A method for recycling and regenerating waste lithium iron phosphate cathode materials

By using a crystal-protected impurity removal solution of lithium salt and soluble phosphate under weak acid conditions, combined with staged redox control and quantitative lithium and phosphorus replenishment, the problem of lithium, phosphorus and iron loss caused by the removal of aluminum and copper impurities in the existing technology has been solved, and efficient regeneration and performance restoration of waste lithium iron phosphate cathode materials have been achieved.

CN123105582APending Publication Date: 2026-11-17CHIZHOU XIAOBU NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611170906.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-04
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies often result in the loss of lithium, phosphorus, and iron elements and damage to the crystal structure when removing aluminum and copper impurities from waste lithium iron phosphate cathode materials, making it difficult to achieve both efficient impurity removal and crystal protection simultaneously.

Method used

A crystal-protected impurity removal solution containing lithium salt and soluble phosphate was used to remove aluminum impurities first under weak acid conditions. Then, copper impurities were removed by adding oxidant in stages by controlling the redox potential. The crystal structure was restored by quantitative lithium and phosphorus supplementation. The electrochemical performance was restored by staged vacuum impregnation and heat treatment.

Benefits of technology

It effectively removes aluminum and copper impurities, reduces the loss of lithium, phosphorus and iron, restores the electrochemical performance and structural integrity of lithium iron phosphate, and improves the capacity and cycle stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105582A_ABST
    Figure CN123105582A_ABST
Patent Text Reader

Abstract

This invention discloses a method for recycling and regenerating waste lithium iron phosphate cathode materials, relating to the field of resource recovery and cathode material regeneration technology for waste lithium-ion batteries. The method involves pre-treating waste cathode sheets to obtain waste powder; adding the waste powder to a crystal protection and impurity removal solution containing lithium salt, soluble phosphate, and carboxylic acid complexing agents; first removing aluminum under non-oxidizing weak acid conditions; then removing copper by controlling the redox potential with an Ag / AgCl reference electrode and adding an oxidant in stages; after solid-liquid separation and gradient washing, the Li, Fe, and P contents are detected and quantitatively replenished; and after vacuum impregnation, granulation, and heat treatment in an inert or reducing atmosphere, regenerated lithium iron phosphate is obtained. The crystal protection and impurity removal solution simultaneously contains lithium ions and soluble phosphate, and through the common ion effect and liquid-solid phase balance adjustment, the dissolution of lithium, phosphorus, and iron elements in lithium iron phosphate under weak acid conditions is reduced, thus making the impurity removal process no longer solely dependent on reducing acidity to achieve crystal protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of resource recycling of waste lithium-ion batteries and regeneration of cathode materials, and particularly to a method for recycling and regenerating waste lithium iron phosphate cathode materials that removes aluminum and copper impurities while inhibiting the dissolution of lithium, phosphorus and iron elements in lithium iron phosphate and restoring the crystal structure and electrochemical performance of lithium iron phosphate. Background Technology

[0002] Lithium iron phosphate (LFP) cathode materials possess advantages such as high safety, long cycle life, good thermal stability, and low raw material cost, making them widely used in power batteries, energy storage batteries, and backup power supplies. With the large-scale retirement of LFP batteries, the resource recovery and direct regeneration of spent LFP cathode materials are gradually becoming an important technological direction in the field of lithium-ion battery recycling.

[0003] Waste lithium iron phosphate cathode materials typically originate from discarded cathode sheets that have undergone dismantling, crushing, stripping, or pulverizing. Because the cathode sheets use aluminum foil as the current collector, and negative electrode copper foil may be mixed in during battery dismantling, crushing, screening, and transportation, the recycled waste powder usually contains varying levels of aluminum and copper impurities. Furthermore, the waste powder may also contain residual binders, electrolyte decomposition products, conductive agents, fluorides, and surface carbonates.

[0004] Even low concentrations of aluminum and copper impurities remaining in recycled lithium iron phosphate materials can significantly impact subsequent battery performance. Aluminum impurities may form aluminum-containing crystalline phases or aluminum-rich interface regions during sintering, affecting particle interfaces and lithium-ion migration. Copper impurities may dissolve, migrate, and deposit during battery charging and discharging, inducing localized micro-short circuits, electrolyte decomposition, and reduced cycle life. Therefore, effective removal of aluminum and copper impurities is necessary before directly recycling spent lithium iron phosphate cathode materials.

[0005] Existing impurity removal processes typically employ inorganic acids, organic acids, complexing agents, or oxidizing agents to leach waste lithium iron phosphate powder. However, there is a clear contradiction between the efficiency of aluminum and copper impurity removal and the preservation of the lithium iron phosphate crystal structure.

[0006] On the one hand, increasing acidity, extending leaching time, or increasing leaching temperature can promote the dissolution of aluminum impurities, but it will also accelerate proton exchange and lattice dissolution on the surface of lithium iron phosphate, causing lithium, phosphorus, and iron elements to enter the liquid phase, resulting in the loss of effective components and damage to the olivine structure.

[0007] On the other hand, copper impurities are difficult to dissolve completely in weak acid and non-oxidizing environments. To improve copper removal rates, oxidants such as hydrogen peroxide and persulfate are usually added. However, strong oxidizing conditions can not only oxidize metallic copper but also destroy the Fe²⁺ in lithium iron phosphate. + Oxidized to Fe³ +This induces lithium iron phosphate delithiation, lattice distortion, formation of lithium-deficient phases such as FePO4, and dissolution of iron.

[0008] If acid, complexing agent, and oxidant are added simultaneously to treat aluminum and copper impurities in the same stage, the oxidant will act on the lithium iron phosphate particles before the aluminum impurities are fully dissolved, causing the impurity removal reaction and crystal destruction reaction to occur simultaneously. Although this type of process can achieve a high aluminum and copper removal rate, it is usually accompanied by a high loss of lithium, phosphorus, and iron. Even if lithium replenishment sintering is performed later, it is difficult to completely restore the original crystal integrity and cycle performance.

[0009] Some existing methods use mild organic acids to reduce the solubility of lithium iron phosphate, but under mild conditions, the aluminum oxide film and metallic copper are difficult to remove completely. Simply increasing the concentration of organic acid or complexing agent may enhance the complexation of iron ions, resulting in iron loss. Therefore, simply adjusting the type, concentration, or leaching temperature cannot fundamentally resolve the contradiction between impurity removal and crystal protection.

[0010] Furthermore, waste lithium iron phosphate particles are prone to surface pores and internal microcracks during long-term cycling and mechanical crushing. Conventional dry-process mixed lithium replenishment can only distribute the lithium replenishing agent on the outer surface of the particles, making it difficult to penetrate into the microcracks. This can easily lead to uneven local lithium concentration, local impurities, and insufficient regeneration. This defect may not be obvious in the initial capacity test, but under long-term cycling and high-rate charge-discharge conditions, it will manifest as increased interfacial impedance, particle pulverization, and accelerated capacity decay.

[0011] Therefore, there is an urgent need to provide a method for recycling and regenerating waste lithium iron phosphate cathode materials, which can improve the removal rate of aluminum and copper impurities, inhibit the leaching of lithium, phosphorus and iron elements, and restore the electrochemical performance of the recycled materials through component compensation and lattice repair. Summary of the Invention

[0012] The technical problem to be solved by this invention is: how to overcome the problem that improving the removal rate of aluminum and copper impurities in existing acid leaching or oxidative leaching processes will exacerbate the dissolution of lithium iron phosphate lattice and Fe²⁺. + The technical challenge of oxidation is to effectively remove aluminum and copper impurities while reducing the loss of lithium, phosphorus and iron elements, maintaining the olivine crystal structure of lithium iron phosphate, and improving the capacity, rate performance and cycle stability of recycled materials through quantitative component compensation and microcrack infiltration repair.

[0013] To achieve the above objectives, the present invention provides the following technical solution: a method for recycling and regenerating waste lithium iron phosphate cathode materials, comprising the following steps.

[0014] S1, waste lithium iron phosphate cathode sheets are discharged, disassembled, electrolyte removed, stripped and sieved to obtain waste powder containing lithium iron phosphate.

[0015] S2, the waste powder is added to a crystal protection and impurity removal solution containing lithium salt, soluble phosphate and carboxylic acid complexing agent, so that the lithium ion concentration in the liquid phase is 0.05-0.60 mol / L and the total phosphorus concentration is 0.02-0.40 mol / L.

