A method for recovering struvite from low-nitrogen wastewater

By employing pre-precipitation and parameter optimization methods, the problems of Ca2+ interference and heavy metal contamination in struvite recovery from low-nitrogen municipal wastewater in China have been solved. This method achieves high-purity, high-yield struvite crystallization, which is applicable to domestic municipal wastewater treatment processes.

CN123105584APending Publication Date: 2026-11-17CHANGSHU TAP WATER CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611229534.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies cannot effectively recover struvite from low-nitrogen municipal wastewater in China. They suffer from problems such as Ca2+ interference, excessive heavy metals, and unstable product purity and yield, and cannot be adapted to domestic municipal wastewater treatment processes.

Method used

By removing Ca2+ and heavy metals through a pre-precipitation impurity removal step, optimizing the feed ratio of magnesium, phosphorus, and nitrogen and the pH value, adding struvite seed crystals, and standardizing the alkali addition and drying operations, high-purity and high-yield struvite crystals can be achieved.

Benefits of technology

It achieves the recovery of high-crystallinity, high-purity struvite, with a stable phosphorus recovery rate of over 75%. The product meets inorganic fertilizer standards and is suitable for domestic municipal wastewater treatment processes without the need for large-scale modifications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105584A_ABST
    Figure CN123105584A_ABST
Patent Text Reader

Abstract

This disclosure provides a method for struvite recovery from low-nitrogen wastewater, relating to the fields of municipal wastewater treatment and phosphorus resource recovery technology. The method includes selecting the supernatant from the sludge dewatering process at the wastewater treatment plant, filtering it, and then detecting the calcium content in the wastewater. 2+ Check if the concentration exceeds the concentration threshold or if the heavy metal content exceeds the total content threshold; if it exceeds the standard, add a pre-precipitant to the wastewater, adjust the pH value of the wastewater, stir the reaction, let it settle, and take the supernatant as the pretreated wastewater; if it does not exceed the standard, use the supernatant of the original wastewater as the pretreated wastewater; add magnesium source, nitrogen source, and sodium hydroxide solution to the pretreated wastewater, adjust the pH value, stir the treatment, and obtain the adjusted wastewater; add struvite seed crystals to the adjusted wastewater, stir evenly, and carry out struvite crystallization reaction to obtain a mixed system containing struvite; filter the mixed system containing struvite for solid-liquid separation, wash the separated solid product with deionized water, and dry it to constant weight to obtain struvite crystals.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure belongs to the field of municipal wastewater treatment and phosphorus resource recovery technology, specifically relating to a method for recovering struvite from low-nitrogen back-end wastewater. Background Technology

[0002] Phosphorus is an essential macronutrient for biological growth and a non-renewable, scarce resource. Global phosphate rock reserves are limited and face the risk of depletion. Municipal wastewater contains a certain concentration of phosphorus; direct discharge not only causes eutrophication but also wastes valuable phosphorus resources. Struvite (MgNH4PO4•6H2O), as a high-quality slow-release phosphate fertilizer, has advantages such as high phosphorus content, slow nutrient release, and minimal leaching, making it an ideal product for phosphorus recovery from municipal wastewater.

[0003] Currently, the EU has widely conducted research and application of struvite recovery technology, the core of which is based on the technical route of "anaerobic process to produce biogas + front-end high-nitrogen wastewater phosphorus recovery". However, there are significant differences between my country's municipal wastewater treatment processes and those of the EU. For example, domestic municipal wastewater treatment plants generally use aerobic treatment processes, do not recover biogas, and after back-end treatment, the nitrogen content of low-nitrogen wastewater such as sludge dewatering supernatant is extremely low (usually 5-15 mg / L); while EU wastewater has a nitrogen content as high as 50-80 mg / L after front-end anaerobic treatment. Therefore, the existing struvite recovery technology in the EU cannot be directly applied to domestic municipal wastewater treatment plants due to insufficient nitrogen source and poor process adaptability.

