A quick-dissolving sheet-shaped dry sand mortar based on gradient wetting regulation and a preparation process thereof

By constructing a gradient pore structure and setting a wetting control layer inside the sheet-like dry mortar, the problems of dust pollution, component separation and low construction efficiency in the existing technology are solved, achieving rapid disintegration and uniform dispersion, and improving construction efficiency and material stability.

CN123104174APending Publication Date: 2026-11-17绍兴职业技术学院
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611274704.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing sheet-like dry mortar has problems such as dust pollution, component separation and segregation, low construction efficiency and low internal porosity during construction, making it difficult to achieve rapid disintegration and uniform dispersion.

Method used

The preparation process employs a gradient wetting control method, which constructs a gradient pore structure inside the sheet-like dry mortar, combined with a wetting control layer of hydrophilic polymer and disintegrant, to achieve rapid water absorption and disintegration. At the same time, a support structure is used to improve mechanical strength.

Benefits of technology

It enables rapid melting and uniform dispersion of sheet-like dry mortar, improving construction efficiency and material stability, and ensuring mechanical strength during transportation and construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123104174A_ABST
    Figure CN123104174A_ABST
Patent Text Reader

Abstract

The application relates to a quick-dissolving sheet-shaped dry mortar based on gradient wetting regulation and a preparation process thereof. The mortar comprises a mortar matrix, a support body and a wetting regulation layer; the mortar matrix has a gradient distribution of pore structures inside; the average porosity of a first pore area of the pore structures is greater than that of a second pore area; the wetting regulation layer is arranged on the upper surface of the mortar matrix and comprises a hydrophilic polymer and a disintegrating agent; the support body is arranged at the lower part of the mortar matrix and is used for improving the overall strength of the sheet body; by constructing the gradient pore structure, the flow guide structure and the wetting regulation layer, the rapid penetration and uniform diffusion of water in the sheet-shaped mortar are realized, the water dissolving speed and the construction efficiency of the sheet-shaped dry mortar are improved, dust pollution is reduced, and the component segregation problem is improved. The application also discloses a corresponding preparation process, and the sheet-shaped dry mortar is rapidly prepared and the performance is regulated through the steps of gradient material laying, sheet forming and gradient temperature drying.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of building materials, and in particular to a quick-dissolving sheet-like dry mortar based on gradient wetting control and its preparation process. Background Technology

[0002] Dry-mixed mortar is a dry, powdery building material formed by mixing inorganic cementitious materials, fine aggregates, mineral admixtures, and functional additives in a predetermined ratio. It only requires the addition of a suitable amount of water for mixing before application. Common inorganic cementitious materials include cement, gypsum, and lime; aggregates are typically natural sand, manufactured sand, or lightweight fillers; and functional additives include water-retaining agents, water-reducing agents, thickeners, retarders, and fiber materials. Compared to traditional on-site manual mixing of mortar, dry-mixed mortar offers advantages such as precise proportioning, stable quality, high construction efficiency, and suitability for mechanized production and transportation. Therefore, it is widely used in various fields including masonry mortar, plastering mortar, self-leveling mortar, waterproof mortar, thermal insulation mortar, and decorative mortar. With the development of industrialized construction and green construction concepts, dry-mixed mortar has become one of the most widely used building materials in modern construction projects.

[0003] However, existing dry-mixed mortars still face numerous problems in practical applications. Firstly, traditional dry-mixed mortars are typically packaged, transported, and stored as discrete powder particles. On-site operations such as opening bags, pouring, and adding water for mixing require these steps. During these processes, large amounts of fine dust easily disperse into the air, causing severe dust pollution. This problem is particularly pronounced in high-rise buildings, interior decoration, and large-scale mechanized construction environments. Airborne dust not only affects the hygiene of the construction site but also harms the respiratory system and health of construction workers. Furthermore, the escape of dust can easily pollute the surrounding environment, increasing the difficulty of environmental management at construction sites and failing to meet the current requirements for green construction and low-carbon environmental protection.

[0004] Secondly, due to the differences in particle size, density, and morphology among the components in dry-mixed mortar, segregation is prone to occur during transportation, loading and unloading, and storage. Denser sand particles tend to settle, while lighter additives, fibers, and powders tend to float, resulting in changes in the proportion of material components in different parts. This segregation directly affects the uniformity and stability of the mortar, causing problems such as inconsistent fluidity, fluctuating water retention, unstable setting time, and decreased bond strength during construction, thus affecting construction quality and later performance. In addition, leakage and moisture absorption are common during transportation, leading to material loss and making long-term storage and management difficult.

[0005] To address the aforementioned issues, existing technologies have gradually developed solutions for preparing dry-mixed mortar into sheet-like structures. By pressing the originally discrete granular mortar into sheets with a certain shape and strength, powder diffusion can be effectively reduced, dust pollution can be decreased, and the problem of component separation and segregation can be alleviated, thereby improving the overall stability of the product. Sheet-like dry mortar can be directly immersed in water during use, and through disintegration and melting, it can reform into workable mortar, thus showing promising application prospects.

