A method for value-added recovery of lithium iron phosphate black powder to prepare high-pressure lithium iron phosphate precursor.
By employing a ternary eutectic solvent calcination, leaching, and crystallization process, the problems of high energy consumption and low product purity in the recycling of waste lithium iron phosphate black powder have been solved, achieving efficient and green high-pressure lithium iron phosphate precursor preparation.
Patent Information
- Application Number
- CN202611215593.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-12
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies for recycling waste lithium iron phosphate black powder suffer from problems such as high energy consumption, lengthy processes, high acid consumption, low impurity removal efficiency, high iron loss, low product added value, and difficulty in preparing high-density lithium iron phosphate precursors.
A ternary eutectic solvent composed of a hydrogen bond acceptor, an oxalate-based hydrogen bond donor, and a reducing agent is used to achieve efficient and selective separation and purification of iron, lithium, and phosphorus through calcination, leaching, aging, and antisolvent crystallization, thereby preparing high-purity monoclinic ferrous oxalate and lithium dihydrogen phosphate.
The process achieves high efficiency and green recycling, producing high-purity ferrous oxalate and lithium dihydrogen phosphate, meeting the requirements of high-pressure lithium iron phosphate precursors, simplifying the process, and reducing environmental pollution and operating costs.
Smart Images

Figure CN123105573A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of waste lithium-ion battery recycling technology, specifically relating to a method for recycling waste lithium iron phosphate black powder, and more particularly to a method for preparing high-pressure lithium iron phosphate precursors, namely high-purity monoclinic ferrous oxalate (α-FeC2O4·2H2O) and lithium dihydrogen phosphate (LiH2PO4), from waste lithium iron phosphate black powder using a ternary eutectic solvent. Background Technology
[0002] As early commercialized lithium iron phosphate (LiFePO4, LFP) batteries reach their 5-8 year service life, the number of retired batteries is rising sharply. The recycling of waste LFP cathode materials (black powder) has become an urgent issue for the sustainable development of the new energy industry. Simultaneously, the increasing demands for longer driving ranges in new energy vehicles are driving a sustained increase in market demand for high-density LFP cathode materials. Therefore, the value-added recycling of waste LFP to prepare its key precursors has significant industrial value.
[0003] Currently, there are two main technical routes for the recovery of LFP black powder. Pyrometallurgy involves high-temperature roasting to convert valuable elements into metals or oxides, which are then extracted separately. However, this method is energy-intensive and primarily focuses on lithium extraction, resulting in significant waste of phosphorus and iron resources. Hydrometallurgy involves acid leaching to completely decompose LFP and then extracting valuable elements stepwise. For example, oxalic acid can be used as a leaching agent to prepare ferrous oxalate and lithium phosphate (CN122344134A), or complete leaching with inorganic acids such as sulfuric acid and hydrochloric acid followed by stepwise precipitation (CN122444199A, CN122326973A). However, this method suffers from lengthy processes, high acid consumption, and low impurity removal efficiency, resulting in products with low added value. In recent years, eutectic solvents (DES) have attracted attention due to their green and designable nature. However, in existing choline chloride-oxalate binary DES systems, ferric iron and oxalate readily form soluble complexes ([Fe(C2O4)3)). 3- This leads to increased iron loss. The ternary DES system of choline chloride-citric acid-ascorbic acid uses a dissolution-precipitation method, requiring the addition of a precipitant to recover iron. This fails to achieve in-situ directional iron retention during leaching and does not address the problem of residual carbon layers from black powder inhibiting leaching efficiency. Furthermore, the ferrous oxalate obtained from existing recovery routes is mostly mixed crystal form or metastable microcrystals, which cannot meet the specific requirements of high-pressure compaction LFP precursors for the iron source phase.
[0004] Therefore, developing a short-process, green method for value-added recovery and preparation of high-density lithium iron phosphate precursors from waste lithium iron phosphate black powder has significant industrial application value. Summary of the Invention
[0005] In view of the problems existing in the background technology, this application provides a method for value-added recovery of lithium iron phosphate black powder to prepare high-pressure lithium iron phosphate precursor.
