A biomass hard carbon anode material, its preparation method and application

By introducing a washable salt-containing agent and segmented Joule heat treatment, the problems of metal migration and microsphere sintering in biomass hard carbon anode materials at high temperatures were solved, and a high-performance anode material suitable for sodium-ion batteries was prepared, improving the uniformity and processing performance of the material and meeting industrial needs.

CN123105597APending Publication Date: 2026-11-17NINGBO UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611142696.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for preparing biomass hard carbon anode materials suffer from problems such as metal component migration and agglomeration during high-temperature Joule heat treatment, localized excessive graphitization, uneven microsphere sintering, and difficulty in completely removing metals. These issues result in material structures that are unsuitable for sodium ion intercalation/adsorption and poor processing performance.

Method used

A washable desalination phase confinement agent is mixed with a biomass carbon source, and then purified by segmented Joule heat treatment and graded washing to form an amorphous carbon and locally ordered carbon microcrystalline structure. This inhibits metal migration and builds conductive channels, ensuring material uniformity and efficient metal removal.

Benefits of technology

This study achieved high tap density, good microsphere morphology, and low residual metal content in biomass hard carbon anode materials, which improved the first coulombic efficiency and cycle stability of sodium-ion batteries, reduced production energy consumption, and increased industrial production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105597A_ABST
    Figure CN123105597A_ABST
Patent Text Reader

Abstract

This invention belongs to the technical field of sodium-ion battery electrode materials, and relates to a biomass hard carbon anode material, its preparation method, and its application. To address the problems of easy sintering of microspheres, easy agglomeration of metal catalysts, and poor carbonization uniformity in the existing Joule heating preparation of biomass hard carbon, this invention involves a hydrothermal reaction of a biomass carbon source, a metal compound catalyst, and a washable salt-containing agent to obtain a composite microsphere precursor. After constructing the precursor layer, segmented Joule heat treatment is performed, followed by graded washing to obtain the target material. This material combines amorphous carbon with locally ordered microcrystals, with a carbon interlayer spacing of 0.36–0.42 nm and residual metal content below 2.0 wt%. When used as a sodium-ion battery anode, it exhibits high specific capacity and excellent cycle stability, making it suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of sodium-ion battery electrode materials, and relates to a biomass hard carbon anode material, its preparation method, and its application. Background Technology

[0002] Sodium-ion batteries are considered an important rechargeable battery technology for large-scale energy storage, low-speed power, and engineering equipment due to the abundance of sodium resources, low cost, and good safety. Hard carbon materials, with their large carbon interlayer spacing, good structural stability, and high sodium-ion storage potential, are among the most promising sodium-ion battery anode materials for industrialization.

[0003] Biomass carbon sources are widely available, inexpensive, and renewable, making them an important raw material for the preparation of hard carbon anode materials. Existing biomass hard carbon is typically prepared through hydrothermal pretreatment, furnace carbonization, or rapid Joule heating. Hydrothermal pretreatment is beneficial for forming carbonaceous microspheres and improving morphological uniformity; Joule heating offers advantages such as rapid heating rates, concentrated energy input, and short processing times, shortening the heat treatment cycle. However, for biomass precursors containing hydrothermal microspheres, relying solely on single-stage high-temperature Joule heating can easily lead to problems such as localized current concentration in the precursor layer, instantaneous release of volatile components, microsphere sintering, and inconsistent carbonization levels inside and outside the microspheres.

[0004] Metal compounds can promote local rearrangement of carbon structures during heat treatment, improving the conductivity and structural stability of materials. However, under rapid high-temperature conditions, metal components are prone to migration and aggregation, leading to excessive local graphitization or the formation of large metal particles. This is not only detrimental to obtaining hard carbon structures suitable for sodium ion intercalation / adsorption, but also increases the difficulty of subsequent acid leaching.

