A hollow silicon-carbon composite material, its preparation method and application

Hollow spherical silicon-carbon composite materials were prepared by mechanical ball milling and oxalate-assisted pyrolysis, which solved the problems of volume expansion and conductivity of silicon-based anode materials in lithium-ion batteries. This method achieved stable interfacial bonding and high capacity characteristics, making it suitable for large-scale production.

CN123105643APending Publication Date: 2026-11-17TAIYUAN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611267615.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing silicon-based anode materials in lithium-ion batteries suffer from limited cycle stability and conductivity due to volume expansion and semiconductor properties. Simple physical mixing makes it difficult to achieve a stable interfacial bond, leading to rapid capacity decay.

Method used

Hollow spherical hollow silicon-carbon composite materials were prepared by mechanical ball milling and oxalate-assisted pyrolysis. The starch molecular chains were broken by mechanical shearing and formed hydrogen bonds with the surface of nano-silicon to form a strong Si−C interface. The decomposition of oxalate was used to form a hollow shell and a catalytic graphitization carbon shell to achieve a stable interfacial bond.

Benefits of technology

It effectively alleviates the volume expansion of silicon, improves conductivity and electrochemical stability, is suitable for large-scale production, and exhibits excellent discharge specific capacity and cycle stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105643A_ABST
    Figure CN123105643A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of lithium-ion battery technology, specifically relating to a hollow silicon-carbon composite material, its preparation method, and its applications. The hollow silicon-carbon composite material of this invention uses silicon as the active component and starch as the carbon precursor. Through the synergistic effect of mechanical ball milling and oxalate-assisted pyrolysis, uniform mixing and interface pre-activation of the raw materials are achieved, and a composite material with a hollow porous structure and a stable silicon-carbon interface is constructed in situ. This material has a large specific surface area and excellent volume expansion adaptability. The carbon shell acts as a mixed conductor of ions and electrons and is highly compatible with silicon, improving conductivity and preventing silicon particle aggregation. When used as a negative electrode material for lithium-ion batteries, it exhibits excellent discharge specific capacity and cycle stability. This invention uses a mechanical ball milling method, which is simple to operate, low in cost, and easy to scale up. The prepared hollow silicon-carbon composite material has potential application value in lithium-ion batteries, energy storage, and adsorption fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium-ion battery technology, specifically relating to a hollow silicon-carbon composite material, its preparation method, and its application. Background Technology

[0002] With the rapid development of electric vehicles and large-scale energy storage industries, the market has placed higher demands on the energy density of lithium-ion batteries. As a core component of lithium-ion batteries, the specific capacity of the anode material is one of the key factors determining the battery's energy density. Therefore, the development of new high-capacity anode materials is urgently needed.

[0003] Silicon, due to its high capacity of 4200 mAh g -1 Silicon, with its theoretical specific capacity, low delithiation potential, and abundant resource reserves, is considered the most promising next-generation lithium-ion battery anode material. However, silicon undergoes volume expansion and contraction exceeding 300% during lithiation / delithiation, leading to the breakage, pulverization, and even detachment of active material particles. This also triggers continuous rupture and regeneration of the solid electrolyte interfacial film on the electrode surface, ultimately resulting in rapid capacity decay and poor cycle stability. Furthermore, silicon's intrinsic semiconductor properties limit its rate performance. Carbon materials possess excellent conductivity and structural stability, which can compensate for silicon's semiconductor defects. However, simply physically mixing silicon and carbon materials is insufficient to achieve a stable interfacial bond, and silicon easily desorbs from the carbon material during cycling. Therefore, there is an urgent need to design a silicon-carbon composite material with strong interfacial bonding and an integrated structure. By constructing a seamless interface, the high capacity characteristics of silicon can be maximized, while fully utilizing the structural stability and conductivity of the carbon matrix, fundamentally promoting the large-scale commercial application of silicon-based anode materials.