[0016] The lithium salt and soluble phosphate provide a lithium ion and phosphate system that, through the common ion effect and liquid-solid phase equilibrium regulation, inhibits the dissolution of lithium and phosphorus elements from lithium iron phosphate into the liquid phase; the carboxylic acid complexing agent is used to complex aluminum ions released from aluminum foil debris, aluminum surface oxide layer or aluminum-containing impurities, so that aluminum impurities are kept in the liquid phase.

[0017] Without the addition of an oxidant, the first stage of leaching is carried out at a pH of 4.2–5.2 to preferentially remove aluminum impurities. When the change rate of liquid phase aluminum concentration in two consecutive adjacent detection intervals is no greater than 5%, the second stage of leaching is carried out directly; or solid-liquid separation is performed, and the resulting solid is redispersed in a crystal-protected impurity removal solution for the second stage of leaching.

[0018] In the second stage of leaching, the oxidant is added in stages, and the redox potential is maintained at 280-480 mV with a saturated potassium chloride Ag / AgCl reference electrode as a reference. The oxidant oxidizes metallic copper or low-valence copper into soluble copper ions, and then the carboxylic acid complexing agent forms a water-soluble complex with the copper ions, thereby removing copper impurities.

[0019] By limiting the timing of oxidant addition and the redox potential, the cumulative iron dissolution rate during the entire process of crystal protection, impurity removal, and washing is kept to no more than 1.0%.

[0020] S3. Solid-liquid separation and washing of the obtained impurity-free solid, determination of lithium, iron and phosphorus content in the impurity-free solid, addition of lithium source based on the determination results, and selective addition of iron source and / or phosphorus source based on the detection results, so that the Li / Fe molar ratio is 1.00-1.08 and the P / Fe molar ratio is 0.98-1.03.

[0021] S4. The replenished material is mixed with a carbon source and heat-treated under an inert or reducing atmosphere to obtain regenerated lithium iron phosphate cathode material.

[0022] Crystal protection and impurity removal mechanism In acidic aqueous solutions, the following simplified solid-liquid equilibrium may occur on the surface of lithium iron phosphate: LiFePO4(s) Li + (aq) + Fe² + (aq) + phosphate system (aq).

[0023] Under actual acidic conditions, the phosphate system may include H2PO4.- HPO4² - and a small amount of PO4³ - Pre-adding lithium ions and soluble phosphates to the liquid phase can increase the chemical potential of lithium and total phosphorus components in the liquid phase, shifting the surface dissolution equilibrium of lithium iron phosphate towards the solid phase and reducing the driving force for lithium and phosphorus to enter the liquid phase from the lithium iron phosphate lattice.

[0024] The common ion effect does not require that only PO4³ is present in the liquid phase. - Instead, it refers to increasing the concentration of lithium ions and total phosphorus components in the liquid phase to change the dissolution balance on the surface of lithium iron phosphate and the balance between different phosphate ions, thereby inhibiting the continuous dissolution of lithium iron phosphate.

[0025] No oxidant is added in the first stage of leaching, maintaining a relatively mild, non-oxidizing environment. Aluminum foil fragments, the aluminum surface oxide layer, and aluminum-containing impurities release aluminum ions under weakly acidic conditions. A carboxylic acid complexing agent forms soluble complexes with the aluminum ions, thereby promoting the dissolution of aluminum impurities. Because no oxidant is added, the Fe²⁺ content in lithium iron phosphate can be reduced. + Oxidized to Fe³ + The degree of.

[0026] In the second-stage leaching, the oxidant was added in stages, and the addition rate was adjusted based on the redox potential (RPP) monitoring results. When the RRP was below 280 mV, the oxidation kinetics of metallic copper were insufficient, leading to a decrease in copper removal rate; when the RRP was above 480 mV, the Fe²⁺ in lithium iron phosphate increased. + It is more easily oxidized, leading to the formation of lithium-deficient phases and increased iron dissolution. Therefore, controlling the redox potential between 280 and 480 mV can achieve a balance between copper oxidation removal and lithium iron phosphate lattice protection.

[0027] Preferred technical solution In a preferred embodiment, step S1 involves cleaning the waste lithium iron phosphate cathode sheet with dimethyl carbonate, diethyl carbonate, or ethyl acetate to remove residual electrolyte.

[0028] In a preferred embodiment, the stripped material is heat-treated at 350–450°C for 30–120 min under an inert atmosphere or vacuum to remove the adhesive and some organic residues.

[0029] In a preferred embodiment, the heat-treated material is crushed and graded to remove aluminum foil particles, copper foil particles and other metal particles with a particle size greater than 150 μm.

[0030] In a preferred embodiment, the lithium salt is selected from one or more of lithium dihydrogen phosphate, lithium sulfate, lithium acetate, and lithium nitrate.

[0031] In a preferred embodiment, the soluble phosphate is selected from one or more of lithium dihydrogen phosphate, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate.

[0032] When lithium dihydrogen phosphate is used, it can be used as both a lithium salt and a soluble phosphate, but the lithium ion concentration and total phosphorus concentration in the liquid phase should be calculated separately based on the amount of lithium ions and total phosphorus it provides.

[0033] In a preferred embodiment, the carboxylic acid complexing agent is selected from one or more of citrate, tartrate, malate and ethylenediaminetetraacetic acid, and its concentration in the crystal protection and impurity removal solution is 0.02 to 0.20 mol / L.

[0034] In a preferred embodiment, during the first stage of leaching, the solid-liquid ratio of waste powder to crystal protection and impurity removal solution is 1g:5-15mL, the leaching temperature is 35-65℃, and the leaching time is 20-90min.

[0035] In a preferred embodiment, the pH of the first-stage leaching is maintained at 4.4 to 5.0 by adding citric acid, acetic acid, or ammonium dihydrogen phosphate.

[0036] In a preferred embodiment, during the first stage of leaching, the liquid aluminum concentration is monitored every 5–15 minutes. The rate of change of liquid aluminum concentration between two consecutive measurements is calculated using the following formula: Liquid aluminum concentration change rate = |CAl,n-CAl,n-1| / CAl,n-1×100%.

[0037] In the formula, CA1,n represents the liquid aluminum concentration in the nth detection, and CA1,n-1 represents the liquid aluminum concentration in the previous detection.

[0038] When the change rate of liquid phase aluminum concentration in two consecutive tests is no greater than 5%, it is determined that the aluminum impurities have reached a state of full dissolution.

[0039] In a preferred embodiment, the second stage of leaching is carried out directly in the same reaction vessel after the first stage of leaching is completed.

[0040] In another preferred embodiment, after the first stage of leaching is completed, solid-liquid separation is performed to remove the aluminum-containing leaching solution, and then the resulting solid is redispersed in a newly prepared crystal protection and impurity removal solution for the second stage of leaching.

[0041] In a preferred embodiment, the oxidant is selected from one or more of hydrogen peroxide, ammonium persulfate, and sodium persulfate.

[0042] In a preferred embodiment, a saturated potassium chloride Ag / AgCl reference electrode is used to detect the redox potential, and the addition rate of the oxidant is adjusted in a closed loop according to the detection value to maintain the redox potential of the second stage leaching at 320-430mV.

[0043] In a preferred embodiment, the temperature of the second stage leaching is 25–55°C, and the time is 10–60 min.

[0044] In a preferred embodiment, the copper and iron content in the liquid phase is detected every 5 to 15 minutes. When the change rate of the liquid phase copper content in two consecutive tests is not greater than 5% and the copper impurity removal rate is not less than 95%, the addition of oxidant is stopped, and solid-liquid separation is completed within 10 minutes after the addition of oxidant is stopped.

[0045] Redox potential control optimization Considering that the crystal protection and impurity removal solution contains solid particles, carboxylic acid complexing agents, residual conductive carbon and a small amount of organic matter, when a common laboratory redox potential electrode is directly immersed in the slurry for a long time, measurement errors may occur due to particle adhesion, electrode surface contamination, response hysteresis or reference drift.

[0046] In a preferred embodiment, an industrial redox potential electrode with automatic cleaning, automatic calibration, and temperature compensation functions is employed. The electrode can be placed in the low-shear measurement zone within the reactor, or in a circulation bypass measurement unit connected to the reactor. A protective sleeve is provided outside the electrode to allow liquid phase passage while blocking direct impact from larger particles.