[0004] Existing technologies for struvite recovery from low-nitrogen municipal wastewater in China have several shortcomings: 1. Most studies are based on simulated water distribution and do not take into account the complex composition of actual municipal wastewater in China, especially the high Ca content in actual wastewater. 2+ Concentrations often exceed 50 mg / L, Ca 2+ Will with PO4 3- 1. Competition for the formation of calcium phosphate or hydroxyapatite precipitates severely interferes with the directional crystallization of struvite, resulting in low yield and insufficient purity in practical applications; 2. Existing processes often fail to control drying conditions, leading to problems such as loss of crystal water and localized over-alkali formation of byproducts, resulting in deviations in yield calculations and unstable product quality; 3. Existing processes cannot simultaneously address the Ca... 2+ Interference and excessive heavy metals make it difficult for the product to meet inorganic fertilizer standards, thus limiting its industrial application. In summary, existing research on struvite recovery from low-nitrogen municipal wastewater in China mainly focuses on optimizing single parameters, failing to form a complete process system adapted to actual wastewater, making industrial application difficult. Summary of the Invention

[0005] This disclosure aims to at least solve one of the technical problems existing in the prior art, and to provide a method for the recovery of struvite suitable for low-nitrogen back-end wastewater.

[0006] This disclosure provides a method for recovering struvite from low-nitrogen wastewater, the method comprising: S110. Select the supernatant from the sludge dewatering supernatant at the back end of the wastewater treatment plant, filter it, and then test the Ca content in the wastewater. 2+ Whether the concentration exceeds the concentration threshold or whether the heavy metal content exceeds the total content threshold; S120, if Ca 2+ If the concentration is above the concentration threshold or the heavy metal content is above the total content threshold, a pre-precipitant is added to the wastewater to adjust it to the first pH value. After stirring and reacting, the wastewater is allowed to settle, and the supernatant is taken as pretreated wastewater. If Ca... 2+ If the concentration is less than the concentration threshold and the heavy metal content is less than the total content threshold, the supernatant of the original wastewater will be used as pretreated wastewater. S130. Add magnesium source, nitrogen source, and sodium hydroxide solution to the pretreated wastewater to adjust the acidity of the wastewater to a second pH value, stir and treat to obtain the adjusted wastewater; S140. Add struvite seed crystals to the adjusted wastewater, stir evenly, and then carry out struvite crystallization reaction to obtain a mixed system containing struvite. S150. The mixed system containing struvite is filtered to separate the solid and liquid components. The separated solid product is washed with deionized water and dried to constant weight to obtain struvite crystals.

[0007] Optionally, in step S110, Ca 2+ The concentration threshold is 50 mg / L, and the total heavy metal content threshold is 0.4 mg / L.

[0008] Optionally, in step S120, the preprecipitant is at least one of calcium hydroxide and sodium carbonate; The ratio of the amount of pre-precipitant added to the wastewater content is (0.1-0.5) g: 1 L.

[0009] Optionally, in step S120, the first pH value is 7.8-8.2, and the reaction is stirred at a speed of 100-200 r / min for 5-15 min, followed by standing precipitation for 30-60 min.

[0010] Optionally, in step S130, the magnesium source is one or a mixture of magnesium chloride and magnesium sulfate; The nitrogen source is one or a mixture of ammonium chloride and ammonium sulfate; The molar ratio of magnesium, phosphorus and nitrogen in the feed is (1.3-1.5):1.0:(1.0-1.3).

[0011] Optionally, in step S130, the sodium hydroxide solution is added dropwise at a constant rate using a peristaltic pump, and the addition is completed within 30 minutes; the second pH value is 9.0-9.5, and then the solution is stirred at a stirring speed of 150-250 r / min for 10-30 minutes.

[0012] Optionally, in step S140, the amount of the struvite seed crystals added is 5% to 10% of the theoretical struvite yield.

[0013] Optionally, in step S140, the temperature of the struvite crystallization reaction is 25-35°C and the time is 2-6 hours.