[0004] Currently, the main methods for preparing silicon-carbon composite materials are high-temperature pyrolysis, chemical vapor deposition (CVD), spray drying, and other methods to obtain the final material. CVD can deposit silicon and carbon layers on a substrate, achieving uniform carbon coverage, but its relatively high production cost hinders industrialization. While spray drying offers fast drying speeds and produces products with uniform particle size and good flowability, it also consumes a lot of energy, requires significant equipment investment, and incurs high maintenance costs. Therefore, there is a need to find a simple, low-cost, and easily scalable method for preparing silicon-carbon anode materials. Summary of the Invention

[0005] In view of this, the purpose of this invention is to provide a hollow silicon-carbon composite material, its preparation method, and its application. The hollow silicon-carbon composite material prepared by this invention has a hollow spherical structure, with nano-silicon particles encapsulated inside a carbon shell, leaving a buffer gap between the nano-silicon particles and the inner wall of the carbon shell. This effectively solves the problem of volume expansion of silicon anodes and significantly improves their conductivity and electrochemical stability. Moreover, the process is simple and suitable for large-scale production.

[0006] To achieve the above objectives, the technical solution of the present invention is as follows:

[0007] In a first aspect, the present invention provides a hollow silicon-carbon composite material, which uses silicon source as active component and starch as carbon precursor. Through the synergistic effect of mechanical ball milling and oxalate-assisted pyrolysis, the raw materials are uniformly mixed and the interface is pre-activated, and a composite material with a hollow porous structure and a stable silicon-carbon interface is constructed in situ. In the hollow porous structure, nano-silicon particles are encapsulated inside the carbon shell, and a buffer gap is left between them and the inner wall of the carbon shell.

[0008] In a second aspect, the present invention provides a method for preparing the hollow silicon-carbon composite material described in the first aspect, comprising the following steps:

[0009] Step 1: Disperse the silicon source in anhydrous ethanol, then add starch and oxalate, stir and mix, and then perform mechanical ball milling, drying, manual grinding and sieving in sequence to obtain the precursor;

[0010] Step 2: The precursor is carbonized, and after acid washing, water washing and drying, hollow silicon-carbon composite material is obtained.

[0011] In the above technical solution, mechanical ball milling plays a dual role at room temperature: on the one hand, it promotes the interaction between hydroxyl groups and oxalate groups in starch, modifying the physicochemical properties of the starch surface and preventing foaming of starch during subsequent pyrolysis; on the other hand, it significantly reduces the particle size of each component, enhances reactivity, and lays the foundation for uniform compounding. During the subsequent carbonization process, the gas released from oxalate decomposition inflates the starch to form a hollow shell structure, while the amorphous carbon produced by starch pyrolysis effectively isolates the electrolyte from direct contact with nano-silicon and alleviates the volume expansion of silicon. More importantly, the mechanical shearing action during ball milling breaks down starch molecular chains and exposes a large number of hydroxyl groups. These hydroxyl groups form hydrogen bonds with the natural oxide layer (SiO2) on the surface of nano-silicon, causing the silicon-carbon interface to transition from simple physical adsorption to chemical bonding. This strong interfacial interaction further transforms into robust Si−C bonds after carbonization, resulting in a thinner SiO2 layer at the interface and a tighter contact between silicon and carbon, effectively buffering volume expansion and promoting electron conduction and interfacial stability. In addition, the metal species produced by the decomposition of oxalate catalyze the graphitization of carbon microspheres, causing the carbon shell to form a graphitized structure, which further improves the conductivity of the material.

[0012] Furthermore, the starch in step 1 is one or more of rice starch, potato starch, corn starch, cassava starch, sweet potato starch, bean starch, and wheat starch.

[0013] Further, in step 1, the silicon source is one or more of nano-silicon, tetraethyl orthosilicate, 3-aminopropyltriethoxysilane, and 3-glycidoxypropyltrimethoxysilane, and its addition amount is 5% to 30% of the total mass of the carbon source. The aim is to achieve uniform molecular-level dispersion of the silicon source in the solid matrix, while simultaneously inhibiting its premature hydrolysis and self-polymerization through a non-aqueous medium. This ensures that the silicon source reaches the starch / oxalate surface in the form of active monomers, thereby enabling targeted condensation reactions with the hydroxyl groups of starch in subsequent processing to form a stable Si−O−C covalent bond interface.