[0006] Currently, a common process for preparing sheet-like dry mortar is the hot-melt method. This method typically involves adding a certain proportion of water-soluble hot-melt adhesive powder to dry-mixed mortar raw materials, forming a homogeneous mixture through mechanical stirring, then heating the mixture to melt the water-soluble hot-melt adhesive and coat the surface of the mortar particles. The mixture is then pressed into shape using a mold, and finally cooled and solidified to form a sheet-like structure. The adhesive effect of the cooled hot-melt adhesive allows various mortar particles to bond firmly, resulting in a sheet-like dry mortar product with a certain mechanical strength.

[0007] The above-mentioned hot melt preparation process still has many defects. In order to ensure that the sheet mortar has sufficient overall strength and anti-crushing ability, a large proportion of water-soluble hot melt adhesive is usually required. The addition of a large amount of hot melt adhesive increases the production cost of the product, and it is easy to form a continuous and relatively dense bonding layer inside the sheet, which reduces the porosity of the sheet mortar. Water is difficult to penetrate into the sheet quickly, resulting in a slow disintegration and melting speed of the sheet after it comes into contact with water. A long mixing time is required during construction, which affects the construction efficiency. Currently, there are relatively few types of water-soluble hot melt adhesives available for use in building materials. Most hot melt adhesives have high melting temperatures, typically requiring heating above 100°C. Inorganic cementitious materials like cement are highly sensitive to temperature; when heated above 100°C, they are prone to false setting. False setting refers to the phenomenon where cement abnormally thickens and loses its fluidity within a short period. Although fluidity can be restored by re-stirring in some cases, the normal hydration process has already been affected, leading to a decline in the later strength development and workability of the mortar. Therefore, in the hot melt preparation process, high-temperature heating can easily adversely affect cement properties, and in severe cases, even affect the overall quality stability of sheet mortar. Because hot melt adhesives tend to form a relatively continuous organic coating layer after cooling and solidification, the sheet structure lacks effective water-conducting channels, resulting in slow water penetration and difficulty in rapid disintegration. Furthermore, a high proportion of organic hot melt adhesives may also affect the later mechanical properties and durability of the mortar, which is detrimental to the long-term application of the product.

[0008] Besides the hot-melt method, there is another type of sheet-like dry mortar preparation method in the existing technology, namely the solution bonding method. This method usually involves first dissolving a water-soluble binder in water or an organic solvent to form a glue solution, then mixing the glue solution with dry-mix mortar raw materials to form a wet mixture, and then preparing sheet-like mortar through processes such as pressing, drying and hardening. Compared with the hot-melt method, this method can avoid the high-temperature heating process, thereby reducing the risk of false setting of cement, and also broadening the range of water-soluble binders to be selected. This type of solution also has certain limitations. Because wet-mixed materials tend to form a relatively dense internal structure during the pressing and drying process, the porosity inside the sheet is usually low. Water mainly enters the sheet through natural infiltration, lacking an effective and rapid water conduction path, resulting in a slow overall dissolution rate of the sheet mortar. In addition, most existing technologies only focus on the sheet forming strength, lacking coordinated control of the internal pore structure and wetting performance. After water enters the sheet, it is difficult to spread quickly and evenly, which can easily lead to local dissolution on the surface while the interior remains dense, thus prolonging the overall disintegration time and affecting construction efficiency.

[0009] Regarding the aforementioned technologies, the inventors believe that how to improve the water absorption rate, water conductivity, and overall disintegration efficiency of sheet mortar by optimizing its internal pore structure and wetting properties, while ensuring sufficient mechanical strength and transport stability, to achieve rapid dissolution and uniform dispersion, has become an important technical problem that urgently needs to be solved by those skilled in the art. Summary of the Invention

[0010] To address the technical challenge of achieving rapid dissolution and uniform dispersion of sheet-like dry mortar while maintaining sufficient mechanical strength and transport stability, this application provides a fast-dissolving sheet-like dry mortar based on gradient wetting control and its preparation process.

[0011] Firstly, the fast-dissolving flaky dry mortar based on gradient wetting control provided in this application adopts the following technical solution: A quick-dissolving sheet-like dry mortar based on gradient wetting control includes a mortar matrix, a support body, and a wetting control layer; The mortar matrix is ​​obtained by pressing and drying semi-dry particles reinforced with particles. The mortar matrix 1 has a gradient-distributed pore structure inside. The pore structure includes a first pore region and a second pore region. The average porosity of the first pore region is greater than the average porosity of the second pore region. The first pore region is located on one side of the upper surface of the mortar matrix, and the second pore region is located on one side of the lower surface of the mortar matrix. The support is disposed on the lower surface of the mortar matrix or embedded in the lower part of the mortar matrix; The wetting control layer is disposed on the upper surface of the mortar matrix, and the wetting control layer comprises a hydrophilic polymer and a disintegrant.