[0006] To achieve the above objectives, this application adopts the following technical solution: A method for preparing high-pressure lithium iron phosphate precursor by value-added recycling of lithium iron phosphate black powder is provided, comprising: S1. Lithium iron phosphate black powder is calcined to obtain the calcined product; S2. The calcined product is mixed with a ternary eutectic solvent containing hydrogen bond acceptor component A, oxalic acid hydrogen bond donor component B and reducing agent component C for leaching reaction. The reaction product is separated into leaching residue and leaching liquid by solid-liquid separation. S3. The leaching residue is mixed with water and aged. After solid-liquid separation, washing and drying, ferrous oxalate dihydrate monoclinic crystal system is obtained. S4. Add phosphate to the leachate, react and then separate the solid and liquid to obtain the purified liquid and precipitate; S5. After the impurity removal liquid is acidified with an acidifying agent, an antisolvent is added to carry out a precipitation reaction. After solid-liquid separation, washing, and drying, lithium dihydrogen phosphate is obtained.
[0007] Compared with the prior art, one or more of the above technical solutions can achieve at least one of the following beneficial effects: The provided recycling process achieves highly efficient and selective separation of iron from lithium and phosphorus. This invention uses oxalic acid as a hydrogen bond donor to directly construct a ternary eutectic solvent, enabling the efficient separation of Fe during leaching. 3+ The in-situ reduction / precipitation synergistic retention method, compared to the existing leaching-then-precipitation route, fundamentally avoids the formation of soluble ferric oxalate complexes, significantly simplifies solid-liquid separation operations, and improves the direct recovery rate of iron resources. Furthermore, through precise control of subsequent aging and antisolvent crystallization, the high-value utilization of both products is further achieved.
[0008] The recovered products are high-value, high-purity, and have precise phase composition, making them directly usable in the synthesis of high-density lithium iron phosphate. By controlling the Ostwald aging process, pure-phase monoclinic α-FeC₂O₄·₂H₂O can be obtained; by controlling the dielectric properties of the antisolvent, battery-grade LiH₂PO₄ can be obtained. Both products achieve a purity of over 99% and exhibit excellent phase consistency, allowing them to be used as precursors for high-density lithium iron phosphate without secondary purification.
[0009] The process is green and environmentally friendly, and the solvent system is recyclable. The eutectic solvent and antisolvent used in this invention can be recovered and recycled through distillation, resulting in extremely low wastewater discharge, which meets the requirements of green chemical development.
[0010] The process is concise, the operating conditions are mild, and the prospects for industrial application are broad. Compared with the lengthy route of multi-step acid leaching and step-by-step precipitation in traditional hydrometallurgy, this invention significantly shortens the process flow, and the operating conditions of each step are within the range that conventional equipment can withstand, thus possessing good economic efficiency and industrial scale-up feasibility. Attached Figure Description
[0011] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0012] Figure 1 This is a process flow diagram of the method of the present invention.
[0013] Figure 2 This is a scanning electron microscope (SEM) image of the recovered ferrous oxalate dihydrate from Example 1.
[0014] Figure 3 The X-ray diffraction (XRD) patterns of ferrous oxalate dihydrate recovered in Example 1 and Comparative Example 2 are shown.
[0015] Figure 4 The image shows the X-ray diffraction (XRD) pattern of lithium dihydrogen phosphate recovered in Example 1. Detailed Implementation
[0016] This invention provides a method for the value-added recovery and preparation of high-pressure lithium iron phosphate precursors from lithium iron phosphate black powder. A green eutectic solvent (DES) is used to selectively recover lithium, iron, and phosphorus from the lithium iron phosphate black powder. The selective and reducing properties of the DES allow for one-step value-added preparation of high-purity ferrous oxalate and lithium dihydrogen phosphate. The biodegradability and recyclability of the DES reduce environmental pollution and acid / alkali consumption. Details are as follows: A typical embodiment of the present invention provides a method for the value-added recovery of lithium iron phosphate black powder to prepare high-pressure lithium iron phosphate precursor, comprising: S1. Lithium iron phosphate black powder is calcined to obtain the calcined product. During the calcination process, lithium iron phosphate undergoes a phase transformation in an oxygen-containing atmosphere. The main reaction is shown in formula (1). The calcined product is a mixed phase of Li3Fe2(PO4)3 and Fe2O3, which is reddish-brown. The purpose of calcination is to avoid the residual carbon layer from hindering the subsequent contact between DES and active materials, and at the same time to transform the olivine phase LFP into a mixed phase structure that is easier for DES to complex and leach.