[0014] Further, in step 1, the oxalate is one or more of cobalt oxalate, potassium oxalate, iron oxalate, ammonium oxalate, zinc oxalate, manganese oxalate, and nickel oxalate, and its addition amount is 30% to 60% of the total mass of the carbon source.

[0015] Furthermore, the conditions for mechanical ball milling in step 1 are: ball-to-material ratio of 10:1, ball milling speed of 400~800 r / min, and ball milling time of 1~6 h.

[0016] Furthermore, the carbonization conditions in step 2 are as follows: the temperature is increased in stages under a nitrogen atmosphere. The conditions for the staged temperature increase include first increasing the temperature to 180-300 ℃ at a heating rate of 1-5 ℃ / min and holding it at that temperature for 1-4 h; then increasing the temperature to 800-1200 ℃ at a heating rate of 1-5 ℃ / min and holding it at that temperature for 1-6 h.

[0017] Furthermore, the acid used for pickling in step 2 is one or more of hydrochloric acid, sulfuric acid, and nitric acid.

[0018] Thirdly, the present invention provides the application of the hollow silicon-carbon composite material described in the first aspect as a negative electrode material for lithium-ion batteries.

[0019] Fourthly, the present invention provides a lithium-ion battery anode material, including the hollow silicon-carbon composite material described in the first aspect.

[0020] Fifthly, the present invention provides a lithium-ion battery, comprising the lithium-ion battery negative electrode material as described in the fourth aspect.

[0021] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0022] (1) The hollow silicon-carbon composite material prepared by the present invention does not require the addition of any template agent during the preparation process. The silicon source, starch and oxalate are mixed evenly by physical mixing ball milling. Hollow silicon-carbon microspheres are obtained by one-step carbonization. The method is simple, the process is short, the cost is low, and it is easy to scale up.

[0023] (2) The starch molecular chains break and the exposed hydroxyl groups under mechanical shearing form hydrogen bonds with the natural oxide layer (SiO2) on the surface of nano-silicon, realizing the transition from simple physical adsorption to interfacial chemical bonding. This strong interfacial interaction helps to form a robust Si−C interface after carbonization, effectively buffering volume expansion and forming a tighter Si−C contact, which is beneficial to electron conduction and interfacial stability.

[0024] (3) The gas released during the thermal decomposition of oxalate blows starch to form a hollow shell structure. At the same time, the metal species produced by the decomposition catalyze the graphitization of carbon microspheres, causing the carbon shell to form a graphitized structure. This composite material has a low I D / I G The value indicates that the carbon shell structure has a high degree of graphitization, thus endowing the material with excellent electron transport capabilities.

[0025] (4) The hollow silicon-carbon composite material of the present invention has a large specific surface area (117 m²). 2 With its excellent volume expansion adaptability and hollow structure providing internal buffer space, the carbon shell effectively mitigates the volume change of silicon during lithium insertion / extraction, preventing silicon particle breakage and agglomeration, thereby improving the cycle life of the composite material. As an electron transport network, the carbon shell promotes ion transport by constructing open channels and is highly compatible with silicon, improving conductivity and preventing silicon particle aggregation. When used as a negative electrode material for lithium-ion batteries, this material exhibits excellent discharge specific capacity and cycle stability. Attached Figure Description

[0026] Figure 1 The image shows the Raman spectrum of the hollow silicon-carbon composite material prepared in Example 1 of this invention.

[0027] Figure 2 The image shows the X-ray powder diffraction pattern of the hollow silicon-carbon composite material prepared in Example 1 of this invention.

[0028] Figure 3 These are scanning electron microscope (SEM) images of the hollow silicon-carbon composite material prepared in Example 1 of this invention at different magnifications.