[0014] Optionally, in step S150, the solid product is washed 2-3 times with deionized water and dried at 38-42°C for 6-8 hours.

[0015] Optionally, the crystallinity of the struvite crystals is ≥85%, the purity is ≥85%, and the phosphorus recovery rate is ≥75%.

[0016] This disclosure provides a method for struvite recovery suitable for low-nitrogen wastewater, addressing the issue that EU struvite recovery processes are not adaptable to domestic conditions. Compared to existing technologies, this method offers the following advantages: 1. This disclosure addresses the challenges of adapting EU processes to domestic conditions and the actual calcium content of wastewater by optimizing the entire set of process parameters, innovating pre-sedimentation and impurity removal steps, and standardizing operational details. 2+ Technical problems such as interference and excessive product impurities are addressed to achieve stable recovery of struvite with high crystallinity, high purity, and low impurities, thus promoting the resource utilization of phosphorus resources in municipal wastewater in China. 2. The pre-precipitation and impurity removal step of this disclosure can simultaneously remove Ca. 2+ Interfering ions and heavy metal ions are eliminated from the source to prevent the interference of coexisting ions on crystallization. This solves the problems of low purity and excessive heavy metals in actual wastewater recovery in existing technologies. The resulting struvite crystals have a purity of ≥85%, and the heavy metal content monitored by the fertilizer fully complies with the relevant standards for inorganic fertilizers in "Organic-Inorganic Compound Fertilizers" (GB / T 18877-2020). 3. By optimizing the entire set of parameters such as feed ratio, pH, and seed crystal addition, and combining them with standardized operating details, the phosphorus recovery rate of the method of this invention is stable at over 75%, and can reach 82.5% under optimal operating conditions, thus solving the problem of large fluctuations in actual wastewater recovery rate in existing technologies. 4. This disclosure clearly specifies key operational details such as alkali addition rate and drying conditions, avoiding problems such as local over-alkali, loss of crystal water, and incomplete drying, ensuring the stability of product quality, and eliminating errors in yield calculation, resulting in high data reliability. 5. This disclosure optimizes the design of municipal wastewater treatment plants in China, taking into account their process characteristics of "aerobic treatment, low nitrogen content at the downstream end, and no biogas production," while also adapting to the high-Ca content of actual wastewater. 2+ Due to its complex composition, it does not require large-scale renovation of existing wastewater treatment plants and can be directly promoted and applied. Attached Figure Description

[0017] Figure 1 This is a flowchart illustrating a specific embodiment of a method for recovering struvite from low-nitrogen back-end wastewater according to this disclosure. Figure 2 This is a schematic flowchart illustrating a specific embodiment of a method for recovering struvite from low-nitrogen back-end wastewater according to the present disclosure. Figure 3 This is a comparison chart of phosphorus recovery yield under different pH conditions in Examples 1-3 of this disclosure; Figure 4 This is a microscopic morphology image of the struvite crystals obtained in Example 1 of this disclosure; Figure 5 This is the XRD pattern of struvite crystals obtained in Example 1 of this disclosure. Detailed Implementation

[0018] To enable those skilled in the art to better understand the technical solutions of this disclosure, the disclosure will be further described in detail below with reference to the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain this disclosure and represent a part of the embodiments of this disclosure, not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this disclosure without creative effort are within the protection scope of this disclosure.

[0019] like Figure 1 and Figure 2 As shown, this disclosure provides a method S100 for the recovery of struvite from low-nitrogen wastewater, specifically including the following steps S110~S150: S110. Select the supernatant from the sludge dewatering supernatant at the back end of the wastewater treatment plant, filter it, and then test the Ca content in the wastewater. 2+ Does the concentration exceed Ca? 2+ Whether the concentration threshold or the total heavy metal content exceeds the total heavy metal content threshold.