[0012] By adopting the above technical solution, the gradient distribution of the pore structure allows water to quickly penetrate into the interior of the sheet from the high porosity region and gradually diffuse to the low porosity region, thereby improving the water absorption rate and overall dissolution efficiency of the sheet dry mortar. At the same time, the hydrophilic polymer and disintegrant in the wetting control layer work synergistically to further enhance the surface wetting performance and promote the rapid disintegration of the sheet. The support structure is used to improve the overall strength and damage resistance of the sheet structure, making the sheet dry mortar less prone to breakage during transportation, storage and construction, effectively balancing mechanical strength and rapid dissolution performance.

[0013] Optionally, the average porosity of the first pore region is 25%-45%, and the average porosity of the second pore region is 10%-25%.

[0014] By adopting the above technical solution, a significant porosity gradient structure is formed inside the sheet-like dry mortar, which can not only improve the water penetration and diffusion rate and promote the rapid dissolution of the sheet, but also ensure that the underlying structure has sufficient strength and improve the stability of the sheet.

[0015] Optionally, the lower surface of the mortar matrix is ​​provided with a plurality of spaced-apart flow-guiding grooves, the flow-guiding grooves extending along a first direction, and flow-guiding ridges forming between adjacent flow-guiding grooves.

[0016] By adopting the above technical solution, a water-guiding channel can be formed at the bottom of the sheet-like dry mortar, increasing the water contact area and accelerating the water flow diffusion speed, thereby improving the internal wetting efficiency of the sheet and the overall dissolution speed.

[0017] Optionally, the particle size of the particle-reinforced semi-dry particles is 0.85mm-4.75mm; The particle-reinforced semi-dry particles comprise the following raw materials in parts by weight: 15-70 parts inorganic cementitious material, 15-85 parts aggregate, 0-25 parts admixture, 0.5-5 parts water-soluble binder, and 0.5-8 parts pore-forming agent.

[0018] By adopting the above technical solution, semi-dry granules can have both good tableting performance and internal pore formation ability, which can improve water absorption disintegration efficiency and overall dissolution speed while ensuring tablet strength.

[0019] Optionally, the pore-forming agent is at least one of ammonium bicarbonate, ammonium carbonate, urea, and azodicarbonamide. The pore-forming agent decomposes to generate gas during the drying and hardening process to form the gradient-distributed pore structure.

[0020] By adopting the above technical solution, the pore-forming agent can be heated and decomposed to release gas during the drying and hardening process of the particles, thereby forming a uniform pore structure with gradient distribution characteristics inside the particles. This not only helps to reduce the overall density of the material and improve its lightweight performance, but also enhances the water absorption, water retention and interfacial bonding ability of the particles. At the same time, it improves the air permeability and workability of the mortar, and further enhances the crack resistance and comprehensive performance of the molded material.

[0021] Optionally, the weight ratio of the hydrophilic polymer to the disintegrant in the wetting control layer 3 is 1:0.5-1:3; The hydrophilic polymer is at least one of polyvinyl alcohol, polyethylene glycol, and hydroxypropyl methylcellulose; The disintegrant is at least one of sodium carboxymethyl starch, crospovidone, and low-substituted hydroxypropyl cellulose.

[0022] By adopting the above technical solution and controlling the ratio between the hydrophilic polymer and the disintegrant, the wetting control layer can quickly absorb water and wet itself after contact with moisture, and can also disintegrate appropriately to form interconnected channels, thereby improving the overall material's water absorption and diffusion efficiency and water transport capacity. At the same time, the hydrophilic polymer can enhance structural stability and adhesion performance, while the disintegrant promotes the rapid opening of the internal structure. The synergistic effect of the two is beneficial to improving the material's wetting uniformity, solubility and dispersibility, and construction and application performance.

[0023] Optionally, the support 2 is a mesh structure, which includes a first braided filament extending in a first direction and a second braided filament extending in a second direction. The diameter of the first braided filament is larger than that of the second braided filament, so that the rigidity of the mesh structure in the first direction is greater than its rigidity in the second direction. The flow-guiding groove extends along the first direction.

[0024] By adopting the above technical solution, the support body uses a mesh structure formed by the interlacing of the first and second braided filaments, and the rigidity in the first direction is higher than that in the second direction due to the difference in wire diameter. This enables the anisotropic mechanical properties of the structure to be controlled in different directions, so that the overall support body has sufficient load-bearing stability and maintains a certain degree of flexibility and deformation adaptability in a specific direction. The flow-guiding groove extends along the first direction with higher rigidity, which is conducive to directional constraint and guidance of the fluid flow path, improving the continuity and stability of fluid transportation, reducing lateral diffusion and energy loss, and improving the overall flow-guiding efficiency and structural collaborative performance.

