A low-melting-point phosphate magnetic sealing glass and its preparation method
By preparing low-melting-point phosphate magnetic sealing glass with a specific composition, a single Fe3O4 crystalline phase is generated, which solves the problems of high toxicity, high softening point and uneven magnetic properties of existing sealing glasses. This achieves low-temperature sealing and good magnetic properties, making it suitable for electromagnetic shielding and magnetic positioning of electronic devices.
Patent Information
- Application Number
- CN202611152788.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-31
- Publication Date
- 2026-11-17
AI Technical Summary
Existing low-melting-point sealing glasses are highly toxic, have high softening points, or have uneven magnetic properties, making it difficult to achieve good flowability and airtightness at low temperatures, and also failing to meet the magnetic response requirements of magnetic sensors and microwave devices.
Low-melting-point phosphate magnetic sealing glass with a specific composition, including P2O5, B2O3, Na2O, Al2O3 and Fe2O3, is used to generate a single Fe3O4 crystalline phase by adjusting chemical stability and crystallization uniformity. The softening point is 460-480℃, and the internal stress is eliminated by annealing.
A single Fe3O4 crystal phase was generated at low temperature, exhibiting good magnetic properties and uniformity, meeting the sealing requirements of electronic devices, and suitable for electromagnetic shielding and magnetic positioning. Moreover, the preparation process is simple and low-cost.
Smart Images

Figure CN123105979A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of magnetic glass materials technology, specifically relating to a low-melting-point phosphate magnetic sealing glass and its preparation method. Background Technology
[0002] As electronic devices evolve towards miniaturization, integration, and low-temperature operation, higher demands are placed on sealing materials. Currently, many devices are connected using adhesive bonding. However, since the adhesive itself is non-magnetic, magnetic performance often weakens at the device joints. Therefore, developing a magnetic glass can effectively compensate for the magnetic loss of the magnetic head. Currently used low-melting-point sealing glass solders are mainly lead-based, vanadium-based, and phosphate-based low-melting-point glasses. However, lead-based and vanadium-based low-melting-point glasses are toxic and pose a significant health risk.
[0003] Sealing glasses need to achieve good fluidity and airtightness at relatively low temperatures (typically below 500°C) without damaging internal sensitive components. Furthermore, in certain specialized applications such as magnetic sensors, microwave devices, and electromagnetic shielding packaging, sealing glasses are also required to possess specific magnetic response characteristics. Existing magnetic sealing glasses are mainly divided into ferrite systems and metal powder composite systems. Ferrite glasses (such as barium ferrite and strontium ferrite) generally have high softening points (>600°C), making them difficult to use for low-temperature sealing. While composite materials of metal powders (such as Fe, Ni, and Co) and glass can lower the softening point, they easily introduce polycrystalline phases, resulting in magnetic inhomogeneity, and the metal particles are prone to oxidation during glass melting, leading to performance degradation. Phosphate glasses, due to their low glass transition temperature and good chemical stability, have become candidate systems for low-melting-point sealing glasses. However, existing phosphate magnetic glasses often precipitate multiple crystalline phases such as Fe2O3 and FePO4, resulting in large fluctuations in the softening point and poor controllability of magnetic properties. Therefore, developing a phosphate magnetic sealing glass that can precipitate a single Fe3O4 crystal phase at low temperatures and has a stable softening point between 460-480℃ has significant industrial application value. Summary of the Invention
[0004] The purpose of this invention is to overcome the shortcomings of the prior art and provide a low-melting-point phosphate magnetic sealing glass and its preparation method.
[0005] The objective of this invention can be achieved through the following technical solutions: A low-melting-point phosphate magnetic sealing glass, the composition of which is as follows by weight percentage: P2O5: 30-40%; B2O3: 10-20%; Na2O: 5-10%; Al2O3: 3-8%; CeO2: 0-1%; Fe2O3: 20-40%.
[0006] Preferably, the Fe2O3 content is 20-35 wt%. This is achieved by adjusting the chemical stability and crystallization uniformity of the glass. After melting, the sealing glass undergoes annealing to produce a single Fe3O4 (magnetite) crystal phase, without the appearance of Fe2O3, FePO4, or other iron-containing crystal phases. Its softening point ranges from 460-480℃.