[0020] In step S110, the supernatant of sludge water from the downstream of the wastewater treatment plant is selected from the supernatant of sludge dewatering from the downstream of a domestic municipal wastewater treatment plant. The nitrogen content is 5-15 mg / L and the phosphorus concentration in the influent is about 74.6 mg / L. Large particulate floating debris and suspended solids are removed by filtration with a 100-150 mesh filter cloth.

[0021] S120, if Ca 2+ Concentration in Ca 2+If the concentration threshold is exceeded or the total heavy metal content exceeds the heavy metal content threshold, a pre-precipitant is added to the wastewater to adjust it to the first pH value. After stirring and reacting, the wastewater is allowed to settle, and the supernatant is taken as pretreated wastewater. If Ca... 2+ Concentration less than Ca 2+ If the concentration threshold and the total heavy metal content are both less than the total content threshold, the supernatant of the original wastewater will be used as pretreated wastewater.

[0022] It should be noted that in step S120, if the Ca in the original supernatant... 2+ If the concentration exceeds the threshold or the total heavy metal content exceeds the standard, it will be pretreated. The supernatant after treatment will be used as the pretreated wastewater in the subsequent steps. If all requirements are met, the supernatant of the original wastewater will be used as the pretreated wastewater in the subsequent steps.

[0023] In step S120, Ca 2+ The concentration threshold is 50 mg / L, for detecting Ca in wastewater. 2+ The concentration must be ≥50 mg / L. If ≥50 mg / L, it is considered unqualified; if less than 50 mg / L, it is considered qualified. Heavy metals include mercury, chromium, lead, arsenic, cadmium, copper, nickel, and zinc. The total heavy metal content threshold is 0.4 mg / L. If the total heavy metal content is ≥0.4 mg / L, it is considered unqualified; if less than, it is considered qualified. This implementation method has been verified through small-scale experiments to reduce the content of Ca... 2+ The concentration was reduced from 55.2 mg / L to below 10 mg / L, and the total heavy metal content of fertilizer monitoring was reduced to below 0.25 mg / L, eliminating the interference of coexisting ions on the crystallization reaction from the source.

[0024] In step S120, the preprecipitant is at least one of calcium hydroxide and sodium carbonate; the ratio of the amount of preprecipitant added to the wastewater content is (0.1-0.5) g: 1L, for example, preferably 0.2-0.4 g: 1L.

[0025] In the preferred embodiment, the preprecipitant is preferably a mixture of calcium hydroxide and sodium carbonate, with a mixing mass ratio of 1:(0.1-2.0). It should be noted that the proportion of the preprecipitant added is related to the original calcium ion content, total carbonate content, and original pH value of the wastewater. After adding the preprecipitant, the pH value of the pretreated wastewater should be controlled within the range of 8±0.2.

[0026] In step S120, the first pH value is 7.8-8.2, and the reaction is stirred at a speed of 100-200 r / min for 5-15 min, followed by standing precipitation for 30-60 min.

[0027] S130. Add magnesium source, nitrogen source, and sodium hydroxide solution to the pretreated wastewater to adjust the acidity of the wastewater to the second pH value, stir and treat to obtain the adjusted wastewater.

[0028] In step S130, the magnesium source is one or a mixture of magnesium chloride and magnesium sulfate; the nitrogen source is one or a mixture of ammonium chloride and ammonium sulfate.

[0029] In step S130, after adding the magnesium source and nitrogen source, the molar ratio of magnesium, phosphorus and nitrogen in the wastewater needs to be controlled to be (1.3-1.5):1.0:(1.0-1.3). This feeding ratio is obtained by referring to the optimal parameters of simulated water distribution and combining them with the actual characteristics of wastewater.

[0030] It should be noted that the phosphorus content in step S130 refers to the phosphorus content detected in the wastewater. Based on the detected phosphorus content, appropriate amounts of magnesium and nitrogen sources are added according to the above feeding ratio.