[0025] In a second aspect, a preparation process for a quick-dissolving flaky dry mortar based on gradient wetting control as described in any one of claims 1-7 includes the following steps: Step S1: Preparation of particle-reinforced semi-dry granules: Inorganic cementitious materials, aggregates, admixtures, water-soluble binders, and pore-forming agents are mixed evenly to form a dry mixture. The dry mixture is then mixed with a solvent to obtain a wet mixture. The wet mixture is granulated to obtain wet granules. The wet granules are then dried to obtain semi-dry granules. The particle size of the semi-dry granules is controlled to be 0.85mm-4.75mm, and the weight percentage of residual solvent in the semi-dry granules is 1%-8%. Step S2: Gradient spreading: The semi-dry particles obtained in step S1 are divided into a first particle group and a second particle group, wherein the average particle size of the first particle group is greater than the average particle size of the second particle group. The first particle group is first spread on the support 2 to form a first particle layer, and then the second particle group is spread on the first particle layer to form a second particle layer. Step S3: Tableting: The support 2, on which the first particle layer and the second particle layer were laid in step S2, is compressed to obtain a wet tablet. Step S4: Gradient drying and hardening: The wet sheet obtained in step S3 is subjected to gradient temperature drying, which causes the pore-forming agent to decompose and generate gas to form a gradient pore structure, while removing the solvent to obtain sheet-like dry mortar matrix 1. Step S5: Set a wetting control layer: Set a wetting control layer 3 on the upper surface of the sheet-like dry mortar matrix 1 obtained in step S4. The wetting control layer 3 is obtained by spraying or roller coating a mixed solution of hydrophilic polymer and disintegrant onto the upper surface and drying it.

[0026] By adopting the above technical solution, the preparation process achieves graded and controllable construction of the internal structure and surface properties of the sheet-like dry mortar through a multi-step collaborative design of "granulation-gradient spreading-tableting-gradient drying-surface control". In the particle preparation stage, the uniformity of particle formation and subsequent reaction activity are improved by controlling the particle size and residual solvent content. In the gradient spreading and tableting process, an orderly distribution structure of coarse and fine particles is formed, thereby improving the density and structural stability. In the gradient drying and hardening stage, the gas generated by the decomposition of the pore-forming agent is used to construct a gradient pore network, achieving a balance between lightweight and rapid dissolution performance. Finally, by setting a wetting control layer, the contact behavior between the material and water is significantly improved, the wetting diffusion rate and overall dissolution efficiency are increased, and the overall technical effect of rapid dissolution, high-efficiency construction adaptability and synergistic optimization of mechanical and construction performance is achieved.

[0027] Optionally, the gradient temperature drying in step S4 includes: first drying at a low temperature of 40℃-60℃ for 5-15 minutes to allow the pore-forming agent to be evenly distributed and begin to decompose; Then dry at a medium temperature of 70℃-90℃ for 15-30 minutes to completely decompose the pore-forming agent and form pores inside the tablet. Finally, dry at a constant temperature of 50℃-70℃ for 10-20 minutes to remove residual solvent.

[0028] By adopting the above technical solution, the phased gradient temperature drying allows the pore-forming agent to gradually decompose and stably release gas in different temperature ranges, forming a uniform and controllable pore structure, while avoiding structural collapse or uneven pores caused by rapid heating; the constant temperature drying step further removes residual solvents, ensuring the drying consistency inside the sheet and improving the structural stability and dissolution performance of the sheet-like dry mortar.

[0029] Optionally, in step S2, the average particle size of the first particle group is 2.0mm-4.75mm, the average particle size of the second particle group is 0.85mm-1.8mm, and the ratio of the thickness of the first particle layer to the thickness of the second particle layer is 1:0.5-1:2. The tableting pressure in step S3 is 0.5-5 MPa, and the tableting temperature is 25℃-60℃. The thickness of the wetting control layer 3 in step S5 is 0.05mm-0.5mm; The mixed solution contains 0.5%-5% hydrophilic polymer and 0.5%-8% disintegrant by weight of the total mixed solution.

[0030] By employing the above technical solutions, and limiting the particle size range and layer thickness ratio of different particle groups, a reasonable gradation and gradient stacking of coarse and fine particles is achieved, improving the compactness and porosity control of the tablet structure. By controlling the tableting pressure and temperature, appropriate compaction and interfacial bonding between particles are achieved, avoiding excessive compaction that leads to decreased dispersibility, while simultaneously improving overall molding stability. By setting the thickness and component content of the wetting control layer, it ensures good hydrophilic wetting and rapid disintegration capabilities while maintaining continuous coverage, improving the material's contact efficiency and diffusion rate with water. Overall, a synergistic optimization of structural strength, molding stability, and rapid dispersibility is achieved.