[0029] Figure 4 The image shows the N2 adsorption-desorption isotherm of the hollow silicon-carbon composite material prepared in Example 1 of this invention.

[0030] Figure 5 This is a pore size distribution diagram of the hollow silicon-carbon composite material prepared in Example 1 of the present invention.

[0031] Figure 6 The Nyquist impedance diagram is shown for the hollow silicon-carbon composite material prepared in Example 1 of this invention.

[0032] Figure 7The image shows the cyclic voltammetry curves of the hollow silicon-carbon composite material prepared in Example 1 of this invention at different scan rates.

[0033] Figure 8 The graph shows the rate performance of the hollow silicon-carbon composite material prepared in Example 1 of this invention at different current densities.

[0034] Figure 9 The graph shows the cycling performance of the hollow silicon-carbon composite material prepared in Example 1 of this invention at a current density of 1 A / g. Detailed Implementation

[0035] To facilitate understanding of the present invention, a more comprehensive description will be given below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a thorough and complete understanding of the disclosure of the present invention.

[0036] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of the invention.

[0037] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this invention can be purchased from the market or prepared by existing methods.

[0038] Example 1

[0039] (1) 0.8 g of nano-silicon powder was added to 30 mL of anhydrous ethanol and dispersed evenly. Then, 4 g of corn starch and 2 g of cobalt oxalate were added in sequence. After stirring and mixing, the mixture was transferred to a ball mill jar and ball milled at 400 r / min for 6 h under the condition of ball-to-material ratio of 10:1. The mixture was then mixed evenly. The resulting slurry was vacuum dried at 80 °C for 12 h. After manual grinding, the slurry was passed through a 350 mesh sieve to obtain a solid powder precursor.

[0040] (2) The precursor was carbonized in a nitrogen atmosphere. First, the temperature was raised to 260℃ at a heating rate of 2℃ / min and held for 2 h. Then, the temperature was raised to 800℃ at a heating rate of 5℃ / min and carbonized for 4 h. After that, it was naturally cooled to room temperature. Then, the product was repeatedly washed with hydrochloric acid solution and distilled water to remove impurities and metal elements. Finally, it was dried in a vacuum oven at 80℃ to obtain hollow silicon-carbon composite material.

[0041] The Raman spectrum of the hollow silicon-carbon composite material prepared in this embodiment is as follows: Figure 1As shown in the figure, the intensity ratio (ID / IG) of the D peak to the G peak of the sample is low, indicating a high degree of graphitization. The high-intensity silicon peak also indicates good purity and crystallinity of the sample. The X-ray powder diffraction pattern of the hollow silicon-carbon composite material prepared in this embodiment is shown below. Figure 2 As shown in the figure, the sample exhibits characteristic peaks of both silicon and carbon, indicating the successful preparation of the silicon-carbon composite material. The scanning electron microscope image is shown below. Figure 3 As shown in the figure, the material exhibits a typical hollow structure. The N2 adsorption-desorption isotherm diagram is shown below. Figure 4 As shown in the figure, the adsorption-desorption isotherm is a typical Type IV isotherm, exhibiting a significant hysteresis loop in the higher relative pressure range (P / P0≈0.4–1.0), indicating that the material possesses a distinct mesoporous structure. The pore size distribution curve is shown below. Figure 5 As shown in the figure, the peak of the pore size distribution is concentrated around 3.5 nm, which is beneficial for the electrolyte to fully wet the pores and promote the rapid transport of lithium ions.

[0042] Example 2

[0043] (1) 0.2 g of tetraethyl orthosilicate was added to 40 mL of anhydrous ethanol and dispersed evenly. Then, 4 g of cassava starch and 2 g of ferric oxalate were added in sequence. After stirring and mixing, the mixture was transferred to a ball mill jar and ball milled at 500 r / min for 2 h with a ball-to-material ratio of 10:1. The mixture was then mixed evenly. The resulting slurry was vacuum dried at 80 °C for 12 h. After manual grinding, the slurry was passed through a 350 mesh sieve to obtain a solid powder precursor.