[0005] In existing technologies, porous carbon-coated metal nanoparticles can be prepared by hydrothermal reaction of transition metal salts with carbon sources followed by calcination and acid washing under an inert atmosphere. Another technology utilizes biomass carbon sources to prepare carbon microspheres hydrothermally, followed by Joule heating after pre-carbonization to obtain graphene-like micro / nanospheres. These technologies have certain significance in catalysts and graphene-like carbon microspheres for lithium-ion batteries, but their technological focus is not entirely the same as the comprehensive requirements of sodium-ion battery hard carbon anodes for moderately ordered structures, large interlayer spacing, low residual metal, and pore stability. Summary of the Invention

[0006] The purpose of this invention is to address the aforementioned problems in the existing technology by proposing a biomass hard carbon anode material. By introducing a washable salt-containing agent and combining it with initial resistance matching of the precursor layer, segmented Joule heat treatment, and graded washing and purification, the hydrothermal microspheres can simultaneously achieve confinement isolation, thermal buffering, establishment of conductive channels, and metal-assisted local structural rearrangement during the rapid carbonization process.

[0007] The objective of this invention can be achieved through the following technical solutions: A method for preparing a biomass hard carbon anode material, the method comprising the following steps: S1. Add biomass carbon source to water and mix evenly. Then add metal compound catalyst and elutable salt phase confinement agent in sequence. Then, after uniform stirring and ultrasonic dispersion, a mixed precursor solution is obtained. S2. The mixed precursor solution is subjected to a hydrothermal reaction. After the reaction is completed, the composite microsphere precursor is obtained by cooling, solid-liquid separation, washing and drying. S3. Construct a precursor layer from the composite microsphere precursor; S4. The precursor layer is subjected to segmented Joule heat treatment under an inert atmosphere. S5. The product after segmented Joule heat treatment is washed to obtain biomass hard carbon anode material.

[0008] In the above method, in step S1, the biomass carbon source is at least one of sugars, starches, celluloses, hemicelluloses, lignins, pectins, and chitosans and their derivatives; and / or the metal compound catalyst is a chloride, nitrate, sulfate, acetate, carbonate, hydroxide, oxide, complex, or organometallic compound containing at least one of iron, cobalt, nickel, copper, zinc, manganese, molybdenum, and tungsten.

[0009] Preferably, the carbon source and water, after being uniformly mixed, have a solid content of 5-45 wt% or a soluble monomer content of 0.2-3.0 mol / L.

[0010] In the above method, in step S1, the elutable salt phase confinement agent includes at least one of alkali metal salts, alkaline earth metal salts, and ammonium salts; wherein the anion of the salt is selected from at least one of chloride ions, sulfate ions, carbonate ions, nitrate ions, phosphate ions, oxalate ions, and citrate ions. The elutable salt phase confinement agent of the present invention is an inorganic or organic salt that can be removed by water washing or water-alcohol washing after heat treatment, including but not limited to alkali metal salts, alkaline earth metal salts, and ammonium salts. During hydrothermal and drying processes, the elutable salt phase confinement agent is distributed inside or between carbon microspheres, acting as a spatial isolation phase and thermal buffer phase during Joule heating, reducing sintering between microspheres and the migration and agglomeration of metal components; after being removed in subsequent washing processes, it can form channels in hard carbon materials that are conducive to electrolyte wetting and sodium ion migration.

[0011] In the above method, the mass ratio of metal compound catalyst to biomass carbon source is 1:(8-100); the mass ratio of elutable salt phase confinement agent to biomass carbon source is (0.03-2.0):1.

[0012] In the above method, in step S2, the hydrothermal reaction temperature is 150-220℃ and the reaction time is 6-24h.

[0013] Preferably, the controlled washing involves washing 1-3 times to remove free acidic components or unbound metal components while retaining a portion of the elutable salt phase.

[0014] In the hydrothermal treatment step, the mixed precursor solution is transferred to a hydrothermal reactor and reacted at 150-220℃ for 6-24 h, causing the biomass carbon source to dehydrate, condense, and nucleate, forming a carbonaceous microsphere precursor containing metal components and an elutable salt phase. After the reaction, solid-liquid separation, controlled washing, and drying are performed to obtain the carbon-metal-salt composite microsphere precursor. The controlled washing differs from complete desalting washing; its purpose is to remove free acidic impurities and excess unbound metal components while retaining a certain proportion of the elutable salt phase.