[0031] In step S130, the sodium hydroxide solution has a mass fraction of 10% and is added dropwise at a uniform rate using a peristaltic pump within 30 minutes to avoid local over-alkaliness and the generation of byproducts such as Mg(OH)2. Finally, the acidity of the wastewater is adjusted to a second pH value of 9.0-9.5. Then, the mixture is stirred at a speed of 150-250 r / min for 10-30 minutes to ensure that the reagent and wastewater are fully mixed.

[0032] In step S130, the second pH value is more preferably 9.5, which helps to improve the phosphorus recovery yield.

[0033] S140. Add struvite seed crystals to the adjusted wastewater, stir evenly, and then place the above system in a crystallization device to carry out struvite crystallization reaction to obtain a mixed system containing struvite.

[0034] In step S140, the amount of struvite seed crystals added is 5% to 10% of the theoretical struvite yield. The seed crystals provide a ready-made solid surface, allowing ions in the solution to deposit and grow directly on the seed crystal surface, bypassing the high-energy barrier of homogeneous nucleation and accelerating the crystallization process. Small-scale experiments have shown that adding 10% seed crystals can increase the phosphorus recovery yield by about 2 percentage points compared to not adding seed crystals.

[0035] In step S140, the temperature of the struvite crystallization reaction is 25-35℃ and the time is 2-6h, more preferably 28-32℃ and 3-5h.

[0036] S150. The mixed system containing struvite is filtered to separate the solid and liquid components. The separated solid product is washed with deionized water and dried to constant weight to obtain struvite crystals.

[0037] In step S150, the solid product is washed 2-3 times with deionized water to remove soluble impurities adhering to the surface; it is then dried in a drying oven at 40°C to constant weight to avoid the struvite losing its water of crystallization due to high temperature, while ensuring thorough drying to eliminate deviations in yield calculation, and finally obtaining struvite crystals.

[0038] In step S150, the crystallinity of the struvite crystals is ≥85%, the purity is ≥85%, the heavy metal content meets the relevant standards for inorganic fertilizers in "Organic-Inorganic Compound Fertilizers" (GB / T 18877-2020), the phosphorus recovery rate is ≥75%, and the preferred yield range is 78%-83%.

[0039] This disclosure addresses the issue of actual wastewater Ca in the prior art. 2+ To address issues such as interference, excessive product impurities, and improper operation, the proposed methods include raw material pretreatment (including pre-precipitation and impurity removal), parameter adjustment, seed crystal addition, crystallization reaction, solid-liquid separation, and drying steps. By optimizing process parameters and innovating the pre-precipitation and impurity removal step, Ca can be removed simultaneously. 2+ The details of interference and heavy metals, standardized alkali addition and drying operations are adapted to the domestic low-nitrogen back-end municipal wastewater treatment process conditions.

[0040] The following will further illustrate the struvite recovery method applicable to low-nitrogen back-end wastewater with specific embodiments: Example 1 A method for recovering struvite from low-nitrogen municipal wastewater in China includes the following steps: 1. Raw material pretreatment: The supernatant from the dewatering of sludge from a municipal wastewater treatment plant in China was used. Its nitrogen content was 8 mg / L, phosphorus content was 74.6 mg / L, and calcium content was... 2+ The concentration was 55.2 mg / L, and the total heavy metal content was 0.45 mg / L. First, large suspended solids were removed by filtration through a 120-mesh filter cloth. Then, a pre-precipitant (sodium carbonate) was added to the filtered wastewater at a dosage of 0.3 g / L (0.3 g of sodium carbonate per 1 L of wastewater). The mixture was stirred at 150 rpm for 10 minutes, then allowed to settle for 40 minutes. The supernatant was taken as the pretreated wastewater. Testing showed that the pretreated Ca... 2+ The concentration decreased to 5.8 mg / L, and the total heavy metal content decreased to 0.15 mg / L.