[0044] (2) The precursor was carbonized in a nitrogen atmosphere. First, the temperature was raised to 180 °C at a rate of 1 °C / min and held for 2 h. Then, the temperature was raised to 1000 °C at a rate of 5 °C / min and carbonized for 6 h. After that, it was naturally cooled to room temperature. Then, the product was repeatedly washed with hydrochloric acid solution and distilled water to remove impurities and metal elements. Finally, it was dried in a vacuum oven at 80 °C to obtain hollow silicon-carbon composite material.

[0045] Example 3

[0046] (1) 0.8 g of tetraethyl orthosilicate was added to 40 mL of anhydrous ethanol and dispersed evenly. Then, 4 g of cassava starch and 1.2 g of zinc oxalate were added in sequence. After stirring and mixing, the mixture was transferred to a ball mill jar and ball milled at 600 r / min for 2 h under the condition of ball-to-material ratio of 10:1. The mixture was then mixed evenly. The resulting slurry was vacuum dried at 80 °C for 12 h. After manual grinding, the slurry was passed through a 350 mesh sieve to obtain a solid powder precursor.

[0047] (2) The precursor was carbonized in a nitrogen atmosphere. First, the temperature was raised to 300 °C at a rate of 4 °C / min and held for 2 h. Then, the temperature was raised to 1000 °C at a rate of 5 °C / min and held for 3 h. After that, it was naturally cooled to room temperature. Then, the product was repeatedly washed with hydrochloric acid solution and distilled water to remove impurities and metal elements. Finally, it was dried in a vacuum oven at 80 °C to obtain hollow silicon-carbon composite material.

[0048] Example 4

[0049] (1) 1.2 g of 3-aminopropyltriethoxysilane was added to 60 mL of anhydrous ethanol and dispersed evenly. Then, 4 g of rice starch and 2.4 g of potassium oxalate were added in sequence. After stirring and mixing, the mixture was transferred to a ball mill jar and ball milled at 600 r / min for 4 h with a ball-to-material ratio of 10:1. The mixture was then dried under vacuum at 80 °C for 12 h. After manual grinding, the mixture was passed through a 350 mesh sieve to obtain a solid powder precursor.

[0050] (2) The precursor was carbonized in a nitrogen atmosphere. First, the temperature was raised to 240℃ at a heating rate of 3℃ / min and held for 2 hours. Then, the temperature was raised to 1200℃ at a heating rate of 5℃ / min and held for 2 hours. After that, it was naturally cooled to room temperature. Then, the product was repeatedly washed with hydrochloric acid solution and distilled water to remove impurities and metal elements. Finally, it was dried in a vacuum oven at 80℃ to obtain hollow silicon-carbon composite material.

[0051] Example 5

[0052] (1) 0.2 g of 3-aminopropyltriethoxysilane was added to 40 mL of anhydrous ethanol and dispersed evenly. Then, 4 g of potato starch and 2.4 g of potassium oxalate were added in sequence. After stirring and mixing, the mixture was transferred to a ball mill jar and ball milled at 800 r / min for 3 h with a ball-to-material ratio of 10:1. The mixture was then dried under vacuum at 80 °C for 12 h. After manual grinding, the mixture was passed through a 350 mesh sieve to obtain a solid powder precursor.

[0053] (2) The precursor was carbonized in a nitrogen atmosphere. First, the temperature was raised to 180 °C at a rate of 3 °C / min and held for 2 h. Then, the temperature was raised to 1000 °C at a rate of 5 °C / min and held for 2 h. After that, it was naturally cooled to room temperature. Then, the product was repeatedly washed with hydrochloric acid solution and distilled water to remove impurities and metal elements. Finally, it was dried in a vacuum oven at 80 °C to obtain hollow silicon-carbon composite material.