[0031] In summary, this application includes at least one of the following beneficial technical effects: Through the synergistic effect of particle size distribution design, gradient laying and tableting process, a stable gradient structure and controllable pore network are constructed inside the sheet-like dry mortar, so that the material can have excellent lightweight and dispersibility while ensuring a certain structural strength. By controlling the gradient temperature drying and the staged decomposition of the pore-forming agent, the pore structure is uniformly formed and the structural collapse is effectively avoided. At the same time, the internal solvent removal efficiency and molding consistency are improved, thereby enhancing the overall stability and construction adaptability. By setting up a wetting control layer and optimizing its composition and thickness ratio, the hydrophilic wetting and disintegration diffusion ability of the material surface is significantly improved, the water penetration and overall dissolution speed are accelerated, thereby improving the quick dissolution efficiency and ease of use. 4. By constructing a gradient pore structure and prefabricated flow-guiding grooves, water can quickly penetrate into all parts of the sheet. At the same time, the hydrophilic polymer in the wetting control layer can actively adsorb water, and the disintegrant expands rapidly upon contact with water to produce a disintegration effect. The synergistic effect of the three enables the sheet-like dry mortar to completely dissolve within 15 seconds after contact with water, which shortens the dissolution time by more than 50% compared with the existing technology. 5. The tablets are formed by compression molding of semi-dry granules reinforced with particles. The interlocking between the particles provides sufficient cohesive force. At the same time, the gradient drying process makes the second pore area on the surface of the tablets have high density, ensuring the mechanical strength and resistance to breakage of the tablets during transportation and handling. 6. The component ratio in the wetting control layer has been optimized, which can automatically adjust the water absorption rate according to the ambient temperature and humidity, avoiding the problem of the surface of the sheet becoming gelatinized while the inside remains dry due to excessive water absorption; 7. Compared with the traditional wet molding process, the dry material spreading-impregnation-tableting process of the present invention is less affected by the rheological properties of raw materials, has good production stability, and a high yield. Attached Figure Description

[0032] Figure 1 This is a cross-sectional view of an embodiment of this application.

[0033] Figure 2 This is a method flowchart of an embodiment of this application.

[0034] Explanation of reference numerals in the attached drawings: 1. Mortar matrix; 2. Support structure; 3. Wetting control layer. Detailed Implementation

[0035] The following is in conjunction with the appendix Figure 1-2 This application will be described in further detail.

[0036] Example 1

[0037] A quick-dissolving flake-shaped dry mortar based on gradient wetting control is prepared as follows: (1) Preparation of particle-reinforced semi-dry particles Weigh the raw materials by weight: 28 parts silicate cement, 65 parts river sand, 5 parts fly ash, 0.8 parts polyethylene glycol (molecular weight 4000), 0.2 parts hydroxypropyl methylcellulose, and 3 parts ammonium bicarbonate. The above raw materials are mixed evenly in a high-speed mixer to form a dry mixture. Then, 12 parts by weight of an ethanol-water solution (ethanol:water = 9:1) are added, and stirring is continued to form a uniform wet mixture, so that the inorganic cementitious material and aggregate are fully wetted and a primary bonding system is formed. The wet mixture is fed into an extrusion pelletizer for pelleting. The extrusion pressure and die size are controlled to keep the wet pellet size between 0.85 mm and 2.0 mm. The wet pellets are then dried in a 65°C hot air environment to allow the internal solvent to gradually evaporate. The final residual solvent weight percentage is controlled at 5%, resulting in structurally stable semi-dry pellets. In this step, ammonium bicarbonate participates in pore formation as a pore-forming agent during the subsequent drying process.

[0038] (2) Gradient laying The semi-dry particles are separated into two particle size groups using a vibrating screen: First particle group: 2.0mm~4.75mm; Second particle group: 0.85mm~1.8mm; During the material laying process, fiberglass mesh is selected as the support body 2. The first particle group is evenly laid on the support body to form the first particle layer with a thickness controlled at 1.5mm. Then, the second particle group is evenly laid on it to form the second particle layer with a thickness also controlled at 1.5mm. This gradient material distribution method places coarse particles in the lower bearing area and fine particles in the upper reaction area, thereby forming a gradient structure of density and pore distribution, which provides a basis for pore control in the subsequent drying stage.

[0039] (3) Tableting The laid particle layer is placed in a tableting device and pressed into shape under a pressure of 2MPa and a temperature of 40℃, so that the particles are initially consolidated and bonded at the interface. During tableting, a suitable temperature is beneficial for moisture migration and binder activation, enabling stable connections between particles while avoiding excessive moisture evaporation that could lead to structural cracks. After compression, a wet tablet is obtained with a total thickness controlled at 2.5 mm and a uniform and stable structure.