[0015] In the above method, in step S3, the precursor layer thickness is 0.3-8 mm and the areal density is 5-200 mg / cm³. 2 .

[0016] Preferably, the initial resistance of the precursor layer is within a stable current-carrying range, ranging from 0.2 to 80 Ω. This invention reduces partial discharge, overheating, and uneven temperature distribution during Joule heating by controlling the precursor layer thickness, compaction degree, salt phase content, and electrode contact state.

[0017] In the above method, step S4, the segmented Joule heat treatment includes: The first section is the conductive framework formation section, with a processing temperature of 400-650℃ and a processing time of 2-20s; The second stage is the salt-confined-metal-assisted structural rearrangement stage, with a processing temperature of 700-1000℃ and a processing time of 3-30s.

[0018] In the above method, step S4, the segmented Joule heat treatment also includes a short-time structural stabilization section. The processing temperature of the short-time structural stabilization section is 800-1100℃, the processing time for a single session is 1-10s, the number of pulses is 1-5, and the interval between adjacent pulses is 2-30s.

[0019] Preferably, the heating rate of the Joule heat treatment is 200-3000℃ / s, and the total high-temperature treatment time does not exceed 80 s.

[0020] In the segmented Joule heat treatment process, the first segment is the conductive framework formation segment, which is used to remove residual moisture and volatile components and form a preliminary continuous carbon framework; the second segment is the salt phase confinement-metal-assisted structure rearrangement segment, which is used to activate the metal components to promote local rearrangement of the carbon layer, while using the elutable salt phase to inhibit the growth of metal particles and the over-sintering of microspheres; if necessary, a third segment, the short-term structure stabilization segment, can also be set to further stabilize the pore structure and locally ordered carbon microcrystals in a short pulse manner.

[0021] Preferably, in the staged washing and purification step, the elutable salt phase is first removed with water or a water-alcohol mixture, then the residual metal components are removed with acid, and finally the material is washed until neutral and dried to obtain the biomass hard carbon anode material. This staged washing method avoids the collapse of pores or local structural damage caused by direct strong acid treatment, and reduces the final residual metal content of the material.

[0022] The present invention also provides a biomass hard carbon anode material, which is prepared by the above method and has an average particle size of 0.2-8 μm; Furthermore, the biomass hard carbon anode material possesses a structure where amorphous carbon and locally ordered carbon microcrystals coexist, with a carbon layer spacing d. 002 The wavelength range is 0.36-0.42 nm, and the residual metal content is less than 2.0 wt%.

[0023] Preferably, the biomass hard carbon anode material is a microsphere, a near-spherical particle, or a secondary aggregate.

[0024] The present invention also provides a sodium-ion battery comprising the above-mentioned biomass hard carbon anode material.

[0025] Compared with the prior art, the present invention has the following beneficial effects: 1. This invention introduces a washable salt-containing agent that acts as a physical isolation barrier and thermal buffer during Joule heating, effectively inhibiting the melting, sintering, and agglomeration of carbon microspheres, thus maintaining good microsphere morphology in the final product and ensuring high tap density and processing performance.

[0026] 2. The confinement effect of the salt phase in this invention "pins" the metal catalyst nanoparticles in situ, greatly inhibiting their migration and growth at high temperatures. This not only ensures that the metal catalyst efficiently promotes local carbon structure rearrangement at the nanoscale, but also makes subsequent acid leaching removal more thorough, ultimately obtaining high-purity hard carbon material with extremely low residual metal content (<2.0 wt%).

[0027] 3. This invention employs a segmented Joule heating process, which pre-constructs a conductive framework in the low-temperature section to ensure a uniform current distribution in the high-temperature section. This fundamentally avoids partial discharge, arcing, and hot spot runaway, thereby improving process safety and product uniformity.