[0047] Before the reaction begins, the electrodes are calibrated using a standard redox buffer solution. During the reaction, the electrode surfaces are pulse-washed with deionized water or a cleaning solution compatible with the crystal protection and impurity removal solution according to a set cycle. When the measurement difference between the two parallel redox potential electrodes exceeds 20mV, the control system initiates the cleaning and verification procedure.

[0048] The oxidant addition system preferably consists of a metering pump, a flow meter, and a controller. The controller uses a proportional-integral-derivative control algorithm to adjust the instantaneous pumping rate of the oxidant.

[0049] To reduce overshoot caused by redox potential signal lag, a preferred embodiment employs a control strategy combining feedforward and feedback. First, the basic addition rate is estimated based on the initial copper impurity content in the waste powder, the target copper removal rate, and the theoretical equivalent of the oxidant. Then, the basic addition rate is fine-tuned based on the real-time feedback results of the redox potential.

[0050] When the redox potential approaches the upper limit of the set value, reduce the oxidant pumping rate; when the redox potential exceeds the upper limit of the set value, stop adding oxidant; when the redox potential drops below the lower limit of the set value, resume low-speed addition.

[0051] By employing the above control methods, the redox potential fluctuation range during the second-stage leaching process can be controlled within ±10mV of the set value, thereby reducing local excess of oxidant and Fe²⁺. + Risk of excessive oxidation.

[0052] Impurity removal and elemental loss calculation The aluminum impurity removal rate is calculated using the following formula: Aluminum impurity removal rate = (mAl,0 - mAl,1) / mAl,0 × 100%.

[0053] In the formula, mAl,0 is the mass of aluminum in the waste powder before treatment, and mAl,1 is the mass of residual aluminum in the purified solid.

[0054] The copper impurity removal rate is calculated using the following formula: Copper impurity removal rate = (mCu,0 - mCu,1) / mCu,0 × 100%.

[0055] In the formula, mCu,0 is the mass of copper in the waste powder before treatment, and mCu,1 is the mass of residual copper in the purified solid.

[0056] The lithium loss rate and phosphorus loss rate are calculated according to the following formulas: Element loss rate = mE,L / mE,0 × 100%.

[0057] In the formula, mE,L is the total mass of the corresponding elements in the first-stage leachate, the second-stage leachate, and the washing solution, and mE,0 is the total mass of the corresponding elements in the waste powder before treatment.

[0058] The cumulative iron dissolution rate during the second stage of copper impurity removal is calculated using the following formula: The cumulative iron dissolution rate in the second stage = mFe,2 / mFe,0 × 100%.

[0059] In the formula, mFe,2 is the total mass of iron in the leachate of the second stage, and mFe,0 is the total mass of iron in the waste powder before treatment.

[0060] In performance evaluation, a more stringent method can be used: the cumulative iron dissolution rate throughout the entire impurity removal process. Cumulative iron dissolution rate during the entire impurity removal process = mFe,L / mFe,0 × 100%.

[0061] In the formula, mFe,L is the sum of the mass of iron in the first-stage leachate, the second-stage leachate, and the washing solution.

[0062] In a preferred embodiment, the cumulative iron dissolution rate in the second stage is no greater than 1.0%; more preferably, the cumulative iron dissolution rate throughout the entire impurity removal process is also no greater than 1.0%.

[0063] Gradient washing In a preferred embodiment, step S3 employs a gradient washing method, first washing the impurity-removing solids with a lithium dihydrogen phosphate solution with a concentration of 0.01–0.10 mol / L and a pH of 5.5–6.5, and then washing with deionized water until the conductivity of the final washing solution is no greater than 500 μS / cm.

[0064] Using lithium dihydrogen phosphate solution for the first stage of washing can reduce secondary dissolution caused by the sudden drop in the concentration of lithium and phosphorus in the liquid phase during the initial washing stage; deionized water is then used to remove residual salts and complexing agents.

[0065] Ingredient compensation In a preferred embodiment, the lithium, iron, and phosphorus content in the purified solid is determined by inductively coupled plasma atomic emission spectrometry.

[0066] In a preferred embodiment, the lithium source is selected from one or more of lithium carbonate, lithium hydroxide, and lithium acetate.

[0067] In a preferred embodiment, the iron source is selected from one or more of ferrous oxalate, ferric phosphate, and ferrous oxide.

[0068] In a preferred embodiment, the phosphorus source is selected from one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and phosphoric acid.

[0069] In a preferred embodiment, the Li / Fe molar ratio after replenishment is 1.02 to 1.05, and the P / Fe molar ratio is 0.995 to 1.015.

[0070] Vacuum impregnation operation optimization In a preferred embodiment, a lithium source, as well as an iron source and / or a phosphorus source, are dissolved or dispersed in a mixed solvent of water and ethanol to form a replenishing solution, wherein the volume ratio of water to ethanol is 1:0.2 to 2.

[0071] After mixing the impurity-removing solid with the replenishing solution, the mixture is impregnated for 10 to 60 minutes under a vacuum of -0.060 to -0.095 MPa, allowing the replenishing solution to penetrate the surface pores and microcracks of the impurity-removing solid particles. After vacuum impregnation, the resulting slurry is spray-dried and granulated at an outlet temperature of 80 to 140°C.

[0072] Considering that the mixed solvent of water and ethanol may boil rapidly under vacuum conditions, in a preferred embodiment, the vacuum impregnation process is carried out in a closed vacuum impregnation tank equipped with a condensation recovery device.

[0073] The material loading volume of the vacuum impregnation tank shall not exceed 70% of its effective volume to allow space for foam and solvent vapor. During the impregnation process, the material temperature shall be maintained at 20-30°C, and the solvent boiling rate shall be controlled by gradually reducing the pressure inside the tank.

[0074] Phased reduction of vacuum can include: In the first stage, the vacuum level is reduced to -0.020 to -0.040 MPa and maintained for 3 to 10 minutes; In the second stage, the vacuum level is reduced to -0.050 to -0.070 MPa and maintained for 5 to 15 minutes. In the third stage, the vacuum level is reduced to the target vacuum level of -0.060 to -0.095 MPa and maintained until the set immersion time ends.

[0075] When the foam height inside the tank reaches the preset upper limit, the control system pauses vacuuming or briefly introduces inert gas to reduce the foam height and prevent slurry from overflowing or splashing.

[0076] Water and ethanol vapors generated during the impregnation process are condensed and recovered by a condenser. After the target impregnation time is reached, nitrogen gas is preferably slowly introduced to restore the pressure inside the tank to atmospheric pressure. Vacuum extraction removes gas from the pores and microcracks of the particles, while the pressure difference generated when atmospheric pressure is restored further propels the replenishing solution into the interior of the particles.

[0077] Carbon coating and heat treatment In a preferred embodiment, the carbon source is selected from one or more of glucose, sucrose, citric acid, polyethylene glycol and asphalt, and its addition amount is 2 to 8% of the mass of the supplemented material.

[0078] In a preferred embodiment, the heat treatment includes first holding at 300–450°C for 1–3 hours, and then raising the temperature to 650–750°C and holding for 2–8 hours.

[0079] The first stage of low-temperature heat treatment is used to decompose organic matter, carbon sources and additives, and to reduce concentrated gas release in the subsequent high-temperature stage; the second stage of high-temperature heat treatment is used to restore the lithium iron phosphate olivine structure, promote the entry of added elements into the crystal lattice and form a carbon coating layer.

[0080] In a preferred embodiment, the heat treatment atmosphere is nitrogen containing 1-5 vol% hydrogen, and the carbon content in the resulting recycled lithium iron phosphate cathode material is 1-4 wt%.

[0081] Compared with the prior art, the present invention provides a method for recycling and regenerating waste lithium iron phosphate cathode materials, which has the following beneficial effects: lithium ions and soluble phosphates are simultaneously set in the crystal protection and impurity removal solution. Through the common ion effect and liquid-solid phase balance adjustment, the dissolution of lithium, phosphorus and iron elements in lithium iron phosphate under weak acid conditions is reduced, so that the impurity removal process no longer relies solely on reducing acidity to achieve crystal protection.

[0082] This invention divides the impurity removal process into a first stage of aluminum removal without the addition of an oxidant and a second stage of copper removal with the addition of a controlled oxidant, thus avoiding prolonged exposure of lithium iron phosphate to an oxidizing environment before aluminum impurities have been fully dissolved.