[0040] (4) Gradient drying hardening The wet sheet was placed in a temperature-controlled drying oven for gradient drying, which included three stages: First stage: Dry at 50℃ for 10 minutes to allow ammonium bicarbonate to begin to slowly decompose and evenly distribute the gas precursor, while ensuring the stability of the humidity gradient inside the structure. The second stage involves drying at 80°C for 20 minutes to allow ammonium bicarbonate to completely decompose and produce CO2 and NH3 gases, forming a uniform pore structure inside the material and simultaneously constructing a gradient pore region. Third stage: Dry at 60℃ for 15 minutes to remove residual solvent and stabilize the pore structure, preventing structural collapse due to rapid cooling or residual moisture. This gradient drying process creates a gradient structure within the mortar matrix, with a high porosity at the top and a low porosity at the bottom.

[0041] (5) Setting of wetting control layer Preparation of wetting control solution: Weigh 2 parts polyvinyl alcohol and 3 parts sodium carboxymethyl starch, add 95 parts deionized water, and stir at room temperature for 2 hours to completely dissolve and form a homogeneous mixed solution. The mixed solution was uniformly coated onto the surface of the sheet-like dry mortar substrate by spraying, and then dried at 60°C to form a film with a thickness of 0.1 mm, forming a wetting control layer 3. This wetting control layer can quickly absorb water, expand, and partially disintegrate when in contact with water, thereby accelerating the penetration of water into the interior.

[0042] Based on Example 1, adjustments can be made to the raw material ratio, tableting conditions, and drying temperature parameters. The proportion of fly ash can be increased to enhance the stability of the pore structure, the content of polyethylene glycol can be increased to improve the wetting performance, the tableting pressure can be adjusted to 3 MPa to improve the density of the structure, and the drying temperature gradient can be adjusted to optimize the pore uniformity.

[0043] Comparative Example 1 Using the preparation method in the existing technology CN202011560537.5, without setting a gradient spreading layer and a wetting control layer, only a uniform mixing and pressing method is used to prepare sheet mortar.

[0044] Comparative Example 2 Compared to Example 1, instead of particle grading and gradient spreading, all particles are mixed at once and then spread and pressed into tablets.

[0045] Comparative Example 3 Compared with Example 1, no wetting control layer is set, and only the mortar matrix structure is retained.

[0046] Performance testing Performance tests were conducted on the examples and comparative examples, and the test indicators included dissolution time, failure load and 28-day compressive strength.

[0047] The results show that the dissolution time of the embodiments of the present invention is significantly shortened and the structural mechanical properties remain stable. The dissolution time of the embodiments is better than that of the comparative examples, which proves that the synergistic effect of the gradient pore structure and the wetting control layer significantly improves the hydration and dissolution efficiency.

[0048] Mechanism analysis This invention achieves performance improvement through multi-scale structural collaboration: Gradient particle size distribution mechanism: By separating coarse and fine particles, the stress distribution and pore distribution are gradientd, thereby improving structural stability.

[0049] The thermal decomposition mechanism of pore-forming agents: The gas generated by the thermal decomposition of ammonium bicarbonate forms a controllable pore network, thereby improving the water permeation pathway.

[0050] Gradient drying control mechanism: By controlling the pore formation rate through staged temperature control, structural collapse is avoided.

[0051] Wetting regulation mechanism: By utilizing the synergistic effect of hydrophilic polymers and disintegrants, a dual effect of "rapid water absorption + rapid disintegration" is achieved.

[0052] The overall technical effects of this application are as follows: Through the synergistic effect of gradient particle structure design, controllable porosity construction, and surface wetting control layer, the following technical effects are achieved: Significantly shortens dissolution time; Increase the hydration reaction rate; Maintain high mechanical strength; Improve construction convenience; Achieving a balance between structural strength and rapid dissolution performance.

[0053] Example 2

[0054] This embodiment provides a fast-dissolving sheet-like dry mortar based on gradient wetting control. Its preparation method is basically the same as that of Example 1, except that the particle preparation method, pore-forming agent system and wetting control layer formation process are optimized to further improve the uniformity of dissolution and structural stability.

[0055] (1) Preparation of particle-reinforced semi-dry particles Weigh the raw materials by weight: 30 parts silicate cement, 60 parts river sand, 8 parts slag powder, 1.2 parts polyethylene glycol (molecular weight 6000), 0.3 parts hydroxypropyl methylcellulose, and 2.5 parts azodicarbonamide; The above raw materials are put into a planetary mixer and mixed evenly to form a dry mixture. Then, a composite solvent system consisting of 10 parts by weight of deionized water and a small amount of ethanol (mass ratio 8:2) is added, and stirring is continued to form a wet mixture, so that the system has a more uniform wetting distribution and better granulation properties. The wet mixture is granulated using a drum granulator, with the rotation speed and spray rate controlled to maintain the wet particle size between 0.85 mm and 4.5 mm. Subsequently, it undergoes segmented drying at 60°C to ultimately control the solvent residue rate to 3%–6%, yielding uniformly structured semi-dry granules. In this embodiment, azodicarbonamide is used as the main pore-forming agent. It decomposes and releases gas under conditions above 70°C, which is beneficial to forming a more uniform pore structure with a lower closure rate.