[0007] The low-melting-point phosphate magnetic glass prepared by this invention uniformly precipitates a large number of spherical spinel crystal phases with a grain size of 200-600 nm, a saturation magnetization of 4.5-22.5 emu / g, and a coercivity greater than 500 Oe.
[0008] This invention also provides a method for preparing the above-mentioned low-melting-point phosphate magnetic sealing glass, comprising the following steps: (1) Weigh each raw material according to the weight percentages mentioned above: ammonium dihydrogen phosphate, boric acid, sodium carbonate, Al2O3, CeO2 and Fe2O3; among them, raw materials containing water of crystallization need to be converted into oxides for measurement in advance; (2) Place the weighed raw materials in a ball mill jar and mix them evenly to obtain the batch material; (3) Load the batch material into a corundum or platinum-rhodium crucible, place it in a high-temperature electric furnace, heat it to 1200-1400℃ at a rate of 3-5℃ / min, and hold it at the temperature for 1-4 hours to melt it; (4) Quickly pour the uniformly molten glass onto a preheated steel plate or into water for water quenching to obtain glass blocks; (5) Place the glass fragments in an annealing furnace and anneal at 400°C for 1-3 hours to eliminate internal stress. Then cool the glass fragments to room temperature in the furnace to obtain the low melting point phosphate magnetic sealing glass.
[0009] Further, in step (2), the raw materials, ethanol solvent and zirconium oxide balls are mixed in a mass ratio of 1:2:1 and ground for 1-3 hours.
[0010] Furthermore, the preferred melting temperature in step (3) is 1300-1400℃.
[0011] Furthermore, in step (5), the cooling rate after annealing is controlled at 1-2℃ / min to prevent the glass from cracking.
[0012] The beneficial effects of this invention are: (1) The present invention provides a low melting point phosphate magnetic glass with a softening point (460-480℃): by optimizing the P2O5-B2O3-Na2O-Al2O3 network structure and introducing an appropriate amount of Fe2O3, the viscosity and softening temperature of the glass are significantly reduced, meeting the requirements of low temperature sealing.
[0013] (2) Generating a single Fe3O4 crystal phase through thermal regime: By utilizing the coordination regulation effect of the phosphate system on iron ions, combined with the clarification and valence stabilization function of CeO2, Fe2O3 is selectively transformed into Fe3O4 during melting and crystallization, avoiding the generation of other impurity phases and ensuring the consistency and stability of magnetic properties.
[0014] (3) The glass prepared by this invention has good magnetic properties: Fe3O4, as a ferromagnetic material, endows the glass with good magnetic permeability and saturation magnetization, making it suitable for electromagnetic shielding, magnetic positioning and sealing, and other applications. The preparation process is simple: no special atmosphere protection is required, and melting can be completed in an air atmosphere. Moreover, the raw materials are widely available, and the cost is lower than that of traditional cobalt-based or nickel-based magnetic glasses. Attached Figure Description
[0015] The present invention will now be further described with reference to the accompanying drawings.
[0016] Figure 1 XRD patterns of the phosphate magnetic glasses prepared in Examples 1-5; Figure 2 CTE images of the phosphate magnetic glasses prepared in Examples 1-5; Figure 3 SEM images of the phosphate magnetic glasses prepared in Examples 1-5; Figure 4 The XRD pattern of the glass prepared in Comparative Example 1; Figure 5 The image shows the CTE pattern of the borosilicate magnetic glass prepared in Comparative Example 2. Detailed Implementation
[0017] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0018] Example 1
[0019] Based on the mass percentages of 30g P2O5, 20g B2O3, 6g Na2O, 3g Al2O3, 1g CeO2, and 20g Fe2O3, calculate and weigh the actual amount of each raw material. After accurate weighing, load the raw materials into a mixing tank at a mass ratio of total raw materials: grinding media: anhydrous ethanol = 1:2:1 and ball mill for 1 hour to ensure uniform mixing. Then, dry the mixture at 90°C for 3 hours to obtain a uniform mixed raw material. The mixed raw materials were placed in a crucible for melting. The temperature was first increased to 1100℃ at 5℃ / min, then increased to the melting temperature at 2℃ / min and held for 1 hour to melt the raw materials into a homogeneous glass melt. The homogeneous molten glass was poured into a preheated copper mold and cooled to form the desired shape. It was then annealed at 400°C for 1 hour to obtain a ferromagnetic glass-ceramic. This glass is denoted as P1.