[0083] This invention uses a saturated potassium chloride (Ag / AgCl) reference electrode as a reference to detect the redox potential in real time. It employs a combination of feedforward and feedback control to adjust the oxidant addition rate, ensuring the redox potential is sufficient to oxidize copper without causing Fe²⁺ in lithium iron phosphate to degrade. + Inside the window where a large amount of oxidation occurs.

[0084] The redox potentials described in this invention are all potential values ​​measured at actual reaction temperatures using a saturated potassium chloride Ag / AgCl electrode as a reference. The examples and comparative examples use the same type of reference electrode and the same calibration method.

[0085] The present invention enables a synergistic improvement in impurity removal rate and lattice protection, under the condition that the copper impurity removal rate is not less than 95%, from the time the waste powder is added to the crystal protection impurity removal solution to the end of the solid-liquid separation, the cumulative amount of iron dissolved in all liquid phases (including the first stage leaching solution, the second stage leaching solution and the washing solution) is not greater than 1.0% of the initial iron content of the waste powder.

[0086] This invention uses lithium dihydrogen phosphate solution and deionized water for gradient washing to reduce secondary delithiation and phosphorus loss of impurity solids during the washing stage.

[0087] This invention provides quantitative replenishment based on the actual lithium, iron, and phosphorus content of the material after impurity removal, thus avoiding the problem that a fixed amount of lithium replenishment cannot adapt to the fluctuations in the composition of waste materials from different sources.

[0088] This invention employs a staged depressurization vacuum impregnation method, which allows the replenishing solution to enter the pores and microcracks of the particles, and reduces the violent boiling of the ethanol-water mixed solvent, slurry splashing, and solvent loss.

[0089] This invention restores the olivine crystal structure and particle conductive network of lithium iron phosphate through segmented heat treatment and in-situ carbon coating, enabling the recycled material to have high initial discharge specific capacity, rate performance and cycle retention. Attached Figure Description

[0090] Figure 1This is a FIB-SEM cross-sectional view of the recycled material in Embodiment 2 of the present invention; Figure 2 This is a HAADF-STEM elemental distribution diagram of the recycled material in Embodiment 2 of the present invention; Figure 3 This is the HRTEM lattice stripe pattern of the recycled material in Embodiment 2 of the present invention. Detailed Implementation

[0091] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0092] Please see Figures 1-3 This invention provides a technical solution for recycling and regenerating waste lithium iron phosphate cathode materials: Without causing technical conflicts, the technical features in the various embodiments can be combined with each other. Unless otherwise stated, all raw materials used are industrial-grade or analytical-grade reagents, and the water used is deionized water. All concentrations refer to the liquid phase concentration after preparation.

[0093] Waste lithium iron phosphate raw materials All embodiments and comparative examples used the same batch of retired power-type lithium iron phosphate battery cathode sheets as raw materials.

[0094] After the positive electrode sheets were safely discharged and disassembled, samples from the same batch were mixed thoroughly. Preliminary analysis revealed the main components of the original waste powder obtained from the stripping of the positive electrode active layer, as shown in Table 1.

[0095] Table 1 Composition of raw waste lithium iron phosphate powder

[0096] To reduce the impact of raw material fluctuations on experimental results, the waste powder from the same batch was thoroughly mixed and then divided into quarters. 1000g of dry-basis waste powder was used for processing in each example and comparative example.

[0097] The second-stage leaching of each group uses an industrial redox potential electrode with automatic rinsing and temperature compensation functions, and the oxidant metering pump is adjusted using a feedforward-PID feedback control method. Unless otherwise specified, the redox potential fluctuation is controlled within ±10mV of the set value.

[0098] Each group of vacuum impregnation was carried out in a closed vacuum impregnation tank equipped with a condensation recovery device. The material loading volume was 60% of the effective volume of the tank, the slurry temperature was controlled at 25±2℃, and the vacuum degree was reduced in stages.

[0099] Example 1 1. Preprocessing The waste lithium iron phosphate cathode sheet was immersed in dimethyl carbonate for 20 minutes each time to remove residual electrolyte.

[0100] The positive electrode active layer was mechanically stripped and heat-treated at 350℃ for 30 minutes under a nitrogen atmosphere. After cooling, it was crushed and sieved using a 150μm screen to remove aluminum foil, copper foil, and other metal particles with a particle size greater than 150μm, resulting in waste powder.

[0101] 2. First stage aluminum removal Prepare a crystal protection and impurity removal solution with a lithium ion concentration of 0.05 mol / L, a total phosphorus concentration of 0.02 mol / L, and a citrate concentration of 0.02 mol / L. Lithium ions are provided by lithium nitrate, and total phosphorus is provided by ammonium dihydrogen phosphate.

[0102] Add the waste powder and crystal protection and impurity removal solution to the reactor at a solid-liquid ratio of 1g:5mL, adjust the pH to 4.2, stir at 35℃ for 20min, and do not add oxidant.

[0103] The liquid phase aluminum concentration is sampled and measured every 5 minutes. The first stage of aluminum removal is completed when the change rate of liquid phase aluminum concentration in two consecutive measurements is no greater than 5%.

[0104] 3. Second stage copper removal Without performing intermediate solid-liquid separation, the system temperature was adjusted to 25°C, and hydrogen peroxide solution was added in portions.

[0105] The initial feedforward addition rate of hydrogen peroxide is calculated based on the copper content in the waste powder, and then the addition rate is finely adjusted by PID feedback control to maintain the oxidation-reduction potential at 280±10mV.

[0106] The reaction was carried out for 10 minutes, and the concentrations of copper and iron in the liquid phase were checked every 5 minutes. When the removal rate of copper impurities was not less than 95% and the change rate of copper concentration in the liquid phase was not greater than 5% for two consecutive times, the addition of oxidant was stopped, and solid-liquid separation was completed within 10 minutes.

[0107] 4. Washing and ingredient replenishment First, wash the solid with a 0.01 mol / L lithium dihydrogen phosphate solution at pH 5.5 to remove impurities, then wash with deionized water until the conductivity of the final wash solution is no greater than 500 μS / cm.

[0108] The lithium, iron, and phosphorus contents in the purified solid were determined, and lithium hydroxide and phosphoric acid were added to make the Li / Fe molar ratio 1.00 and the P / Fe molar ratio 0.98 after replenishment.

[0109] 5. Vacuum impregnation and heat treatment Lithium hydroxide and phosphoric acid were prepared in a mixed solvent of water and ethanol at a volume ratio of 1:0.2 to form a replenishing solution.

[0110] Add the impurity-removed solid to the replenishing solution, first reduce the vacuum to -0.030 MPa and maintain it for 3 min, then reduce it to -0.050 MPa and maintain it for 5 min, and finally reduce it to -0.060 MPa and maintain it for 10 min. After impregnation, slowly introduce nitrogen gas to restore the pressure to atmospheric pressure.

[0111] The material was dried at 80℃ and spray-granulated. 2% glucose (by weight of the replenished material) was added as a carbon source. Under a nitrogen atmosphere containing 1 vol% hydrogen, the material was first held at 300℃ for 1 hour, then heated to 650℃ and held for 2 hours, followed by natural cooling to obtain recycled lithium iron phosphate material with a residual carbon content of 1.02 wt%.

[0112] Example 2 The positive electrode was cleaned with ethyl acetate, heat-treated at 400℃ for 60 min under vacuum, and then sieved using a 150μm sieve.

[0113] The concentration of lithium ions in the crystal protection and impurity removal solution is 0.30 mol / L, the concentration of total phosphorus is 0.20 mol / L, and the concentration of citrate is 0.08 mol / L. Lithium ions are provided by lithium sulfate and lithium dihydrogen phosphate, and total phosphorus is provided by lithium dihydrogen phosphate.

[0114] The solid-liquid ratio of waste powder to crystal protection and impurity removal solution is 1g:10mL. The first stage leaching is carried out at pH 4.7, temperature 50℃, and time 60min, without the addition of oxidant.

[0115] If the change rate of liquid aluminum concentration is no greater than 5% in two consecutive tests, solid-liquid separation is not performed, and the temperature is lowered to 40℃.

[0116] An oxidant feedforward addition curve was established based on the copper content and theoretical equivalent of hydrogen peroxide in the waste powder. The hydrogen peroxide addition rate was adjusted by PID feedback control to maintain the redox potential at 380±10mV. The second leaching stage lasted 30 minutes, with copper and iron concentrations monitored every 10 minutes.