[0017] (1) S2. The calcined product is mixed with a ternary eutectic solvent containing hydrogen bond acceptor component A, oxalic acid hydrogen bond donor component B and reducing agent component C for leaching reaction. The reaction product is separated into leaching residue and leaching liquid by solid-liquid separation. Specifically, hydrogen bond acceptor component A, oxalate hydrogen bond donor component B and reducing agent component C are mixed and heated to a clear and transparent liquid to obtain a ternary eutectic solvent with a rich hydrogen bond network structure. The calcined product from step S1 was leached with a ternary eutectic solvent (DES) at a certain solid-liquid ratio under constant temperature stirring. After the reaction, the solid and liquid were separated to obtain leaching residue and leaching solution. The leaching residue mainly consisted of high-purity ferrous oxalate dihydrate (FeC2O4·2H2O), while the leaching solution was enriched with Li, P, and small amounts of impurity ions such as Al and Fe. The Li3Fe2(PO4)3 and Fe2O3 in the calcined product underwent a three-step in-situ reaction of dissociation, reduction, and precipitation in the ternary eutectic solvent system described in this invention.
[0018] First, the abundant hydrogen bond network in DES targets and weakens the lattice energy of the Fe-O bond through hydrogen bonding, thus promoting Fe... 3+ The Fe is released from the solid lattice (see equations (2)~(3)); secondly, the uniformly dispersed reducing agent component C (such as ascorbic acid) in the DES releases the Fe in situ at the molecular scale. 3+ Reduced to Fe 2+ (Equation (4)), the kinetic rate of this reduction reaction is significantly better than that of Fe. 3+ The complexation reaction with oxalate effectively avoids the formation of soluble iron oxalate complexes ([Fe(C2O4)3]). 3- The generation of ); finally, Fe 2+ The oxalate ions, which are in situ dissociated in the DES, are captured and immediately precipitate as ferrous oxalate (Equation (5)). It should be emphasized that "in situ" refers to Fe... 3+ The reduction and precipitation occur sequentially within the same reaction microregion the moment the iron dissociates from the solid lattice and enters the liquid phase microregion, rather than first leaching all the iron into the liquid phase and then adding a precipitant. This in-situ tandem reaction mechanism is key to achieving efficient and selective separation of iron from lithium and phosphorus.
[0019] (2) (3) (4) (5) Where Red represents the reduced state of the reducing agent, and O x Represents the oxidation state of the reducing agent; S3. The leaching residue is mixed with water and aged. After solid-liquid separation, washing and drying, monoclinic ferrous oxalate dihydrate (α-FeC2O4·2H2O) is obtained. The core mechanism of aging is the Ostwald ripening process: in a hot water medium at 80-100℃, the initially precipitated metastable ferrous oxalate (usually a β-orthorhombic or mixed phase) in the leaching residue gradually dissolves and recrystallizes into the thermodynamically most stable monoclinic α-FeC₂O₄·2H₂O, following the principle of minimum thermodynamic free energy. This phase has a layered crystal structure, which is conducive to the interlayer insertion and extraction of lithium ions. Its regular lamellar morphology helps to improve the compaction density of the electrode, making it the optimal iron source phase for preparing high-compact-density lithium iron phosphate cathode materials. If the aging step is omitted, the resulting ferrous oxalate is mostly a β-phase or mixed crystal form, lacking ordered layered channels, which makes it difficult to meet the requirements for preparing high-compact-density lithium iron phosphate.
[0020] S4. Add phosphate to the leachate, react and then separate the solid and liquid to obtain the purified liquid and precipitates of aluminum phosphate and / or iron phosphate; this process can reduce Al residue to <50ppm and Fe residue to <10ppm, meeting the purity requirements of battery-grade lithium dihydrogen phosphate. S5. After the impurity-removing liquid is acidified with an acidifying agent, an antisolvent is added to carry out a precipitation reaction. At this time, the dielectric constant of the system is significantly reduced, and the solvent's ability to solvate ions is weakened, resulting in a sharp decrease in the solubility of LiH2PO4, thereby inducing its crystallization. After solid-liquid separation, washing, and drying, lithium dihydrogen phosphate is obtained.