[0041] 2. Parameter adjustment: Add 0.031 mol magnesium chloride (magnesium source) and 0.024 mol ammonium chloride (nitrogen source) to 10 L of pretreated wastewater, and control the molar ratio of magnesium, phosphorus and nitrogen to be 1.3:1.0:1.0; use a peristaltic pump to add 10% sodium hydroxide solution by uniform dripping, and complete the dripping within 30 min, adjust the acidity of the wastewater to pH=9.5, control the stirring speed to 200 r / min, and the stirring time to 20 min.

[0042] 3. Seed crystal addition: Add guanoite seed crystals to the system at a rate of 10% of the theoretical guanoite yield, and stir until homogeneous.

[0043] 4. Crystallization reaction: The system was placed in a 10-15L crystallization apparatus, and the crystallization temperature was controlled at 30℃ for 4 hours to carry out the struvite crystallization reaction, so as to obtain a mixed system containing struvite.

[0044] 5. Solid-liquid separation and drying: The mixed system was filtered to separate the solid and liquid, washed three times with deionized water, and dried in a drying oven at 40℃ to constant weight (the difference between two weighings <0.001g) for 7 hours to obtain struvite crystals.

[0045] Testing revealed that the struvite crystals obtained in this embodiment had a crystallinity of 88% and a purity of 90%. Of the five key monitored heavy metals, mercury, chromium, lead, and cadmium were not detected; arsenic content was 13.2 mg / kg; the other three heavy metals, copper (6.9 mg / kg), zinc (153.2 mg / kg), and nickel (not detected), were also present. Figure 3 As shown, the phosphorus recovery rate was 82.5%, and all indicators met the standards for inorganic fertilizers.

[0046] like Figure 4 As shown, the sample crystals are mainly regular rod-shaped / prismatic, which is a typical morphology of struvite (magnesium ammonium phosphate), and the crystal outlines are clear.

[0047] like Figure 5 As shown, the sharp peak shape indicates good crystallinity. Comparison with the standard PDF card of struvite shows that the position of the main peak corresponds completely with the characteristic peak of magnesium ammonium phosphate hexahydrate, and there are no obvious impurity peaks, proving that the main phase of the product is struvite.

[0048] Example 2 A method for recovering struvite from low-nitrogen municipal wastewater in China differs from Example 1 in that: In step (1), the pre-precipitant is 0.2 g / L sodium carbonate. The dosage of sodium carbonate is 0.2 g / L, that is, 0.2 g sodium carbonate is added to 1 L of wastewater. After stirring and reacting for 5 min, the mixture is allowed to settle for 30 min. After pretreatment, Ca 2+The concentration decreased to 18.2 mg / L, and the total heavy metal content was 0.22 mg / L; In step (2), the pH is adjusted to 9.0, the stirring speed is 150 r / min, and the stirring time is 25 min; In step (3), the seed crystal addition amount is 5% of the theoretical yield; In step (4), the crystallization temperature is 28℃ and the crystallization time is 5h.

[0049] Testing revealed that the struvite crystals obtained in this embodiment had a crystallinity of 86% and a purity of 84%. Of the five key monitored heavy metals, mercury, chromium, lead, and cadmium were not detected; arsenic content was 14.8 mg / kg; the other three heavy metals, copper (9.2 mg / kg), zinc (187.4 mg / kg), and nickel (not detected), were also present. Figure 3 As shown, the phosphorus recovery rate was 73.5%.

[0050] Example 3 A method for recovering struvite from low-nitrogen municipal wastewater in China differs from Example 1 in that: In step (1), the pre-precipitant is 0.4 g / L sodium carbonate. The dosage of sodium carbonate is 0.4 g / L, that is, 0.4 g of sodium carbonate is added to 1 L of wastewater. After stirring and reacting for 15 min, the mixture is allowed to stand and precipitate for 60 min. After pretreatment, Ca 2+ The concentration decreased to 4.7 mg / L, and the total heavy metal content was 0.14 mg / L; In step (2), 0.036 mol of magnesium source, which is a mixture of magnesium sulfate and magnesium chloride in a mass ratio of 1:1, 0.029 mol of ammonium chloride (nitrogen source), the molar ratio of feed is 1.5:1.0:1.2, the pH is adjusted to 9.2, the stirring speed is 250 r / min, and the stirring time is 15 min; In step (3), the seed crystal addition amount is 8% of the theoretical yield; In step (4), the crystallization temperature is 32℃ and the crystallization time is 3h.