[0117] The impurity-removing solids were first washed with a 0.05 mol / L lithium dihydrogen phosphate solution at pH 6.0, and then washed with deionized water until the conductivity of the final wash solution was 328 μS / cm.

[0118] Based on the test results, lithium carbonate and ferrous oxalate were added to make the Li / Fe molar ratio 1.04 and the P / Fe molar ratio 1.005.

[0119] The supplementary agent was dispersed in a mixed solvent of water and ethanol in a volume ratio of 1:1. The vacuum was first reduced to -0.030 MPa and maintained for 5 min, then reduced to -0.060 MPa and maintained for 10 min, and finally reduced to -0.080 MPa and maintained for 30 min. The solvent vapor generated during the impregnation process was condensed and recovered. After impregnation, nitrogen gas was slowly introduced to restore the pressure to atmospheric pressure.

[0120] The material was dried at 110℃ and spray-granulated. Sucrose at 5% of the mass of the supplemented material was added as a carbon source. Under a nitrogen atmosphere containing 3 vol% hydrogen, the material was first kept at 380℃ for 2 hours, and then heated to 700℃ for 5 hours to obtain recycled lithium iron phosphate material with a residual carbon content of 2.21 wt%.

[0121] Example 3 The positive electrode was cleaned with diethyl carbonate, heat-treated at 450℃ for 120 min under nitrogen atmosphere, and then sieved using a 150μm sieve.

[0122] The concentration of lithium ions in the crystal protection and impurity removal solution is 0.60 mol / L, the concentration of total phosphorus is 0.40 mol / L, and the concentration of ethylenediaminetetraacetate is 0.20 mol / L. Lithium ions are provided by lithium acetate, and total phosphorus is provided by diammonium hydrogen phosphate.

[0123] The solid-liquid ratio of waste powder to crystal protection and impurity removal solution is 1g:15mL. The first stage leaching is carried out at pH 5.2, temperature 65℃, and time 90min, without the addition of oxidant.

[0124] After the aluminum impurities were fully dissolved, sodium persulfate was added directly in portions to maintain the redox potential at 480±10mV. The second stage of leaching was carried out at 55℃ for 60 minutes, with copper and iron concentrations measured every 15 minutes.

[0125] The sample was washed with a 0.10 mol / L lithium dihydrogen phosphate solution at pH 6.5, and then washed with deionized water until the conductivity of the final wash solution was 296 μS / cm.

[0126] Lithium acetate and iron phosphate were added to make the Li / Fe molar ratio 1.08 and the P / Fe molar ratio 1.03.

[0127] The vacuum degree was successively reduced to -0.035MPa, -0.065MPa and -0.095MPa, and the sample was immersed at the target vacuum degree for 60 min, dried at 140℃ and spray granulated.

[0128] Add asphalt at 8% of the mass of the supplemented material as a carbon source, and in a nitrogen atmosphere containing 5 vol% hydrogen, first heat at 450℃ for 3 hours, then heat to 750℃ for 8 hours to obtain recycled lithium iron phosphate material with a residual carbon content of 3.96 wt%.

[0129] Example 4 The positive electrode was cleaned with ethyl acetate and then heat-treated at 380°C for 45 min under vacuum.

[0130] The concentrations of lithium ions, total phosphorus, and tartrate in the crystal protection and impurity removal solution were 0.15 mol / L, 0.08 mol / L, and 0.05 mol / L, respectively. Lithium ions were provided by lithium sulfate, and total phosphorus by ammonium dihydrogen phosphate.

[0131] The solid-liquid ratio was 1g:8mL, and the first stage leaching was carried out at a pH of 4.4, a temperature of 42℃, and a time of 40min.

[0132] After the aluminum impurities were fully dissolved, the temperature was adjusted to 25℃, and ammonium persulfate was added in portions to maintain the redox potential at 320±10mV. The second leaching stage lasted 10 minutes, and the concentrations of copper and iron were checked every 5 minutes.

[0133] After washing, lithium carbonate, ferrous oxalate, and ammonium dihydrogen phosphate were added to make the Li / Fe molar ratio 1.02 and the P / Fe molar ratio 0.995.

[0134] The material was impregnated under a vacuum of -0.060 MPa for 10 min and dried at 80 °C. Citric acid, accounting for 2% of the mass of the replenished material, was added as a carbon source. The material was then heated at 300 °C for 1 h and then at 650 °C for 2 h under a nitrogen atmosphere containing 1 vol% hydrogen. The residual carbon content of the resulting material was 1.08 wt%.

[0135] Example 5 The positive electrode was cleaned with diethyl carbonate and then heat-treated at 430°C for 100 min under a nitrogen atmosphere.

[0136] The concentrations of lithium ions, total phosphorus, and malate in the crystal protection and impurity removal solution were 0.50 mol / L, 0.35 mol / L, and 0.15 mol / L, respectively. Lithium ions were provided by lithium acetate, and total phosphorus was provided by diammonium hydrogen phosphate.

[0137] The solid-liquid ratio was 1g:14mL, and the first stage leaching was carried out at a pH of 5.0, a temperature of 60℃, and a time of 80min.

[0138] After the aluminum impurities were fully dissolved, the temperature was adjusted to 55℃, and sodium persulfate was added in portions to maintain the redox potential at 430±10mV. The second leaching stage lasted 60 minutes, and the concentrations of copper and iron were measured every 15 minutes.

[0139] After washing, lithium acetate and iron phosphate were added to make the Li / Fe molar ratio 1.05 and the P / Fe molar ratio 1.015.

[0140] The material was impregnated under a vacuum of -0.095 MPa for 60 min and dried at 140 °C. A mixed carbon source of polyethylene glycol and asphalt, accounting for 8% of the mass of the supplemented material, was added. The mixture was then heated at 450 °C for 3 h and then at 750 °C for 8 h under a nitrogen atmosphere containing 5 vol% hydrogen. The residual carbon content of the resulting material was 3.91 wt%.

[0141] Example 6 The positive electrode was cleaned with dimethyl carbonate and then heat-treated at 410℃ for 75 min under vacuum conditions.

[0142] The first-stage crystal protection and impurity removal solution contains 0.35 mol / L lithium ions, 0.22 mol / L total phosphorus, and 0.03 mol / L ethylenediaminetetraacetic acid (EDTA). Lithium ions are supplied by both lithium nitrate and lithium dihydrogen phosphate, while total phosphorus is supplied by lithium dihydrogen phosphate.

[0143] The solid-liquid ratio was 1g:10mL, the pH was 4.6, the temperature was 48℃, and the leaching time was 55min.

[0144] After the aluminum impurities are fully dissolved, solid-liquid separation is performed, followed by washing with a small amount of crystal-protecting and impurity-removing solution of the same composition. The resulting solid is then redispersed in a freshly prepared crystal-protecting and impurity-removing solution.

[0145] In the second stage, hydrogen peroxide was added in portions, and the redox potential was maintained at 390±10mV at 42℃ for leaching for 35 minutes.

[0146] After washing, lithium hydroxide, ferrous oxide, and phosphoric acid were added to make the Li / Fe molar ratio 1.035 and the P / Fe molar ratio 1.010.

[0147] The material was impregnated under a vacuum of -0.085 MPa for 40 min and dried at 120 °C. A mixed carbon source of glucose and polyethylene glycol, accounting for 4.5% of the mass of the replenished material, was added. The mixture was then heated at 400 °C for 2 h and then at 710 °C for 4 h under a nitrogen atmosphere containing 2.5 vol% hydrogen. The resulting material had a residual carbon content of 2.35 wt%.

[0148] Comparative Example 1 differs only in that lithium sulfate or other lithium salts are not added to the crystal protection and impurity removal solution. Ammonium dihydrogen phosphate is used to provide a total phosphorus concentration of 0.20 mol / L, and the citrate concentration, pH, and other process conditions are the same as in Example 2.

[0149] Comparative Example 2 differs only in that lithium dihydrogen phosphate or other soluble phosphates are not added to the crystal protection and impurity removal solution. Lithium sulfate is used to maintain the lithium ion concentration at 0.30 mol / L, and the citrate concentration, pH, and other process conditions are the same as in Example 2.