[0020] Example 2
[0021] Based on the mass percentages of 35g P2O5, 10g B2O3, 8g Na2O, 1g Al2O3, 1g CeO2, and 25g Fe2O3, calculate and weigh the actual amount of each raw material. After accurate weighing, load the raw materials into a mixing tank at a mass ratio of total raw materials: grinding media: anhydrous ethanol = 1:2:1 and ball mill for 2 hours to ensure uniform mixing. Then, dry the mixture at 80℃ for 3 hours to obtain a uniform mixed raw material. The mixed raw materials were placed in a crucible for melting. The temperature was first increased to 1100℃ at 5℃ / min, then increased to the melting temperature at 2℃ / min and held for 2.5h to melt the raw materials into a homogeneous glass melt. The homogeneous molten glass was poured into a preheated copper mold and cooled to form the desired shape. It was then annealed at 400°C for 1.5 hours to obtain a ferromagnetic glass-ceramic. This glass is denoted as P2.
[0022] Example 3
[0023] Based on the mass percentages of 30g P2O5, 10g B2O3, 5g Na2O, 4g Al2O3, 1g CeO2, and 30g Fe2O3, calculate and weigh the actual amount of each raw material. After accurate weighing, load the raw materials into a mixing tank at a mass ratio of total raw materials: grinding media: anhydrous ethanol = 1:2:1 and ball mill for 1.5 hours to ensure uniform mixing. Then dry the mixture at 60°C for 2.5 hours to obtain a uniform mixed raw material. The mixed raw materials were placed in a crucible for melting. The temperature was first increased to 1100℃ at 5℃ / min, then increased to the melting temperature at 2℃ / min and held for 2 hours to melt the raw materials into a homogeneous glass melt. The homogeneous molten glass was poured into a preheated copper mold and cooled to form the desired shape. It was then annealed at 400°C for 1.3 hours to obtain a ferromagnetic glass-ceramic. This glass is designated P3.
[0024] Example 4
[0025] Based on the mass percentages of 30g P2O5, 10g B2O3, 6g Na2O, 3g Al2O3, 1g CeO2, and 30g Fe2O3, calculate and weigh the actual amount of each raw material. After accurate weighing, load the raw materials into a mixing tank at a mass ratio of total raw materials: grinding media: anhydrous ethanol = 1:2:1 and ball mill for 3 hours to ensure uniform mixing. Then, dry the mixture at 70℃ for 4 hours to obtain a uniform mixed raw material. The mixed raw materials were placed in a crucible for melting. The temperature was first increased to 1100℃ at 5℃ / min, then increased to the melting temperature at 2℃ / min and held for 2 hours to melt the raw materials into a homogeneous glass melt. The homogeneous molten glass was poured into a preheated copper mold and cooled to form the desired shape. It was then annealed at 400°C for 2 hours to obtain a ferromagnetic glass-ceramic. This glass is designated P4.
[0026] Example 5
[0027] Based on the mass percentages of 30g P2O5, 10g B2O3, 5g Na2O, 4g Al2O3, 1g CeO2, and 30g Fe2O3, calculate and weigh the actual amount of each raw material. After accurate weighing, load the raw materials into a mixing tank at a mass ratio of total raw materials: grinding media: anhydrous ethanol = 1:2:1 and ball mill for 3 hours to ensure uniform mixing. Then, dry the mixture at 90℃ for 3 hours to obtain a uniform mixed raw material. The mixed raw materials were placed in a crucible for melting. The temperature was first increased to 1100℃ at 5℃ / min, then increased to the melting temperature at 2℃ / min and held for 1 hour to melt the raw materials into a homogeneous glass melt. The homogeneous molten glass was poured into a preheated copper mold and cooled to form the desired shape. It was then annealed at 400°C for 1 hour to obtain a ferromagnetic glass-ceramic. This glass is designated P5.