[0021] In some preferred embodiments, in step S1, the calcination temperature is 400~800℃, for example, 400℃, 500℃, 600℃, 700℃, 800℃, etc.; the calcination time is 2~6 hours, for example, 2h, 3h, 4h, 5h, 6h, etc.; the carbon content of the calcined product is ≤0.05%. If the temperature is too low, the residual carbon layer (carbon content >0.1%) in the lithium iron phosphate black powder is difficult to completely oxidize and remove, reducing the selective leaching efficiency of subsequent DES; if the temperature is too high, it will cause severe sintering between particles, increasing the solid-phase diffusion resistance, which is not conducive to sufficient contact between DES and active materials.
[0022] In some preferred embodiments, the hydrogen bond acceptor component A is at least one of a choline compound or a guanidine salt compound containing a quaternary ammonium salt structure; the choline compound containing a quaternary ammonium salt structure is a choline derivative; the guanidine salt compound containing a quaternary ammonium salt structure is an inorganic acid salt type guanidine compound; preferably, choline chloride.
[0023] In some preferred embodiments, the oxalic acid hydrogen bond donor component B is oxalic acid and / or oxalic acid dihydrate, preferably solid oxalic acid dihydrate.
[0024] In some preferred embodiments, the reducing agent component C is at least one of ascorbic acid, citric acid, aminocarboxylic acid, hydroxycarboxylic acid, and sulfonic acid, preferably ascorbic acid.
[0025] In some preferred embodiments, the molar ratio of the hydrogen bond acceptor component A to the oxalate-based hydrogen bond donor component B is 1:0.6 to 1:3, for example, 1:0.6, 1:0.8, 1:1, 1:1.2, 1:1.5, 1:1.8, 1:2, 1:2.2, 1:2.5, 1:2.8, 1:3, etc., preferably 1:1 to 1:2, which focuses more on the hydrogen bond saturation and viscosity balance of the system.
[0026] In some preferred embodiments, the molar ratio of the reducing agent component C to the hydrogen bond acceptor component A is 0.3 to 0.8:1, for example, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, etc.
[0027] In some preferred embodiments, in step S2, the solid-liquid mass ratio of the leaching reaction is 1:5 to 1:20, for example, 1:5, 1:8, 1:10, 1:12, 1:15, 1:18, 1:20, etc.
[0028] In some preferred embodiments, in step S2, the temperature of the leaching reaction is 50~120℃, for example 50℃, 60℃, 70℃, 80℃, 90℃, 100℃, 110℃, 120℃, etc.
[0029] In some preferred embodiments, in step S2, the leaching reaction time is 0.5 to 8 hours, for example, 0.5h, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, etc.
[0030] In some preferred embodiments, in step S2, the stirring speed of the leaching reaction is 100~600 rpm, for example, 100 rpm, 200 rpm, 300 rpm, 400 rpm, 500 rpm, 600 rpm, etc.
[0031] In some preferred embodiments, in step S3, the solid-liquid mass ratio of the aging treatment is 1:2 to 1:8, for example, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, etc.
[0032] In some preferred embodiments, in step S3, the aging treatment temperature is 80~100℃, for example 80℃, 85℃, 90℃, 95℃, 100℃, etc.
[0033] In some preferred embodiments, in step S3, the aging treatment time is 4 to 24 hours, for example, 4 hours, 6 hours, 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours, 24 hours, etc.
[0034] In some preferred embodiments, in step S4, the reaction temperature is 20~80℃, for example 20℃, 30℃, 40℃, 50℃, 60℃, 70℃, 80℃, etc., preferably 40~60℃. Under mild heating conditions, phosphate ions react with Al... 3+ Residual Fe 3 + The generated phosphate precipitate particles are large and easy to filter, and the formation of Al(OH)3 colloids can be effectively avoided. Under these conditions, the concentration can be stably controlled at <30 mg / L, and the Fe residue can be controlled at <10 mg / L, providing a pure mother liquor environment for the subsequent crystallization of high-purity lithium dihydrogen phosphate.
[0035] In some preferred embodiments, in step S4, the reaction time is 0.5 to 3 hours, for example, 0.5h, 1h, 2h, 3h, etc.