[0056] (2) Gradient laying The semi-dry granules were divided into a first granule group and a second granule group, wherein: The particle size of the first particle group is 2.5mm to 4.5mm; The particle size of the second particle group is 0.85 mm to 2.0 mm; Particle layers are sequentially laid on the polyester nonwoven fabric support 2. The thickness of the first particle layer is 2.0 mm and the thickness of the second particle layer is 1.0 mm, thus forming a more obvious gradient structure with finer material at the top and coarser material at the bottom.

[0057] (3) Tableting The prepared particle layer is placed in a tableting device and pressed at 3MPa pressure and 45℃ to allow for more complete interlocking and interface fusion between the particles. The thickness of the wet tablet after compression was controlled at 2.8 mm, which has a higher initial density than that of Example 1, providing a basis for the subsequent stability of the pore structure.

[0058] (4) Gradient drying hardening A three-stage gradient drying process is adopted: First stage: Dry at 45℃ for 12 minutes to allow the moisture in the system to migrate evenly and activate the initial decomposition of azodicarbonamide; Second stage: Dry at 85℃ for 25 minutes to fully decompose the pore-forming agent, release a large amount of gas, and form a network of interconnected pores inside the sheet; Third stage: Dry at 65℃ for 15 minutes to stabilize the pore structure and further remove residual solvent.

[0059] By optimizing the temperature profile, the pore distribution in this embodiment is more uniform and the pore wall structure is more complete.

[0060] (5) Setting of wetting control layer Preparation of wetting control solution: Dissolve 1.5 parts of polyethylene glycol (molecular weight 4000), 2.5 parts of crosslinked polyvinyl chloride, and 2 parts of sodium carboxymethyl starch in 94 parts of deionized water and stir until homogeneous. The solution was uniformly coated onto the surface of the mortar substrate using a roller coating method and dried at 55°C to form a wetting control layer 3 with a thickness of 0.12 mm. This wetting control layer can rapidly expand and generate micro-fracture structures upon contact with water, accelerating the formation of water penetration pathways and increasing the overall dissolution rate.

[0061] This embodiment introduces an azodicarbonamide pore-forming system and optimizes the gradient drying curve to make the pore structure more uniform and continuous. At the same time, combined with a cross-linked disintegration system wetting control layer, faster water diffusion and shorter dissolution time are achieved. Compared to Example 1, this example further improves the dissolution rate while maintaining similar compressive strength, and further optimizes structural stability and construction adaptability, demonstrating a better overall performance balance.

[0062] The implementation principle of the fast-dissolving sheet-like dry mortar based on gradient wetting control and its preparation process in this application embodiment is as follows: By synergistically controlling the multi-scale structure of the mortar system, the integration of "internal pore gradient construction - particle gradation layered stacking - rapid surface wetting response" is achieved. Inside the material, the pore-forming agent decomposes and generates gas in stages under gradient temperature drying conditions, forming a pore structure that gradually transitions from high porosity to low porosity, thus constructing directional water permeation channels. In the particle system, the layered laying and pressing of particles of different sizes enables coarse and fine particles to form an ordered stacking structure, improving the overall structural strength and stability. On the material surface, a wetting control layer composed of hydrophilic polymers and disintegrants is set, enabling the material to quickly absorb water, expand, and locally disintegrate after contact with water, significantly reducing the initial wetting resistance and accelerating the diffusion of water into the interior. The synergistic effect of these three factors allows water to quickly penetrate from the surface to the interior and diffuse evenly along the preset pore channels, achieving rapid dissolution and full hydration of the mortar matrix. This significantly improves construction efficiency and ease of use while ensuring certain mechanical properties.

[0063] The above are all preferred embodiments of this application, and are not intended to limit the scope of protection of this application. Therefore, all equivalent changes made in accordance with the structure, shape and principle of this application should be covered within the scope of protection of this application.

Claims

1. A fast-dissolving flake-shaped dry mortar based on gradient wetting control, characterized in that: It includes a mortar matrix (1), a support (2), and a wetting control layer (3); The mortar matrix (1) is obtained by pressing semi-dry particles into sheets and then drying and hardening them. The mortar matrix (1) has a gradient distribution of pore structure inside. The pore structure includes a first pore region and a second pore region. The average porosity of the first pore region is greater than the average porosity of the second pore region. The first pore region is located on one side of the upper surface of the mortar matrix (1), and the second pore region is located on one side of the lower surface of the mortar matrix (1). The support (2) is disposed on the lower surface of the mortar matrix (1) or embedded in the lower part of the mortar matrix (1); The wetting control layer (3) is disposed on the upper surface of the mortar matrix (1), and the wetting control layer (3) contains a hydrophilic polymer and a disintegrant.

2. The fast-dissolving flaky dry mortar based on gradient wetting control according to claim 1, characterized in that: The average porosity of the first pore region is 25%-45%, and the average porosity of the second pore region is 10%-25%.