[0028] 4. The hard carbon material prepared by this invention has both amorphous carbon regions and locally ordered carbon microcrystals, and forms a suitable carbon interlayer spacing of 0.36-0.42 nm, which is conducive to the rapid insertion / extraction of sodium ions and ensures high initial coulombic efficiency and cycling stability.

[0029] 5. The entire high-temperature heat treatment process of this invention is completed within tens of seconds. Compared with the hours or even tens of hours of traditional furnace carbonization, the production efficiency is increased by hundreds of times and the energy consumption is significantly reduced, which fully meets the requirements of cost and efficiency for large-scale industrial production. Attached Figure Description

[0030] Figure 1 This is a SEM image of the sodium-ion battery anode material prepared in Example 6 of this invention.

[0031] Figure 2 This is the EIS diagram of the sodium-ion battery anode material prepared in Example 6 of this invention.

[0032] Figure 3 This is the XRD pattern of the sodium-ion battery anode material prepared in Example 6 of this invention. Detailed Implementation

[0033] The following are specific embodiments of the present invention, which further describe the technical solution of the present invention, but the present invention is not limited to these embodiments. Without departing from the core idea of ​​the present invention, those skilled in the art can make equivalent substitutions or adjustments to the type of carbon source, the type of metal compound, the type of elutable salt phase confinement agent, the thickness of the precursor layer, the Joule heating program, and the washing conditions.

[0034] Unless otherwise specified, in the following examples, the hydrothermal products were collected by centrifugation and then washed 1-2 times with deionized water in a controlled manner, and the drying temperature was 70°C. The Joule heat treatment atmosphere was argon, and the gas flow rate was 80 mL / min; Desalination is achieved by washing with deionized water using agitation. Pickling was performed using 1 mol / L hydrochloric acid. After pickling, the solution was washed with deionized water until neutral and then vacuum dried at 80°C for 12 hours.

[0035] Example 1:

[0036] S1. Dissolve 18 g of glucose in 100 mL of deionized water and stir for 30 min to obtain a glucose solution; add 0.48 g of ferric chloride and 3.0 g of sodium chloride as elutable salt-containing agents and sonicate for 1 h.

[0037] S2. The mixed solution was transferred to a hydrothermal reactor and reacted at 180°C for 12 h. After cooling, the precipitate was collected by centrifugation, washed in a controlled manner, and dried to obtain the carbon-iron-salt composite microsphere precursor.

[0038] S3. Spread the precursor evenly between two pieces of graphite paper and press it lightly into a precursor layer of about 2.0 mm thickness. The initial resistance is measured to be within the range where it can be stably energized.

[0039] S4. Perform segmented Joule heat treatment under argon protection: the first stage is heated to 550℃ and held for 8 s, and the second stage is heated to 850℃ and held for 12 s.

[0040] S5. After cooling, the material is first washed with water to remove salt, then acid washed to remove residual iron components, and dried to obtain a hard carbon anode material with an average particle size of 0.5 μm, a carbon interlayer spacing d002 of 0.39 nm, and a residual metal content of 0.3 wt%.

[0041] Example 2:

[0042] The difference from Example 1 lies only in that sodium carbonate was used as the elutable salt confinement agent, with an addition amount of 2.5 g; the hydrothermal temperature was 180°C, and the hydrothermal time was 16 h; the precursor layer thickness was approximately 1.5 mm. The first stage of Joule heat treatment was held at 520°C for 10 s, and the second stage was held at 830°C for 15 s. After water washing, desalting, acid washing, and drying, a hard carbon anode material was obtained.

[0043] Example 3:

[0044] The difference from Example 1 lies only in that 18 g of glucose was dissolved in 100 mL of deionized water, and 0.48 g of nickel nitrate and 3.5 g of sodium sulfate were added as elutable desalting phase confinement agents. After ultrasonic dispersion for 1 h, a hydrothermal reaction was carried out at 170 °C for 16 h. The resulting composite microsphere precursor was compacted into a precursor layer of approximately 2.5 mm thickness after controlled washing and drying. The Joule heat treatment consisted of a first stage at 540 °C for 8 s and a second stage at 800 °C for 15 s, followed by water washing, acid washing, and drying to obtain the hard carbon anode material.