[0036] In some preferred embodiments, in step S4, the pH value of the purified solution is 3 to 4, for example, 3, 3.5, 4, etc.
[0037] In some preferred embodiments, in step S4, the phosphate is sodium phosphate and / or sodium dihydrogen phosphate.
[0038] In some preferred embodiments, in step S5, the acidification treatment involves adjusting the pH of the reaction system to 2-3.
[0039] In a partially preferred embodiment, the acidifying agent in step S5 is phosphoric acid.
[0040] In some preferred embodiments, the antisolvent in step S5 is at least one of C1-C4 alcohols, acetone, and dimethyl sulfoxide, preferably acetone or anhydrous ethanol. The antisolvent effect is stronger, the supersaturation precipitation rate of lithium dihydrogen phosphate is milder, and it is beneficial to the growth of large-particle crystals.
[0041] In some preferred embodiments, in step S5, the volume ratio of the purified liquid to the antisolvent is 1:1 to 1:7, preferably 1:4 to 1:6, such as 1:4, 1:4.5, 1:5, 1:5.5, 1:6, etc. A high proportion of antisolvent, while increasing the yield, will lead to more impurities being co-precipitated, causing the product purity to drop below 99%.
[0042] In some preferred embodiments, in step S5, the temperature of the precipitation reaction is 0~40℃, such as 0℃, 10℃, 20℃, 30℃, 40℃, etc., and more preferably 0~10℃. The low temperature environment further reduces the solubility of LiH2PO4 in the mixed solvent and greatly improves the crystallization yield.
[0043] In some preferred embodiments, the method further includes: distilling the liquid phase obtained from solid-liquid separation in step S5 to remove and recover the antisolvent and water, then replenishing the lost components B and C to prepare a new ternary eutectic solvent and returning it to step S2 for recycling, and returning the collected antisolvent to step S5 for recycling.
[0044] In some embodiments, the distillation temperature in step S5 is 70~90℃.
[0045] In some embodiments, the solid-liquid separation in steps S2 to S5 can be filtration or centrifugation, the washing liquid can be ethanol, the drying temperature can be 60~80℃, and the drying time can be selected according to actual needs.
[0046] To facilitate understanding of this application, the following description will be more comprehensive and detailed in conjunction with the accompanying drawings and preferred embodiments, but the scope of protection of this application is not limited to the following specific embodiments.
[0047] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of this application.
[0048] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this application are available on the market or can be prepared by existing methods.
[0049] The main elemental contents of the lithium iron phosphate black powder used in the following embodiments and comparative examples are shown in Table 1.
[0050] Table 1. Element content (wt%) of lithium iron phosphate black powder Example 1 A method for the value-added recovery and preparation of high-pressure lithium iron phosphate precursor from lithium iron phosphate black powder, the process flow diagram is as follows: Figure 1 As shown, it includes: S1. Take 50g of lithium iron phosphate black powder, place it in a muffle furnace and heat it to 650℃ at a rate of 5℃ / min. Keep it at the temperature for 4 hours and roast it in an air atmosphere. After natural cooling, reddish-brown roasted products Li3Fe2(PO4)3 and Fe2O3 are obtained, with a carbon content of 0.04 wt%.
[0051] S2. Choline chloride, oxalic acid, and L-ascorbic acid were mixed in a molar ratio of 1:0.6:0.3 and stirred and heated at 70°C for 2 hours until a clear and transparent liquid was formed, yielding a ternary eutectic solvent. The reddish-brown calcined product of S1 was mixed with DES at a solid-liquid ratio of 1:10 (g:g), and leached at 70°C for 6 hours. After leaching, the mixture was filtered to obtain ferrous oxalate and a leachate containing impurities such as lithium and phosphorus.
[0052] S3. Ferrous oxalate obtained in S2 was slurried with deionized water at a solid-liquid ratio of 1:4 and aged at 90℃ for 20 hours. After centrifugation and filtration, the mixture was washed three times with ethanol and then placed in a 60℃ constant temperature oven for 6 hours to obtain high-purity monoclinic ferrous oxalate dihydrate (α-FeC2O4·2H2O), with the following morphology. Figure 2 As shown, SEM reveals that it exhibits distinct layered monoclinic crystal characteristics. Furthermore, the XRD curves are as follows... Figure 3 As shown (and the XRD curve of Comparative Example 2 is shown for comparison), its characteristic diffraction peaks are in perfect agreement with the α-FeC2O4·2H2O standard card (PDF No. 04-015-7971), indicating that the synthesized ferrous oxalate is a layered monoclinic α-FeC2O4·2H2O.