[0051] Testing revealed that the struvite crystals obtained in this embodiment had a crystallinity of 87% and a purity of 89%. Of the five key monitored heavy metals, mercury, chromium, lead, and cadmium were not detected; arsenic content was 12.2 mg / kg; the other three heavy metals, copper (5.3 mg / kg), zinc (143.8 mg / kg), and nickel (not detected), were also present. Figure 3 As shown, the phosphorus recovery rate was 73.9%.

[0052] Comparative Example 1 (EU process adapted to domestic wastewater) The same batch of domestic municipal wastewater mentioned above was treated using the EU struvite recovery process, with the following steps: 1. Take 10L of high-nitrogen wastewater from the front end, add magnesium chloride / magnesium oxide, control the molar ratio of magnesium, phosphorus and nitrogen to be 1.2:1.0:1.0, directly aerate to adjust the pH to 9.0, stir at 200r / min for 20min, without pre-precipitation and impurity removal steps; 2. Crystallize at 30℃ for 4 hours without adding seed crystals; 3. After solid-liquid separation, the product is dried at 40℃ for 3 hours to obtain the product.

[0053] Testing revealed that the product obtained in Comparative Example 1 had a crystallinity of 72%, a purity of 76%, and Ca... 2+ The product has a high impurity content. Of the five key monitored heavy metals, mercury, lead, and cadmium were not detected; chromium content was 15.1 mg / kg; arsenic content was 16.2 mg / kg; and the other three heavy metals, copper (11.7 mg / kg), zinc (278.9 mg / kg), and nickel (not detected), were also present. The phosphorus recovery rate was 65.2%, and the product purity and heavy metal content did not meet the standards for inorganic fertilizers.

[0054] Comparative Example 2 (without pre-precipitation impurity removal step) The difference from Example 1 is that the pre-precipitation and impurity removal step (1) is omitted, while the remaining process parameters are the same as in Example 1.

[0055] Testing revealed that the struvite crystals obtained in Comparative Example 2 had a crystallinity of 80% and a purity of 77%. Of the five key monitored heavy metals, mercury, lead, and cadmium were not detected; chromium content was 15.2 mg / kg; arsenic content was 16.8 mg / kg; and the other three heavy metals, copper (12.3 mg / kg), zinc (280.4 mg / kg), and nickel (not detected), were also present. The phosphorus recovery rate was 82.3%. (Due to the presence of Ca...) 2+ The competitive precipitation process resulted in low product purity and excessive heavy metals, failing to meet inorganic fertilizer standards, demonstrating that the pre-precipitation and impurity removal step is crucial for improving product quality.

[0056] Comparative Example 3 (drying conditions not specified) The difference from Example 1 is that in step (5), constant temperature drying at 70°C for 3 hours was used, and constant weight was not controlled.

[0057] Testing revealed that the product obtained in Comparative Example 3 had a crystallinity of only 70% due to the loss of some of the water of crystallization caused by high temperature. Furthermore, due to incomplete drying, the calculated yield was as high as 103.2%, indicating serious data distortion and unstable product quality.

[0058] It should be noted that the method described above, as verified by small-scale experiments, can stably achieve the recovery of high-purity, low-impurity struvite, and all indicators meet national standards. Preliminary industrial-scale calculations show that it can process 1000 cubic meters per day. 3Taking a wastewater treatment plant treating low-nitrogen municipal wastewater as an example, the method of this invention can recover approximately 12 kg of struvite daily and approximately 4.4 tons of phosphorus resources annually. The obtained struvite has a crystallinity of ≥85%, a purity of ≥85%, and the content of all eight heavy metals meets the standards for inorganic fertilizers. The phosphorus recovery rate is consistently above 75%, and can reach 82.5% under optimal operating conditions. The method is simple to operate and highly adaptable to various equipment, and can be directly applied to phosphorus recovery in domestic municipal wastewater treatment plants to achieve the recycling of phosphorus resources. This not only reduces phosphorus emissions from municipal wastewater but also generates significant economic benefits while reducing the environmental costs of wastewater treatment, demonstrating promising prospects for industrial application.