[0054] Example 6

[0055] (1) 0.8 g of 3-glycidoxypropyltrimethoxysilane was added to 50 mL of anhydrous ethanol and dispersed evenly. Then, 4 g of wheat starch and 2 g of nickel oxalate were added in sequence. After stirring and mixing, the mixture was transferred to a ball mill jar and ball milled at 700 r / min for 4 h using physical mechanical ball milling at a ball-to-material ratio of 10:1. The mixture was then dried under vacuum at 80 °C for 12 h. After manual grinding, the mixture was passed through a 350 mesh sieve to obtain a solid powder precursor.

[0056] (2) The precursor is carbonized in a nitrogen atmosphere. First, the temperature is raised to 200 ℃ at a heating rate of 2 ℃ / min and held for 1 h. Then, the temperature is raised to 900 ℃ at a heating rate of 5 ℃ / min and carbonized for 1 h. After that, it is naturally cooled to room temperature. Then, the product is repeatedly washed with hydrochloric acid solution and distilled water to remove impurities and metal elements. Finally, it is dried in a vacuum oven at 80 ℃ to obtain hollow silicon-carbon composite material.

[0057] Example 7

[0058] (1) 0.8 g of 3-glycidoxypropyltrimethoxysilane was added to 30 mL of anhydrous ethanol and dispersed evenly. Then, 4 g of sweet potato starch and 2.4 g of manganese oxalate were added in sequence. After stirring and mixing, the mixture was transferred to a ball mill jar and ball milled at 400 r / min for 2 h with a ball-to-material ratio of 10:1. The mixture was then dried under vacuum at 80 °C for 12 h. After manual grinding, the mixture was passed through a 350 mesh sieve to obtain a solid powder precursor.

[0059] (2) The precursor was carbonized in a nitrogen atmosphere. First, the temperature was raised to 280 °C at a heating rate of 2 °C / min and held for 2 h. Then, the temperature was raised to 1100 °C at a heating rate of 5 °C / min and carbonized for 4 h. After that, it was naturally cooled to room temperature. Then, the product was repeatedly washed with hydrochloric acid solution and distilled water to remove impurities and metal elements. Finally, it was dried in a vacuum oven at 80 °C to obtain hollow silicon-carbon composite material.

[0060] Comparative Example 1

[0061] Referring to Example 1, but instead of ball milling, manual grinding was performed. The specific preparation process is as follows:

[0062] (1) 0.8 g of nano-silicon powder was added to 30 mL of anhydrous ethanol and dispersed evenly. Then, 4 g of corn starch and 2 g of cobalt oxalate were added in sequence. After stirring and mixing, the mixture was transferred to a mortar and ground by manual grinding. The mixture was then dried under vacuum at 80 °C for 12 h. After being taken out and manually ground, it was passed through a 350-mesh sieve to obtain a solid powder precursor.

[0063] (2) The precursor was carbonized in a nitrogen atmosphere. First, the temperature was raised to 260 °C at a heating rate of 2 °C / min and held for 2 h. Then, the temperature was raised to 800 °C at a heating rate of 5 °C / min and carbonized for 4 h. After that, it was naturally cooled to room temperature. Then, the product was repeatedly washed with hydrochloric acid solution and distilled water to remove impurities and metal elements. Finally, it was dried in a vacuum oven at 80 °C to obtain silicon-carbon composite material.

[0064] Comparative Example 2

[0065] Referring to Example 1, but without adding oxalate, the specific preparation process is as follows:

[0066] (1) 0.8 g of tetraethyl orthosilicate was added to 30 mL of anhydrous ethanol and dispersed evenly. Then, 4 g of corn starch was added directly, stirred and mixed, and transferred to a ball mill jar. Physical mechanical ball milling was used at a ball-to-material ratio of 10:1 at 400 r / min for 4 h to grind and mix evenly. The resulting slurry was then vacuum dried at 80 ℃ for 12 h. After manual grinding, it was passed through a 350-mesh sieve to obtain a solid powder precursor.