[0045] Example 4:

[0046] The difference from Example 1 lies only in that 18 g of glucose, 0.60 g of cobalt nitrate, and a mixed elutable salt-containing agent composed of sodium chloride / sodium sulfate in a 1:1 mass ratio were added to 100 mL of deionized water. After stirring and ultrasonic dispersion, the mixture was hydrothermally reacted at 190°C for 12 h. The resulting precursor, after drying, formed a precursor layer approximately 2.0 mm thick. Joule heat treatment was performed with the following steps: first, 560°C for 6 s; second, 880°C for 10 s; and third, a short pulse at 930°C for 3 s, repeated twice. After graded washing and purification, a hard carbon anode material was obtained.

[0047] Example 5:

[0048] The difference from Example 1 lies only in that 34.2 g of sucrose was dissolved in 100 mL of deionized water, and 0.60 g of ferric chloride and 4.0 g of sodium chloride were added as elutable salt-confining agents. After ultrasonic dispersion for 1 h, the mixture was hydrothermally reacted at 180 °C for 18 h. The resulting carbon-iron-salt composite microsphere precursor was dried and spread into a precursor layer approximately 3.0 mm thick. Joule heat treatment was performed with a first stage at 550 °C for 10 s and a second stage at 850 °C for 15 s. After water washing, desalting, acid washing, and drying, a hard carbon anode material was obtained.

[0049] Example 6:

[0050] The difference from Example 1 lies only in that 16.2 g of starch was dispersed in 100 mL of deionized water, and 0.48 g of ferric chloride and 2.0 g of trisodium phosphate were added as elutable desalting phase confinement agents. After stirring and ultrasonic dispersion, the mixture was hydrothermally reacted at 200°C for 16 h. The resulting precursor was then controlled washing and drying, and compacted into a precursor layer approximately 2.0 mm thick. Joule heat treatment was performed with a first stage at 530°C for 12 s and a second stage at 820°C for 18 s, followed by water washing, acid washing, and drying to obtain the hard carbon anode material.

[0051] Figure 1 This is a SEM image of the sodium-ion battery anode material prepared in Example 6 of the present invention. As can be seen from the image, the obtained material has a spherical or microspherical morphology, the particles are relatively uniformly dispersed, and there is no obvious sintering or agglomeration. This indicates that the elutable salt phase confinement and segmented Joule heat treatment are beneficial to maintaining the precursor microsphere structure.

[0052] Figure 2 The image shows the EIS diagram of the sodium-ion battery anode material prepared in Example 6 of this invention. As can be seen from the image, the obtained electrode exhibits a small charge transfer impedance and good interfacial transport characteristics, indicating that the material is beneficial to improving the electron / ion co-transport capability after metal-assisted local structural rearrangement.

[0053] Figure 3This is the XRD pattern of the sodium-ion battery anode material prepared in Example 6 of the present invention. As can be seen from the figure, the obtained material exhibits broadened diffraction peaks in the characteristic region of carbon materials, indicating that it is mainly composed of amorphous hard carbon structure and contains locally ordered carbon microcrystalline structure, which is beneficial to the insertion / extraction of sodium ions.

[0054] Example 7:

[0055] The difference from Example 1 lies only in that sodium carboxymethyl cellulose was dispersed in deionized water at a solid content of 20 wt%, and nickel nitrate and sodium chloride were added as elutable salt-confining agents, wherein the mass ratio of nickel nitrate hexahydrate to sodium carboxymethyl cellulose was 1:30, and the mass ratio of sodium chloride to sodium carboxymethyl cellulose was 0.20:1. The mixture was hydrothermally reacted at 200°C for 20 h, and the resulting precursor was spread into a precursor layer approximately 1.8 mm thick. Joule heat treatment was performed with a first stage at 570°C for 8 s and a second stage at 900°C for 8 s. After graded washing and purification, hard carbon anode material was obtained.