[0059] It is understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of this disclosure, and this disclosure is not limited thereto. For those skilled in the art, various modifications and improvements can be made without departing from the spirit and substance of this disclosure, and these modifications and improvements are also considered to be within the scope of protection of this disclosure.

Claims

1. A method for recovering struvite from low-nitrogen wastewater, characterized in that, The recycling method includes: S110. Select the supernatant from the sludge dewatering supernatant at the back end of the wastewater treatment plant, filter it, and then test the Ca content in the wastewater. 2+ Whether the concentration exceeds the concentration threshold or whether the heavy metal content exceeds the total content threshold; S120, if Ca 2+ If the concentration is above the concentration threshold or the heavy metal content is above the total content threshold, a pre-precipitant is added to the wastewater to adjust it to the first pH value. After stirring and reacting, the wastewater is allowed to settle, and the supernatant is taken as pretreated wastewater. If Ca... 2+ If the concentration is less than the concentration threshold and the heavy metal content is less than the total content threshold, the supernatant of the original wastewater will be used as pretreated wastewater. S130. Add magnesium source, nitrogen source, and sodium hydroxide solution to the pretreated wastewater, adjust the wastewater to a second pH value, stir and treat to obtain the adjusted wastewater; S140. Add struvite seed crystals to the adjusted wastewater, stir evenly, and then carry out struvite crystallization reaction to obtain a mixed system containing struvite. S150. The mixed system containing struvite is filtered to separate the solid and liquid components. The separated solid product is washed with deionized water and dried to constant weight to obtain struvite crystals.

2. The recycling method according to claim 1, characterized in that, In step S110, Ca 2+ The concentration threshold is 50 mg / L, and the total heavy metal content threshold is 0.4 mg / L.

3. The recycling method according to claim 1, characterized in that, In step S120, the preprecipitant is at least one of calcium hydroxide and sodium carbonate; The ratio of the amount of pre-precipitant added to the wastewater content is (0.1-0.5) g: 1 L.

4. The recycling method according to claim 1, characterized in that, In step S120, the first pH value is 7.8-8.2, and the reaction is stirred at a speed of 100-200 r / min for 5-15 min, followed by standing precipitation for 30-60 min.

5. The recycling method according to claim 1, characterized in that, In step S130, the magnesium source is one or a mixture of magnesium chloride and magnesium sulfate; The nitrogen source is one or a mixture of ammonium chloride and ammonium sulfate; The molar ratio of magnesium, phosphorus and nitrogen in the feed is (1.3-1.5):1.0:(1.0-1.3).

6. The recycling method according to claim 1, characterized in that, In step S130, the sodium hydroxide solution is added dropwise at a constant rate using a peristaltic pump, and the addition is completed within 30 minutes; the second pH value is 9.0-9.5, and then the mixture is stirred at a stirring speed of 150-250 r / min for 10-30 minutes.

7. The recycling method according to claim 1, characterized in that, In step S140, the amount of the struvite seed crystals added is 5% to 10% of the theoretical struvite yield.

8. The recycling method according to claim 1, characterized in that, In step S140, the temperature of the struvite crystallization reaction is 25-35℃, and the time is 2-6h.

9. The recycling method according to claim 1, characterized in that, In step S150, the solid product is washed 2-3 times with deionized water and dried at 38-42°C for 6-8 hours.

10. The recycling method according to claim 1, characterized in that, The struvite crystals have a crystallinity of ≥85%, a purity of ≥85%, and a phosphorus recovery rate of ≥75%.