[0067] (2) The precursor was carbonized in a nitrogen atmosphere. First, the temperature was raised to 260 °C at a heating rate of 2 °C / min and held for 2 h. Then, the temperature was raised to 800 °C at a heating rate of 5 °C / min and carbonized for 4 h. After that, it was naturally cooled to room temperature. Then, the product was repeatedly washed with hydrochloric acid solution and distilled water to remove impurities and metal elements. Finally, it was dried in a vacuum oven at 80 °C to obtain silicon-carbon composite material.

[0068] Electrochemical testing

[0069] The performance of the hollow silicon-carbon composite materials prepared in Examples 1-7 and Comparative Examples 1-2 for lithium-ion batteries was tested using a half-cell test method, as detailed below:

[0070] The silicon-carbon composite materials prepared in Examples 1-7 and Comparative Examples 1-2 were used as the negative electrode active material. A conductive agent, binder, and solvent were mixed evenly and stirred to form a slurry. The binder used was polyacrylic acid (LA132), the conductive agent was SP (conductive carbon black), and the solvent was N-methylpyrrolidone (NMP). The slurry ratio was 8:1:1 for silicon-carbon composite material, SP, LA132, and NMP, with 250 mL of NMP used. The slurry was then coated onto copper foil and dried in a vacuum oven at 80-100 °C for 12 h to form the negative electrode sheet. The electrolyte was a LiPF6 solution with a concentration of 1 mol / L, wherein the solvent was a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) in a 1:1 volume ratio. A lithium metal sheet was used as the counter electrode, and a polypropylene (PP) membrane was used as the separator. A half-cell was assembled in a glove box. Constant current charge-discharge experiments were conducted using the LAND battery testing system, with the charge-discharge voltage limited to 0.005~2V.

[0071] The Nyquist impedance diagram obtained from the electrochemical testing of the silicon-carbon composite material prepared in Example 1 ( Figure 6 ), Cyclic volt-ampere curve ( Figure 7 ), rate performance ( Figure 8 ) and cycle performance ( Figure 9 This indicates that the material exhibits excellent electrochemical performance in lithium-ion battery anodes. At a current density of 0.5 A / g, the initial discharge specific capacity is 1247 mA h / g.

[0072] The physical and electrochemical properties of the silicon-carbon composite materials prepared in Examples 1-7 and Comparative Examples 1-2 are shown in Table 1.

[0073] Table 1. Physical and electrochemical properties of silicon-carbon composite materials.

[0074] <![CDATA[Specific surface area (m 2 / g)]]> <![CDATA[Degree of graphitization (I D / I G )]]> First reversible capacity (mAh / g) First-time Coulomb efficiency (%) Cyclic capacity retention rate (%) Example 1 117 0.91 1247 92 84 Example 2 115 0.99 1215 90 81 Example 3 114 0.97 1206 91 80 Example 4 106 0.95 1046 90 83 Example 5 110 0.96 1126 88 80 Example 6 108 1.00 1006 84 82 Example 7 91 0.92 1235 89 81 Comparative Example 1 681 1.03 898 69 23 Comparative Example 2 32 1.05 806 82 59

[0075] As shown in Table 1, the materials in Examples 1-7 have a large specific surface area, providing sufficient electrolyte contact interface and abundant ion transport channels to promote rapid lithium ion migration. The high degree of graphitization indicates the synthesis of a good graphitized structure. The uniform and dense carbon coating improves conductivity while avoiding direct contact between silicon and the electrolyte, resulting in good cycle performance. The initial reversible capacity is >1000 mAh / g, the initial coulombic efficiency is >85%, and the capacity retention is >80%. These materials exhibit advantages such as high energy density, high initial efficiency, and high capacity retention. Comparative Example 1 exhibits low initial reversible capacity, initial coulombic efficiency, and cycle capacity retention. This is because simple physical mixing cannot achieve uniform dispersion and a stable interface, preventing starch molecules from breaking down and exposing hydroxyl groups. Consequently, these molecules cannot interact with the silicon source to encapsulate silicon. Furthermore, the excessively large specific surface area leads to intense side reactions between the exposed nano-silicon and the electrolyte, resulting in low initial reversible capacity and initial coulombic efficiency. Comparative Example 2 also shows reduced specific surface area, initial reversible capacity, initial coulombic efficiency, and cycle capacity retention. This is because the absence of oxalate prevents the utilization of the gas generated by thermal decomposition to blow up the carbon precursor and the activation effect of the metal, thus hindering the formation of a porous hollow shell structure in the carbon precursor. Additionally, the lack of metal-catalyzed graphitization results in the formation of the carbon microsphere graphitization structure. Consequently, the electrochemical performance of the silicon-based material component declines, leading to reduced initial reversible capacity, initial coulombic efficiency, and cycle capacity retention.