[0056] Example 8:

[0057] The difference from Example 1 lies only in that sodium lignosulfonate was dispersed in deionized water to form a dispersion with a solid content of 15 wt%. Zinc acetate dihydrate and sodium carbonate were added as salt-confining agents for elution. After ultrasonic dispersion for 2 h, a hydrothermal reaction was carried out at 180 °C for 20 h. The resulting composite precursor was dried and compacted into a precursor layer approximately 2.8 mm thick. The Joule heat treatment consisted of a first stage at 500 °C for 15 s and a second stage at 780 °C for 20 s. Afterward, the material was washed with water for desalting, washed with a weak acid, and dried to obtain a hard carbon anode material.

[0058] Example 9:

[0059] The difference from Example 1 lies only in that xylan was dispersed in deionized water at a solid content of 25 wt%, and ferric chloride, nickel nitrate, and a mixed elutable salt-limiting agent composed of sodium chloride / sodium sulfate at a mass ratio of 1:1 were added. The total mass ratio of ferric chloride and nickel nitrate hexahydrate to xylan was 1:25, and the mass ratio of the mixed elutable salt-limiting agent to xylan was 0.30:1. The mixture was hydrothermally reacted at 190°C for 18 h. The resulting precursor was constructed as a precursor layer approximately 2.2 mm thick. Joule heat treatment was performed with the first stage at 560°C for 8 s, the second stage at 870°C for 12 s, and the third stage at 950°C for 4 s. After graded washing and purification, hard carbon anode material was obtained.

[0060] Example 10: The difference from Example 1 lies only in that chitosan was dispersed in a 1 wt% aqueous acetic acid solution to form a dispersion with a solid content of 10 wt%. Ferric chloride and ammonium chloride were added as elutable salt-limiting agents. After ultrasonic dispersion, the mixture was hydrothermally reacted at 170°C for 12 h. The resulting precursor was spread into a precursor layer of approximately 1.5 mm thickness after controlled washing and drying. Joule heat treatment was performed with the following steps: first, 520°C for 10 s; second, 840°C for 10 s; and third, a short pulse at 900°C for 3 s, repeated twice. After water washing, desalting, acid washing, and drying, a hard carbon anode material was obtained.

[0061] Comparative Example 1: The only difference from Example 1 is that no elutable salt phase confinement agent was added.

[0062] Comparative Example 2: The only difference from Example 1 is that a single-stage Joule heat treatment is used, i.e., the temperature is 850°C and the time is 12 seconds.

[0063] Comparative Example 3: The difference from Example 1 is that conventional furnace carbonization is used, in which the material is placed in a tube furnace, heated to 850°C at 5°C / min under argon protection, and held for 2 hours.

[0064] Comparative Example 4: The only difference from Example 1 is that the metal compound catalyst ferric chloride was not added.

[0065] Comparative Example 5: The only difference from Example 1 is that the mass ratio of sodium chloride to biomass carbon source is 0.01:1.

[0066] Comparative Example 6: The only difference from Example 1 is that the mass ratio of sodium chloride to biomass carbon source is 5:1.

[0067] Performance testing: The prepared negative electrode material was mixed with conductive carbon black and polyvinylidene fluoride at a mass ratio of 8:1:1, and N-methylpyrrolidone was added to form a slurry. This slurry was then coated onto copper foil and vacuum dried to form an electrode sheet. Using sodium metal as the counter electrode and 1 mol / L NaClO4 / ethylene carbonate-dimethyl carbonate (ethylene carbonate-dimethyl carbonate volume ratio 1:1) as the electrolyte, a CR2032 coin cell was assembled. The specific capacity was tested at a current density of 100 mA / g within the voltage range of 0.01-3V, and the results are shown in Table 1 below.

[0068] Table 1: Performance test results of the anode materials prepared in the examples and comparative examples

[0069] The embodiments herein cover any points not exhaustively within the scope of the technical claims of this invention, as well as new technical solutions formed by equivalent substitutions of one or more technical features in the embodiments. These are all within the scope of the claims of this invention. Furthermore, in all listed or unlisted embodiments of this invention, each parameter in the same embodiment merely represents an instance (i.e., a feasible solution) of its technical solution, and there is no strict coordination or limitation relationship between the parameters. The parameters can be substituted for each other without violating axioms and the claims of this invention, unless otherwise stated.