[0150] Comparative Example 3 differs only in that citrate or other carboxylic acid complexing agents are not added to the crystal protection and impurity removal solution. The pH of the system is maintained at 4.7 using dilute sulfuric acid, and the lithium ion concentration, total phosphorus concentration, and other process conditions are the same as in Example 2.

[0151] Comparative Example 4 differs only in that all hydrogen peroxide is added in stages from the start of the first stage of leaching, and the redox potential is maintained at 380±10 mV throughout the entire reaction process in both the first and second stages. The total amount of oxidant and the total reaction time are the same as in Example 2.

[0152] Comparative Example 5 differed only in that the redox potential of the second-stage leaching was maintained at 240±10mV. Other conditions were the same as in Example 2.

[0153] Comparative Example 6 differed only in that the redox potential of the second-stage leaching was maintained at 520±10mV. Other conditions were the same as in Example 2.

[0154] Comparative Example 7 differs only in that step S3 does not involve adding lithium, iron, and / or phosphorus sources based on the measurement results. After the impurity-removed solids undergo the same washing process, carbon source is added directly in the same mass ratio as in Example 2, and the same heat treatment is performed.

[0155] Comparative Example 8 differed only in that the replenishing solution and the impurity-removing solid were stirred and impregnated at atmospheric pressure for 30 minutes, without vacuum impregnation at -0.080 MPa. Other conditions were the same as in Example 2.

[0156] Performance testing methods 1. Element content and impurity removal rate test The contents of lithium, iron, phosphorus, aluminum and copper were determined in accordance with GB / T 30902—2014 "Determination of impurity elements in inorganic chemical products by inductively coupled plasma optical emission spectrometry (ICP-OES)".

[0157] Solid samples were digested in a closed system using nitric acid, hydrochloric acid, and a suitable amount of hydrofluoric acid, and then analyzed by ICP-OES after being brought to a final volume. Liquid samples were analyzed after acidification and dilution.

[0158] Based on the aforementioned calculation formula, the aluminum impurity removal rate, copper impurity removal rate, lithium loss rate, phosphorus loss rate, cumulative iron dissolution rate in the second stage, and cumulative iron dissolution rate throughout the entire impurity removal process are calculated respectively.

[0159] The cumulative iron leaching rate listed in Table 2 adopts a more stringent cumulative iron leaching rate throughout the entire impurity removal process, which is the ratio of the sum of the iron element mass in the first-stage leachate, the second-stage leachate, and the washing solution to the total iron element mass in the original waste powder.

[0160] 2. Phase and lattice structure testing Phase analysis was performed in accordance with GB / T 30904—2014 "X-ray diffraction method for crystal structure analysis of inorganic chemical products".

[0161] Cu Kα radiation was used, with a tube voltage of 40 kV and a tube current of 40 mA. The scanning range was 10° to 80° and the scanning speed was 2° / min.

[0162] The full-spectrum fitting method was used to perform semi-quantitative or quantitative analysis on the XRD-resolvable crystal phases, and to calculate the relative contents of the olivine-type LiFePO4 main crystal phase and XRD-resolvable crystal phases such as FePO4, Li3PO4, and Fe2O3.

[0163] The "LiFePO4 main crystalline phase content" and "total amount of XRD-resolvable crystalline and impurity phases" in this specification refer to the relative content obtained after normalization within the range of crystalline phases that can be identified and fitted by XRD, and are not equivalent to the actual total material composition of the sample.

[0164] X-ray diffraction (XRD) is insensitive to trace amounts of crystalline phases, phases with low crystallinity, and amorphous phases. Carbon coatings, amorphous residues, and trace substances below the detection or fitting reliability limit are not included in the total amount of XRD-resolvable crystalline and impurity phases. Therefore, this index is used to compare the crystalline phase integrity of each sample, not to characterize the total impurity content in the sample.

[0165] 3. Iron price status test The surface valence state of iron was determined in accordance with GB / T 19500—2025, "General Rules for X-ray Photoelectron Spectroscopy Analysis".

[0166] Fe²⁺ was calculated using peak fitting of the Fe 2p spectrum. + The proportion of the total iron surface signal. All samples were subjected to the same background subtraction, peak shape, and constraint conditions.

[0167] 4. Particle size testing Particle size distribution was determined according to GB / T 19077-2024 "Particle Size Distribution by Laser Diffraction".

[0168] D10, D50 and D90 were measured using ethanol as the dispersion medium under the same ultrasonic time and circulation rate.

[0169] 5. Specific surface area test Specific surface area was determined according to GB / T 19587—2017 "Determination of Specific Surface Area of ​​Solid Substances by Gas Adsorption BET Method".

[0170] The sample was degassed under vacuum at 150℃ for 4 hours, and the BET specific surface area was determined using nitrogen as the adsorbed gas.

[0171] 6. Carbon content test The carbon content was tested according to the carbon content test method in GB / T 30835—2014 "Carbon Composite Lithium Iron Phosphate Cathode Materials for Lithium-ion Batteries".

[0172] 7. Electrochemical performance testing Electrochemical performance was tested in accordance with the relevant test methods of GB / T 30835—2014 "Carbon Composite Lithium Iron Phosphate Cathode Materials for Lithium-ion Batteries", and the following sample preparation conditions were uniformly adopted.

[0173] Recycled lithium iron phosphate material, conductive carbon black, and polyvinylidene fluoride were mixed in a mass ratio of 80:10:10, and a slurry was prepared using N-methylpyrrolidone as a solvent. The slurry was uniformly coated onto aluminum foil, vacuum dried, and then rolled and stamped.

[0174] CR2032 button cells were assembled in an argon glove box, with lithium metal sheets as the counter electrode, polyolefin membranes as the separators, and a 1 mol / L LiPF6 mixed solution of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate.

[0175] The test temperature is 25±2℃, and the charge / discharge voltage range is 2.0~3.8V.

[0176] The 0.1C first discharge specific capacity test includes: charging to 3.8V at 0.1C, then charging at constant voltage until the current drops to 0.02C, letting stand for 10 minutes, and then discharging to 2.0V at 0.1C.

[0177] The initial coulombic efficiency is calculated as the ratio of the initial discharge capacity to the initial charge capacity.

[0178] Rate performance was tested sequentially at 0.1C, 0.5C, 1C, 2C and 5C, with each rate cycled for 5 weeks, and the discharge specific capacity of the last week of the corresponding rate was taken.

[0179] Cycling performance is measured at 1C charge and 1C discharge for 500 cycles. Capacity retention is calculated as the ratio of the discharge capacity at cycle 500 to the discharge capacity at cycle 3.

[0180] Test Results Table 2. Test results of impurity removal rate and elemental loss.

[0181] As shown in Table 2, the aluminum removal rate of Examples 1 to 6 was 95.6% to 99.2%, and the copper removal rate was 95.1% to 99.0%. Meanwhile, the cumulative iron dissolution rate of the entire impurity removal process calculated using a more stringent statistical method was no more than 1.0%.

[0182] The lithium loss rate of Example 2 was 0.72%, the phosphorus loss rate was 0.48%, and the cumulative iron dissolution rate was 0.36%, indicating that the preferred intermediate region has a better crystal protection effect.

[0183] In Comparative Example 1, removing only lithium salt increased the lithium loss rate to 6.42% and the cumulative iron dissolution rate to 2.31%; in Comparative Example 2, removing only soluble phosphate increased the phosphorus loss rate to 6.08% and the cumulative iron dissolution rate to 2.58%. These results indicate that lithium ions and total phosphorus components inhibit lithium and phosphorus dissolution, respectively, and their combined presence further reduces iron loss.

[0184] Comparative Example 3, without the addition of carboxylic acid complexing agent, had an aluminum removal rate of only 43.8%, indicating that relying solely on a weak acid environment is insufficient to remove aluminum impurities. Carboxylic acid complexing agent is an important component for achieving selective aluminum removal.

[0185] In Comparative Example 4, the oxidant was added at the beginning of the first stage. Although the removal rates of aluminum and copper were still relatively high, the lithium loss rate, phosphorus loss rate, and cumulative iron dissolution rate increased to 4.86%, 3.72%, and 2.96%, respectively. This indicates that the timing control of removing aluminum first and then copper is not a simple adjustment of the process sequence, but an important measure to reduce the oxidative damage of lithium iron phosphate.