[0053] S4. Add sodium phosphate to the leaching solution containing Li and P to adjust the pH to 4. Stir at 50°C for 2 hours to precipitate and remove impurities such as aluminum and trace iron. After filtration, the purified solution and aluminum phosphate / ferric phosphate precipitate are obtained.
[0054] S5. The pH of the purified solution was adjusted to 2.5 with phosphoric acid for acidification. Then, acetone was added dropwise as a countersolvent at a flow rate of 5 mL / min and a volume ratio of 1:6. The precipitation temperature was 0℃, and the precipitation time was 3 h. Afterward, centrifugation and filtration were performed to obtain the countersolvent filter residue and the countersolvent solution. The countersolvent filter residue was washed three times with ethanol and then placed in an 80℃ incubator for 6 hours to obtain solid lithium dihydrogen phosphate. Its XRD curve is shown below. Figure 4 As shown, by Figure 4 The characteristic diffraction peaks are in perfect agreement with the LiH2PO4 standard card (PDF No. 04-012-8800), and no impurity peaks are observed, indicating that pure phase LiH2PO4 has been synthesized.
[0055] S6, DES Regeneration and Recycling: Evaporate excess water in the antisolvent at 80°C and collect the antisolvent acetone by distillation. Add the standard loss amount of oxalic acid and ascorbic acid solid powder and continue stirring and heating at 70°C for 2 hours until transparent to regenerate DES.
[0056] Example 2 This embodiment is basically the same as that of Embodiment 1, except that the hydrogen bond acceptor in step S2 is betaine hydrochloride.
[0057] Example 3 This embodiment is basically the same as Embodiment 1, except that the hydrogen bond acceptor in step S2 is guanidine hydrochloride.
[0058] Example 4 This embodiment is basically the same as Embodiment 1, except that tartaric acid is used as the reducing agent in step S2.
[0059] Example 5 This embodiment is basically the same as Embodiment 1, except that malonic acid is used as the reducing agent in step S2.
[0060] Example 6 This embodiment is basically the same as Embodiment 1, except that citric acid is used as the reducing agent in step S2.
[0061] Example 7 This embodiment is basically the same as Embodiment 1, except that in step S2, choline chloride and oxalic acid are mixed in a molar ratio of 1:3.
[0062] Example 8 This embodiment is basically the same as Embodiment 1, except that in step S2, choline chloride and L-ascorbic acid are mixed in a molar ratio of 1:0.8.
[0063] Example 9 This embodiment is basically the same as Embodiment 1, except that in step S2, choline chloride and L-ascorbic acid are mixed in a molar ratio of 1:1.2.
[0064] Example 10 This embodiment is basically the same as Embodiment 1, except that the solid-liquid mass ratio is 1:5 in step S2.
[0065] Example 11 This embodiment is basically the same as embodiment 1, except that the solid-liquid mass ratio in step S2 is 1:15.
[0066] Example 12 This embodiment is basically the same as Embodiment 1, except that the temperature in step S2 is 50°C.
[0067] Example 13 This embodiment is basically the same as embodiment 1, except that the temperature in step S2 is 120°C and the leaching reaction is carried out in a closed pressure vessel.
[0068] Example 14 This embodiment is basically the same as Embodiment 1, except that the antisolvent in step S5 is methanol.
[0069] Example 15 This embodiment is basically the same as Embodiment 1, except that the antisolvent in step S5 is ethanol.
[0070] Example 16 This embodiment is basically the same as that of Embodiment 1, except that the antisolvent in step S5 is isopropanol.