[0076] The above description is only for better explaining the embodiments of the present invention and is not intended to limit them. Any modifications or equivalent substitutions that do not depart from the spirit and scope of the present invention shall fall within the scope of the present invention.

Claims

1. A hollow silicon-carbon composite material, characterized in that, It uses silicon source as active component and starch as carbon precursor. Through the synergistic effect of mechanical ball milling and oxalate-assisted pyrolysis, the raw materials are uniformly mixed and the interface is pre-activated. A composite material with hollow porous structure and stable silicon-carbon interface is constructed in situ. In the hollow porous structure, nano-silicon particles are encapsulated inside the carbon shell, and a buffer gap is left between them and the inner wall of the carbon shell.

2. The method for preparing the hollow silicon-carbon composite material according to claim 1, characterized in that, Includes the following steps: Step 1: Disperse the silicon source in anhydrous ethanol, then add starch and oxalate, stir and mix, and then perform mechanical ball milling, drying, manual grinding and sieving in sequence to obtain the precursor; Step 2: The precursor is carbonized, and after acid washing, water washing and drying, hollow silicon-carbon composite material is obtained.

3. The method for preparing hollow silicon-carbon composite material according to claim 2, characterized in that, In step 1, the starch is one or more of the following: rice starch, potato starch, corn starch, cassava starch, sweet potato starch, bean starch, and wheat starch.

4. The method for preparing hollow silicon-carbon composite material according to claim 2, characterized in that, In step 1, the silicon source is one or more of nano-silicon, tetraethyl orthosilicate, 3-aminopropyltriethoxysilane, and 3-glycidoxypropyltrimethoxysilane, and its addition amount is 5% to 30% of the total starch mass; the oxalate is one or more of cobalt oxalate, potassium oxalate, ferric oxalate, ammonium oxalate, zinc oxalate, manganese oxalate, and nickel oxalate, and its addition amount is 30% to 60% of the total starch mass.

5. The method for preparing hollow silicon-carbon composite material according to claim 2, characterized in that, The conditions for mechanical ball milling in step 1 are: ball-to-material ratio of 10:1, ball milling speed of 400~800 r / min, and ball milling time of 1~6 h.

6. The method for preparing hollow silicon-carbon composite material according to claim 2, characterized in that, The carbonization conditions in step 2 are as follows: the temperature is increased in stages under a nitrogen atmosphere. The conditions for the staged temperature increase include first increasing the temperature to 180-300 ℃ at a heating rate of 1-5 ℃ / min and holding it at that temperature for 1-4 h; then increasing the temperature to 800-1200 ℃ at a heating rate of 1-5 ℃ / min and holding it at that temperature for 1-6 h.

7. The method for preparing hollow silicon-carbon composite material according to claim 2, characterized in that, The acid used for pickling in step 2 is one or more of hydrochloric acid, sulfuric acid, and nitric acid.

8. The application of the hollow silicon-carbon composite material according to claim 1 as a negative electrode material for lithium-ion batteries.

9. A lithium-ion battery anode material, characterized in that, Includes the hollow silicon-carbon composite material as described in claim 1.

10. A lithium-ion battery, characterized in that, Including the lithium-ion battery anode material as described in claim 9.