[0186] Comparative Example 5 had a redox potential of 240 mV, and its copper removal rate was only 72.4%; Comparative Example 6 had a redox potential of 520 mV, and its copper removal rate reached 99.3%, but the cumulative iron dissolution rate increased to 5.12%. The above results prove that too low a redox potential cannot fully remove copper, while too high a redox potential will damage the lithium iron phosphate structure.

[0187] The impurity removal data of Comparative Examples 7 and 8 are similar to those of Example 2, indicating that composition compensation and vacuum wetting mainly play a role in subsequent lattice repair, rather than the front-end impurity removal process.

[0188] Table 3 Results of Structure and Powder Properties of Recycled Materials

[0189] The relative content of the main crystalline phase of LiFePO4 and the total amount of XRD-resolvable crystalline and impurity phases in Table 3 are the results obtained after normalizing the crystalline phases that can be identified by XRD and participate in the fitting. They do not include amorphous carbon, amorphous residues, and trace phases below the XRD detection or reliable fitting limit.

[0190] The relative content of the main crystalline phase of LiFePO4 in Examples 1 to 6 was 97.4%–98.8%, and Fe²⁺ was 97.4%–98.8%. + The proportion of iron in the total iron content is 94.8% to 97.9%, indicating that the present invention can maintain a relatively complete lithium iron phosphate olivine structure after impurity removal and regeneration.

[0191] In Example 2, the relative content of the main crystalline phase of LiFePO4 reached 98.8%, and the total amount of XRD-resolvable crystalline impurities was 1.2%. This result indicates that, within the range of crystalline phases that can be resolved by XRD, Example 2 is dominated by the main crystalline phase of LiFePO4, but does not mean that the total amount of all trace impurities, amorphous phases, or carbon coating layers in the sample is only 1.2%.

[0192] Comparative Examples 1 and 2, due to the lack of lithium ion or phosphate protection, exhibited more lithium-deficient iron phosphate phase and iron-containing phosphate crystal phase, respectively.

[0193] Comparative Example 4: Due to the early addition of the oxidant, Fe² + The proportion decreased to 86.1%; in comparative example six, due to excessively high redox potential, Fe² + The proportion further decreased to 79.8%, and the relative content of the main crystalline phase of LiFePO4 was only 89.7%. This result is consistent with the increase in the cumulative iron dissolution rate in Table 3.

[0194] Comparative Example 7 did not undergo composition compensation. Although it was sintered in a reducing atmosphere, the total amount of crystalline and impurity phases that could be resolved by XRD was still 5.2% because the Li / Fe molar ratio and P / Fe molar ratio were not restored to the target range.

[0195] Comparative Example 8 was impregnated under normal pressure. Although the overall element ratio was the same as in Example 2, the supplemented elements were mainly concentrated on the outer surface of the particles. The degree of repair of the microcrack area inside the particles was low, resulting in a higher total amount of XRD-resolvable crystalline and impurity phases than in Example 2.

[0196] Table 4 Electrochemical performance test results

[0197] The initial discharge specific capacity at 0.1C in Examples 1 to 6 was 153.8–159.2 mAh / g, and the capacity retention rate after 500 cycles at 1C was 91.8%–96.0%, which was significantly higher than that of the waste powder before treatment and the comparative examples.

[0198] The specific capacity of the first discharge at 0.1C in Example 2 was 159.2 mAh / g, the specific capacity at 5C was 126.8 mAh / g, and the capacity retention rate after 500 cycles at 1C was 96.0%. This indicates that by using lithium-phosphorus co-protection, staged impurity removal, potential control, quantitative replenishment, vacuum wetting, and segmented sintering, the impurity removal purity, crystal integrity, and long-term cycle stability can be improved simultaneously.

[0199] Comparative Examples 1 and 2 lacked lithium salt and soluble phosphate, respectively. Due to element loss and the increase of XRD-resolved crystalline impurities, their 0.1C first discharge specific capacity decreased to 141.8 mAh / g and 139.7 mAh / g, respectively.

[0200] In Comparative Example 3, the aluminum impurities were not sufficiently removed, resulting in a significant decrease in both the initial discharge specific capacity and cycle retention rate. This indicates that residual aluminum impurities can affect the interface and long-term cycle performance of the recycled material.

[0201] Comparative Example 4: An oxidant was added in advance, so that the lithium iron phosphate was in an oxidizing environment for a long time. Its initial discharge specific capacity was only 136.2 mAh / g, and the capacity retention rate after 500 cycles was 80.8%.

[0202] Although Comparative Example 5 showed less damage to the lithium iron phosphate crystals, its copper removal rate was insufficient, resulting in a high residual copper content. Therefore, its initial capacity was acceptable, but its 500-cycle retention rate was only 83.6%. This result indicates that initial capacity alone cannot adequately evaluate the copper removal effect, and residual copper primarily manifests as long-term latent failure.

[0203] Comparative Example 6 uses an excessively high redox potential, Fe² + Extensive oxidation leads to a decrease in the relative content of the main crystalline phase of LiFePO4, resulting in the lowest initial discharge specific capacity and cycle performance.

[0204] Comparative Example 7 did not undergo quantitative component compensation, and its impurity removal rate was close to that of Example 2. However, because the ratio of lithium, iron and phosphorus did not return to the target range, the initial discharge specific capacity was only 142.6 mAh / g.

[0205] Comparative Example 8 was impregnated under normal pressure, and its initial capacity was higher than that of Comparative Example 7, but its 5C capacity and long-term cycle retention rate were still significantly lower than those of Example 2, indicating that vacuum impregnation has an effect on the uniform repair of microcrack areas inside the particles.

[0206] Figure 1 As shown in the figure, the outer contour of the particle is complete, and the internal cross-section is generally continuous and relatively dense, with only a small number of closed pores and local microcracks, and no obvious through cracks. In the figure, 1 represents the outer contour of the particle, 2 represents the internal cross-section of the particle, 3 represents closed pores, 4 represents microcracks, 5 represents the platinum protective layer, and 6 represents the main lithium iron phosphate region. The scale bar is 1 μm.

[0207] Figure 2 In the figure, (a) is a HAADF-STEM image, (b) to (f) are the elemental distribution maps of Fe, P, O, Al and Cu, respectively, and (g) is a superimposed image of Fe, P and O. As can be seen from the figure, Fe, P and O are evenly distributed, while Al and Cu only show scattered weak signals and no obvious local enrichment is observed.

[0208] Figure 3 As can be seen from the figure, the internal lattice fringes of the material are clear and continuous. The interplanar spacings of (020) and (101) are measured to be approximately 0.300 nm and 0.421 nm, respectively. The FFT spots are regular, indicating that the recycled material has good olivine-type crystal order.

[0209] A comparison of Example 2 with Comparative Examples 1 and 2 shows that lithium ions and soluble phosphates are not ordinary background electrolytes. Both reduce the dissolution of lithium and phosphorus, respectively, and together reduce iron loss. The cumulative iron dissolution rate during the entire impurity removal process in Example 2 was only 0.36%, significantly lower than 2.31% in Comparative Example 1 and 2.58% in Comparative Example 2.

[0210] A comparison of Example 2 and Comparative Example 3 shows that the carboxylic acid complexing agent is an important component for improving aluminum removal efficiency. Under the same pH and lithium-phosphorus protection conditions, without the addition of the carboxylic acid complexing agent, the aluminum removal efficiency decreased from 98.8% to 43.8%.

[0211] A comparison of Example 2 and Comparative Example 4 shows that by not adding an oxidant in the first stage and allowing the aluminum impurities to fully dissolve before oxidizing to remove copper, the exposure time of lithium iron phosphate to oxidizing conditions can be shortened. This timing relationship reduced the cumulative iron dissolution rate from 2.96% to 0.36%.

[0212] A comparison of Example 2 with Comparative Examples 5 and 6 shows that the redox potential window has a criticality. Below this window, copper removal is insufficient; above this window, Fe²⁺ removal is inadequate. + Oxidation and iron dissolution are significantly amplified. Therefore, the redox potential range defined in this invention is not an arbitrarily chosen conventional process parameter.

[0213] The comparison between Example 2 and Comparative Example 7 shows that controlling the impurity removal process alone is insufficient to restore the electrochemical performance of waste lithium iron phosphate. Quantitative replenishment based on the actual elemental composition of the material after impurity removal is also necessary.

