (7) to rotate at high speed, the servo hydraulic cylinder (18) pushes the upsetting side workpiece (14) to move towards the rotating side workpiece (7) for contact friction, and at the same time, the TIG welding torch (11) preheats the upsetting side workpiece (14), and the resulting flash (26) is squeezed and filled to the root of the bevel; Step 4: Turn on the high-frequency ultrasonic vibration device (21) to input high-frequency mechanical vibration energy into the welding area.
7. The method for controlling the interface composition and flash of dissimilar metal inertial friction welding according to claim 6, characterized in that, The bevel is a double-sided V-shaped bevel (24) with an angle of 30°-60°; In step three, the flash (26) is guided by the metal ceramic layer (12) and squeezed into the root area of the double-sided V-shaped bevel (24).
8. The method for controlling the interface composition and flash of dissimilar metal inertial friction welding according to claim 6, characterized in that, In step two, the welding current is 50A-200A, the welding voltage is 5V-15V, the arc length is 1mm-4mm, the wire feed speed is 2mm / s-5mm / s, and a molten metal layer with a thickness of 5mm-20mm is formed (25). In step three, the rotational speed of the flywheel (6) is 500rpm-3000rpm, the pushing speed of the upsetting side workpiece (14) is 5mm / s-50mm / s, the friction pressure is 20MPa-200MPa, and the upsetting pressure is 50MPa-400MPa.
9. The method for controlling the interface composition and flash of dissimilar metal inertial friction welding according to claim 6, characterized in that, The rotating side workpiece (7) is made of titanium alloy, the upsetting side workpiece (14) is made of steel, and the filler wire in step two is one of copper-based welding wire, nickel-based welding wire, molybdenum-based welding wire, zirconium-based welding wire, silver-based welding wire, or high-entropy alloy welding wire.
10. The method for controlling the interface composition and flash of dissimilar metal inertial friction welding according to claim 6, characterized in that, In step four, the frequency of the high-frequency ultrasonic vibration device (21) is 5kHz-50kHz, and the amplitude output range is 20μm-100μm.