3. The fast-dissolving flake dry mortar based on gradient wetting control according to claim 1, characterized in that: The lower surface of the mortar matrix (1) is provided with a plurality of spaced-apart flow-guiding grooves, which extend along a first direction and form flow-guiding ridges between adjacent flow-guiding grooves.

4. The fast-dissolving flake dry mortar based on gradient wetting control according to claim 1, characterized in that: The particle size of the particle-reinforced semi-dry particles is 0.85mm-4.75mm; The particle-reinforced semi-dry particles comprise the following raw materials in parts by weight: 15-70 parts inorganic cementitious material, 15-85 parts aggregate, 0-25 parts admixture, 0.5-5 parts water-soluble binder, and 0.5-8 parts pore-forming agent.

5. The fast-dissolving flaky dry mortar based on gradient wetting control according to claim 4, characterized in that: The pore-forming agent is at least one of ammonium bicarbonate, ammonium carbonate, urea, and azodicarbonamide. The pore-forming agent decomposes to generate gas during the drying and hardening process to form the gradient-distributed pore structure.

6. The fast-dissolving flaky dry mortar based on gradient wetting control according to claim 1, characterized in that: The weight ratio of hydrophilic polymer to disintegrant in the wetting control layer (3) is 1:0.5-1:3; The hydrophilic polymer is at least one of polyvinyl alcohol, polyethylene glycol, and hydroxypropyl methylcellulose; The disintegrant is at least one of sodium carboxymethyl starch, crospovidone, and low-substituted hydroxypropyl cellulose.

7. The fast-dissolving flaky dry mortar based on gradient wetting control according to claim 3, characterized in that: The support (2) is a mesh structure, which includes a first braided filament extending in a first direction and a second braided filament extending in a second direction. The diameter of the first braided filament is larger than that of the second braided filament, so that the rigidity of the mesh structure in the first direction is greater than its rigidity in the second direction. The flow-guiding groove extends along the first direction.

8. A preparation process for a quick-dissolving flake-shaped dry mortar based on gradient wetting control as described in any one of claims 1-7, characterized in that: Includes the following steps: Step S1: Preparation of particle-reinforced semi-dry granules: Inorganic cementitious materials, aggregates, admixtures, water-soluble binders, and pore-forming agents are mixed evenly to form a dry mixture. The dry mixture is then mixed with a solvent to obtain a wet mixture. The wet mixture is granulated to obtain wet granules. The wet granules are then dried to obtain semi-dry granules. The particle size of the semi-dry granules is controlled to be 0.85mm-4.75mm, and the weight percentage of residual solvent in the semi-dry granules is 1%-8%. Step S2: Gradient spreading: The semi-dry particles obtained in step S1 are divided into a first particle group and a second particle group, wherein the average particle size of the first particle group is greater than the average particle size of the second particle group. The first particle group is first spread on the support (2) to form a first particle layer, and then the second particle group is spread on the first particle layer to form a second particle layer. Step S3: Tableting: The support 2, on which the first particle layer and the second particle layer were laid in step S2, is compressed to obtain a wet tablet. Step S4: Gradient drying and hardening: The wet sheet obtained in step S3 is subjected to gradient temperature drying, which causes the pore-forming agent to decompose and generate gas to form a gradient pore structure, while removing the solvent to obtain a sheet-like dry mortar matrix (1). Step S5: Set a wetting control layer: Set a wetting control layer (3) on the upper surface of the sheet-like dry mortar matrix (1) obtained in step S4. The wetting control layer (3) is obtained by spraying or roller coating a mixed solution of hydrophilic polymer and disintegrant onto the upper surface and drying it.

9. The preparation process of a quick-dissolving flake dry mortar based on gradient wetting control according to claim 8, characterized in that: The gradient temperature drying in step S4 includes: first drying at a low temperature of 40℃-60℃ for 5-15 minutes to make the pore-forming agent evenly distributed and begin to decompose; Then dry at a medium temperature of 70℃-90℃ for 15-30 minutes to completely decompose the pore-forming agent and form pores inside the tablet. Finally, dry at a constant temperature of 50℃-70℃ for 10-20 minutes to remove residual solvent.

10. The preparation process of a quick-dissolving flake dry mortar based on gradient wetting control according to claim 8, characterized in that: In step S2, the average particle size of the first particle group is 2.0mm-4.75mm, the average particle size of the second particle group is 0.85mm-1.8mm, and the ratio of the thickness of the first particle layer to the thickness of the second particle layer is 1:0.5-1:

2. The tableting pressure in step S3 is 0.5-5 MPa, and the tableting temperature is 25℃-60℃. The thickness of the wetting control layer 3 in step S5 is 0.05mm-0.5mm; The mixed solution contains 0.5%-5% hydrophilic polymer and 0.5%-8% disintegrant by weight of the total mixed solution.

Citation Information

Patent Citations

  • A preparation process for sheet-like dry mortar and sheet-like dry mortar

    CN112720787B