[0071] Example 17 Following the method of Example 1, the DES regenerated in step S6 was returned to step S2 for recycling, and a total of 5 leaching cycles were performed. The precipitation rate of Fe in each cycle was: 98.2% in the first cycle, 97.8% in the second cycle, 97.1% in the third cycle, 96.3% in the fourth cycle, and 95.5% in the fifth cycle. After the fifth cycle, the purity of the recovered ferrous oxalate was 98.9 wt%, and the purity of lithium dihydrogen phosphate was 99.1 wt%. Even after 5 cycles, ferrous oxalate still maintained a pure monoclinic crystal system. The results indicate that the DES of the present invention has good recycling performance after regeneration, confirming the industrial reliability of the S6 regeneration step.
[0072] Comparative Example 1 This comparative example is basically the same as Example 1, except that in step S2, a single oxalic acid aqueous solution (concentration of 1.5 mol / L) is used instead of the ternary eutectic solvent as the leaching agent.
[0073] Comparative Example 2 The comparative example is basically the same as Example 1, except that no aging treatment is performed in step S3 (i.e., the leaching residue is directly washed and dried after filtration).
[0074] The XRD pattern of the recovered ferrous oxalate is shown below. Figure 3 As shown, the obtained ferrous oxalate is orthorhombic ferrous oxalate (β-FeC2O4·2H2O).
[0075] Comparative Example 3 The only difference between this comparative example and Example 1 is that step S1 is omitted, and lithium iron phosphate black powder is directly used as raw material for subsequent selective leaching.
[0076] The leachate after leaching in step S2 was collected, and the leaching rate of each element was tested by ICP.
[0077] The leaching data and product purity of each embodiment and comparative example are shown in Table 2 below.
[0078] Table 2 Table 2 shows that the ferrous oxalate prepared in Examples 1-16 has a high purity, reaching up to 99.6%. Correspondingly, the lithium dihydrogen phosphate prepared using the antisolvent has a purity of at least 96%, and can reach as high as 99.8%. This indicates that the method provided by this invention can prepare high-purity ferrous oxalate and battery-grade lithium dihydrogen phosphate, meeting the requirements for preparing high-density lithium iron phosphate precursors. Example 9 shows that when the amount of reducing agent increases to a certain extent, the lithium / phosphorus / aluminum leaching rate is low. Analysis suggests that when the amount of ascorbic acid is too high, the leaching system exists in a solid-liquid mixed state, making it difficult to form a complete DES system, resulting in low overall leaching efficiency.
[0079] In Comparative Example 1, only oxalic acid was used for the leaching of lithium iron phosphate. Iron exhibited a high leaching rate, but ferrous oxalate precipitate could not be formed. This is because Fe... 3+ It reacts with oxalic acid to form a soluble [Fe(C2O4)3] 3- The complex enters the solution. In Comparative Example 2, reducing the aging process lowers the purity of ferrous oxalate. Furthermore, the resulting orthorhombic β-FeC₂O₄·2H₂O has inherent defects for preparing high-pressure lithium iron phosphate. In Comparative Example 3, omitting the pretreatment step significantly reduces the system's continuous leaching ability, resulting in a decrease in overall leaching rate and low ferrous oxalate purity. Analysis shows this is because the pretreatment roasting process avoids residual carbon layers hindering subsequent contact between DES and the active material, while simultaneously transforming the olivine phase LFP into a mixed phase structure that more easily complexes with DES for leaching, thus promoting leaching.
[0080] The above description is only a preferred embodiment of this application. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of this application, and these improvements and modifications should also be considered within the scope of protection of this application.
Claims
1. A method for value-added recovery of lithium iron phosphate black powder to prepare high-pressure lithium iron phosphate precursor, characterized in that, include: S1. Lithium iron phosphate black powder is calcined to obtain the calcined product; S2. The calcined product is mixed with a ternary eutectic solvent containing hydrogen bond acceptor component A, oxalic acid hydrogen bond donor component B and reducing agent component C for leaching reaction. The reaction product is separated into leaching residue and leaching liquid by solid-liquid separation. S3. The leaching residue is mixed with water and aged. After solid-liquid separation, washing and drying, ferrous oxalate dihydrate monoclinic crystal system is obtained. S4. Add phosphate to the leachate, react and then separate the solid and liquid to obtain the purified liquid and precipitate; S5. After the impurity removal liquid is acidified with an acidifying agent, an antisolvent is added to carry out a precipitation reaction. After solid-liquid separation, washing, and drying, lithium dihydrogen phosphate is obtained.