[0214] The comparison between Example 2 and Comparative Example 8 shows that, with the same total amount of additives, vacuum wetting can improve the distribution of additive elements in the pores and microcracks inside the particles, thereby improving high-rate performance and long-term cycling stability.

[0215] Therefore, this invention does not simply list lithium salts, phosphates, complexing agents, oxidants, lithium replenishment, and sintering techniques side by side, but rather forms the following mutually restrictive and complementary technical chain: lithium-phosphate co-protection is used to suppress lattice dissolution in acidic crystal protection and impurity removal solutions; preferential aluminum removal under non-oxidizing conditions is used to shorten the exposure time of lithium iron phosphate to the oxidizing environment; and controlled potential copper removal is used to balance the copper oxidation rate and Fe²⁺. + Stability; redox potential feedforward-feedback control is used to overcome electrode response hysteresis and signal fluctuations in complex slurries; gradient washing is used to reduce the loss of secondary elements after impurity removal; quantitative replenishment is used to eliminate compositional differences between different waste batches; staged vacuum impregnation is used to improve the compositional uniformity of defective areas inside particles and suppress violent boiling of mixed solvents; staged sintering and in-situ carbon coating are used to restore the olivine structure and conductive network.

[0216] The above-mentioned technical steps are functionally interconnected and together achieve the technical effects of efficient removal of aluminum and copper, cumulative iron dissolution rate not exceeding 1.0%, increased proportion of LiFePO4 main crystal phase, and recovery of long-term cycling performance.

Claims

1. A method for recycling and regenerating waste lithium iron phosphate cathode materials, characterized in that, Includes the following steps: S1, waste lithium iron phosphate positive electrode sheets are discharged, disassembled, electrolyte removed, stripped and sieved to obtain waste powder containing lithium iron phosphate; S2, the waste powder is added to a crystal protection and impurity removal solution containing lithium salt, soluble phosphate, and carboxylic acid complexing agent, so that the lithium ion concentration in the liquid phase is 0.05-0.60 mol / L and the total phosphorus concentration is 0.02-0.40 mol / L; the lithium salt and soluble phosphate are used to increase the concentration of lithium ions and phosphorus-containing anions in the liquid phase to inhibit the dissolution of lithium iron phosphate surface and the migration of lithium and phosphorus elements into the liquid phase; the carboxylic acid complexing agent forms a water-soluble complex with the aluminum ions released by aluminum impurities; the first stage leaching is carried out under conditions of pH 4.2-5.2 without the addition of an oxidant; when the change rate of liquid phase aluminum concentration in two consecutive adjacent detection intervals is not greater than 5%, the second stage leaching is carried out directly, or the solid is separated by solid-liquid separation and the resulting solid is redispersed in the crystal protection and impurity removal solution for the second stage leaching; S3, after solid-liquid separation and washing, the obtained impurity-removed solid is analyzed for lithium, iron, and phosphorus content. A lithium source is added, and iron and / or phosphorus sources are selectively added based on the test results to achieve a Li / Fe molar ratio of 1.00–1.08 and a P / Fe molar ratio of 0.98–1.

03. In the second stage of leaching, an oxidant is added in stages, and the redox potential is maintained at 280–480 mV using a saturated potassium chloride Ag / AgCl reference electrode to remove copper impurities through oxidative complexation. From the addition of the waste powder to the crystal-protected impurity-removing solution to the end of the solid-liquid separation, the cumulative amount of iron dissolved in all liquid phases (including the first stage leaching solution, the second stage leaching solution, and the washing solution) is no more than 1.0% of the initial iron content of the waste powder. S4. The replenished material is mixed with a carbon source and heat-treated under an inert or reducing atmosphere to obtain regenerated lithium iron phosphate cathode material.

2. The method for recycling and regenerating waste lithium iron phosphate cathode material according to claim 1, characterized in that, Step S1 includes: cleaning the waste lithium iron phosphate cathode sheet with dimethyl carbonate, diethyl carbonate or ethyl acetate to remove electrolyte; heat-treating the stripped material at 350-450℃ for 30-120 minutes under an inert atmosphere or vacuum; crushing and classifying the heat-treated material, and sieving out aluminum foil particles, copper foil particles and other metal particles with a particle size greater than 150μm.

3. The method for recycling and regenerating waste lithium iron phosphate cathode material according to claim 1, characterized in that, The lithium salt is selected from one or more of lithium dihydrogen phosphate, lithium sulfate, lithium acetate, and lithium nitrate; the soluble phosphate is selected from one or more of lithium dihydrogen phosphate, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate; the carboxylic acid complexing agent is selected from one or more of citrate, tartrate, malate, and ethylenediaminetetraacetate, and the concentration of the carboxylic acid complexing agent in the crystal protection and impurity removal solution is 0.02–0.20 mol / L.

4. The method for recycling and regenerating waste lithium iron phosphate cathode material according to claim 1, characterized in that, During the first stage of leaching, the solid-liquid ratio of the waste powder to the crystal protection and impurity removal solution is 1g:5-15mL, the leaching temperature is 35-65℃, the leaching time is 20-90min, and the pH is maintained at 4.4-5.0 by adding citric acid, acetic acid, or ammonium dihydrogen phosphate.

5. The method for recycling and regenerating waste lithium iron phosphate cathode material according to claim 1, characterized in that, The oxidant is selected from one or more of hydrogen peroxide, ammonium persulfate, and sodium persulfate; the redox potential of the second stage leaching is detected by a saturated potassium chloride Ag / AgCl reference electrode, and the addition rate of the oxidant is adjusted in a closed loop according to the detection value to maintain the redox potential at 320-430mV.

6. The method for recycling and regenerating waste lithium iron phosphate cathode material according to claim 5, characterized in that, The second stage leaching temperature is 25–55℃ and the time is 10–60 min. During the reaction, the copper and iron content in the liquid phase is detected every 5–15 min. When the change rate of copper concentration in the liquid phase in two consecutive adjacent detection intervals is not greater than 5%, the addition of oxidant is stopped, and solid-liquid separation is completed within 10 min after the addition of oxidant is stopped. The copper impurity removal rate calculated based on the cumulative copper element mass in the liquid phase or the residual copper content in the solid after solid-liquid separation is not less than 95%.

7. The method for recycling and regenerating waste lithium iron phosphate cathode material according to claim 1, characterized in that, The washing in step S3 adopts a gradient washing method, which includes first washing the impurity-removing solid with a lithium dihydrogen phosphate solution with a concentration of 0.01 to 0.10 mol / L and a pH of 5.5 to 6.5, and then washing with deionized water until the conductivity of the final washing solution is not greater than 500 μS / cm.

8. The method for recycling and regenerating waste lithium iron phosphate cathode material according to claim 1, characterized in that, The lithium, iron, and phosphorus contents in the purified solid were determined by inductively coupled plasma atomic emission spectrometry (ICP-AES). The lithium source was selected from one or more of lithium carbonate, lithium hydroxide, and lithium acetate; the iron source was selected from one or more of ferrous oxalate, ferric phosphate, and ferrous oxide; and the phosphorus source was selected from one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and phosphoric acid. The Li / Fe molar ratio after replenishment was 1.02–1.05, and the P / Fe molar ratio was 0.995–1.

015.

9. The method for recycling and regenerating waste lithium iron phosphate cathode material according to claim 8, characterized in that, The lithium source, iron source, and / or phosphorus source are dissolved or dispersed in a mixed solvent of water and ethanol to form a replenishing solution. The impurity-removing solid is mixed with the replenishing solution and then vacuum-impregnated for 10 to 60 minutes at a gauge pressure of -0.060 to -0.095 MPa relative to the local atmospheric pressure, so that the replenishing solution enters the surface pores and microcracks of the impurity-removing solid particles. After vacuum impregnation, the resulting slurry is spray-dried and granulated at an outlet temperature of 80 to 140°C.

10. The method for recycling and regenerating waste lithium iron phosphate cathode material according to claim 9, characterized in that, The carbon source is selected from one or more of glucose, sucrose, citric acid, polyethylene glycol and asphalt, and the amount of carbon source added is 2-8% of the mass of the material after replenishment; the heat treatment includes first holding at 300-450℃ for 1-3 hours, and then raising the temperature to 650-750℃ and holding for 2-8 hours, and the atmosphere of the heat treatment is nitrogen containing 1-5 vol% hydrogen, and the carbon content in the resulting recycled lithium iron phosphate cathode material is 1-4 wt%.