[0070] The technical means disclosed in this invention are not limited to those described above, but also include technical solutions composed of any combination of the above technical features. The above descriptions are specific embodiments of this invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of this invention, and these improvements and modifications are also considered within the scope of protection of this invention.

[0071] The specific embodiments described herein are merely illustrative of the spirit of the invention. Those skilled in the art to which this invention pertains may make various modifications or additions to the described specific embodiments or use similar methods to substitute them, without departing from the spirit of the invention or exceeding the scope defined by the appended claims.

Claims

1. A method for preparing a biomass hard carbon anode material, characterized in that, The method includes the following steps: S1. Add biomass carbon source to water and mix evenly. Then add metal compound catalyst and elutable salt phase confinement agent in sequence. Then, after uniform stirring and ultrasonic dispersion, a mixed precursor solution is obtained. S2. The mixed precursor solution is subjected to a hydrothermal reaction. After the reaction is completed, the composite microsphere precursor is obtained by cooling, solid-liquid separation, washing and drying. S3. Construct a precursor layer from the composite microsphere precursor; S4. The precursor layer is subjected to segmented Joule heat treatment under an inert atmosphere. S5. The product after segmented Joule heat treatment is washed to obtain biomass hard carbon anode material.

2. The method according to claim 1, characterized in that, In step S1, the biomass carbon source is at least one of sugars, starches, celluloses, hemicelluloses, lignins, pectins, and chitosans and their derivatives; and / or the metal compound catalyst is a chloride, nitrate, sulfate, acetate, carbonate, hydroxide, oxide, complex, or organometallic compound containing at least one of iron, cobalt, nickel, copper, zinc, manganese, molybdenum, and tungsten.

3. The method according to claim 1, characterized in that, In step S1, the elutable salt phase confinement agent includes at least one of alkali metal salt, alkaline earth metal salt, and ammonium salt; wherein the anion of the salt is selected from at least one of chloride ion, sulfate ion, carbonate ion, nitrate ion, phosphate ion, oxalate ion, and citrate ion.

4. The method according to claim 1, characterized in that, The mass ratio of metal compound catalyst to biomass carbon source is 1:(8-100); the mass ratio of elutable salt phase confinement agent to biomass carbon source is (0.03-2.0):

1.

5. The method according to claim 1, characterized in that, In step S2, the hydrothermal reaction temperature is 150-220℃, and the reaction time is 6-24h.

6. The method according to claim 1, characterized in that, In step S3, the precursor layer has a thickness of 0.3-8 mm and a surface density of 5-200 mg / cm³. 2 .

7. The method according to claim 1, characterized in that, In step S4, the segmented Joule heat treatment includes: the first segment is the conductive framework formation segment, with a treatment temperature of 400-650℃ and a treatment time of 2-20s; the second segment is the salt phase confinement-metal-assisted structure rearrangement segment, with a treatment temperature of 700-1000℃ and a treatment time of 3-30s.

8. The method according to claim 7, characterized in that, In step S4, the segmented Joule heat treatment also includes a short-time structural stabilization section. The processing temperature of the short-time structural stabilization section is 800-1100℃, the processing time for a single session is 1-10s, the number of pulses is 1-5, and the interval between adjacent pulses is 2-30s.

9. A biomass hard carbon anode material, characterized in that, The negative electrode material is prepared by the method described in any one of claims 1-8, and has an average particle size of 0.2-8 μm; Furthermore, the biomass hard carbon anode material possesses a structure where amorphous carbon and locally ordered carbon microcrystals coexist, with a carbon layer spacing d. 002 The wavelength range is 0.36-0.42 nm, and the residual metal content is less than 2.0 wt%.

10. A sodium-ion battery, characterized in that, The sodium-ion battery includes the biomass hard carbon anode material as described in claim 9.