2. The method for preparing high-pressure lithium iron phosphate precursor by value-added recycling of lithium iron phosphate black powder as described in claim 1, characterized in that, In step S1, the calcination temperature is 400~800℃; the calcination time is 2~6 hours; the calcination is carried out in an air and / or oxygen atmosphere; and the carbon content of the obtained calcined product is ≤0.05%.
3. The method for value-added recovery and preparation of high-pressure lithium iron phosphate precursor by lithium iron phosphate black powder as described in claim 1, characterized in that, The hydrogen-bonded acceptor component A is at least one of choline compounds and guanidine salt compounds containing a quaternary ammonium salt structure; specifically, it includes at least one of choline derivatives and inorganic acid salt type guanidine compounds; preferably, it contains choline chloride. And / or, the oxalic acid hydrogen bond donor component B is oxalic acid and / or oxalic acid dihydrate, preferably solid oxalic acid dihydrate; And / or, the reducing agent component C is at least one of ascorbic acid, citric acid, aminocarboxylic acid, hydroxycarboxylic acid, and sulfonic acid, preferably ascorbic acid.
4. The method for value-added recovery and preparation of high-pressure lithium iron phosphate precursor by lithium iron phosphate black powder as described in claim 1, characterized in that, The molar ratio of the hydrogen bond acceptor component A to the oxalate hydrogen bond donor component B is 1:0.6 to 1:3, preferably 1:1 to 1:2; And / or, the molar ratio of the reducing agent component C to the hydrogen bond acceptor component A is 0.3:1 to 0.8:
1.
5. The method for value-added recovery and preparation of high-pressure lithium iron phosphate precursor by lithium iron phosphate black powder as described in claim 1, characterized in that, In step S2, the solid-liquid mass ratio of the leaching reaction is 1:5 to 1:20; And / or, in step S2, the temperature of the leaching reaction is 50~120℃; And / or, in step S2, the leaching reaction time is 0.5~8h; And / or, in step S2, the stirring speed of the leaching reaction is 100~600 rpm.
6. The method for value-added recovery and preparation of high-pressure lithium iron phosphate precursor by lithium iron phosphate black powder as described in claim 1, characterized in that, In step S3, the solid-liquid mass ratio of the aging treatment is 1:2 to 1:8; And / or, in step S3, the aging treatment temperature is 80~100℃; And / or, in step S3, the aging process takes 4 to 24 hours.
7. The method for value-added recovery and preparation of high-pressure lithium iron phosphate precursor by lithium iron phosphate black powder as described in claim 1, characterized in that, In step S4, the phosphate is sodium phosphate and / or sodium dihydrogen phosphate; And / or, in step S4, the reaction temperature is 20~80℃; And / or, in step S4, the reaction time is 0.5~3h; And / or, in step S4, the pH value of the purified solution is 3~4.
8. The method for value-added recovery and preparation of high-pressure lithium iron phosphate precursor by lithium iron phosphate black powder as described in claim 1, characterized in that, In step S5, the acidifying agent is phosphoric acid; And / or, in step S5, the antisolvent is at least one of C1-C4 alcohols, acetone, and dimethyl sulfoxide.
9. The method for value-added recovery and preparation of high-pressure lithium iron phosphate precursor by lithium iron phosphate black powder as described in claim 1, characterized in that, In step S5, the acidification treatment involves adjusting the pH of the reaction system to 2-3. And / or, in step S5, the volume ratio of the purified liquid to the antisolvent is 1:1 to 1:7; And / or, in step S5, the temperature of the precipitation reaction is 0~40℃.
10. The method for value-added recovery and preparation of high-pressure lithium iron phosphate precursor by lithium iron phosphate black powder as described in claim 1, characterized in that, Also includes: The liquid phase obtained from the solid-liquid separation in step S5 is distilled to remove and recover the antisolvent and water. Then, the lost components B and C are added to prepare a new ternary eutectic solvent for recycling.
Citation Information
Patent Citations
Method for selectively extracting lithium from waste lithium iron phosphate pole piece powder
CN122326973A
Method for preparing high-purity ferrous oxalate and high-purity lithium phosphate from waste lithium iron phosphate black powder and products thereof
CN122344134A
Method for recycling lithium from waste lithium iron phosphate battery
CN122444199A