[0028] Comparative Example 1 Comparative Example 1 is a phosphate glass component that does not contain Fe2O3. The glass formulation consists of 30g P2O5, 10g B2O3, 5g Na2O, 4g Al2O3, and 1g CeO2 by mass percentage. The actual amount of each raw material was calculated and weighed. After accurate weighing, the raw materials were ball-milled in a mixing jar at a mass ratio of total raw materials: grinding media: anhydrous ethanol = 1:2:1 for 3 hours to ensure uniform mixing. The mixture was then dried at 90°C for 3 hours to obtain a homogeneous mixture. The mixed raw materials were placed in a crucible for melting. The temperature was first increased to 1100℃ at a rate of 5℃ / min, then increased to the melting temperature at a rate of 2℃ / min and held for 1 hour to melt the raw materials into a homogeneous glass liquid. The homogeneous glass liquid was poured into a preheated copper mold to cool and solidify, and then annealed at 400℃ for 1 hour to obtain an amorphous glass, denoted as P6. Its XRD (e.g., ...) is shown in the image. Figure 4As shown, the glass is amorphous and does not contain Fe3O4 crystals, thus lacking magnetic properties. This does not meet the requirements of this invention.
[0029] Comparative Example 2 This is a borosilicate glass system, free of P2O5. The specific composition is: 30g SiO2, 10g B2O3, 5g Na2O, 4g Al2O3, 1g CeO2, and 20g Fe2O3. Calculate and weigh the actual amount of each raw material. After accurate weighing, load the raw materials into a mixing jar at a mass ratio of total raw materials: grinding media: anhydrous ethanol = 1:2:1 and ball mill for 3 hours to ensure uniform mixing. Then dry at 90℃ for 3 hours to obtain a homogeneous mixture. Place the mixture in a crucible for melting, first increasing the temperature to 1100℃ at 5℃ / min, then increasing it to the melting temperature at 2℃ / min and holding for 1 hour to melt the raw material into a homogeneous glass melt. The homogeneous molten glass was poured into a preheated copper mold and cooled to form the desired shape. It was then annealed at 500℃ for 1 hour to obtain a magnetic microcrystalline glass containing Fe3O4 crystals, denoted as S1. However, CTE testing showed its softening point to be 620℃ (e.g., Figure 5 As shown in the figure, the softening point of the magnetic glass obtained from P1-P5 is much higher.
[0030] Combining XRD, CTE and SEM (e.g.) Figures 1-3 As shown in the analysis results, the glasses in all embodiments of the present invention precipitate a single Fe3O4 crystal phase. No Fe2O3 or FePO4 impurity phase peaks were observed in the XRD patterns, indicating stable and controllable magnetic modulation. The inflection point of the CTE thermal expansion curve confirms that the softening point of each embodiment is stable in the 460-480℃ range, indicating that the magnetic glass of the present invention has a low melting point, suitable for sealing electronic components. SEM images show a large number of uniformly dispersed spherical Fe3O4 nanocrystals in the glass matrix, with grain sizes concentrated in the 200-600nm range. Furthermore, as the Fe2O3 content increases from 20wt% to 40wt%, the grain number density increases regularly without significant coarsening, confirming the intrinsic structural basis for the increase in saturation magnetization (4.5-22.5 emu / g) with increasing Fe2O3 content. In summary, these three factors fully demonstrate that the glass of this invention possesses a single crystal phase, uniform microstructure, and adjustable magnetic properties at low-temperature sealing temperatures, providing a solid theoretical and performance foundation for low-temperature magnetic sealing applications.
[0031] Table 1. Saturation magnetization and coercivity of phosphate glasses prepared in Examples 1-5
[0032] The above detailed embodiments provide a specific description of the analytical methods involved in this invention. It should be noted that the above description is only intended to help those skilled in the art better understand the methods and ideas of this invention, and is not intended to limit the scope of the invention. Without departing from the principles of this invention, those skilled in the art can make appropriate adjustments or modifications to this invention, and such adjustments and modifications should also fall within the protection scope of this invention.
Claims
1. A low-melting-point phosphate magnetic sealing glass, characterized in that, Its components, by weight percentage, are as follows: P2O5: 30-40%; B2O3: 10-20%; Na2O: 5-10%; Al2O3: 3-8%; CeO2: 0-1%; Fe2O3: 20-40%.
2. The low-melting-point phosphate magnetic sealing glass according to claim 1, characterized in that, The Fe2O3 content is 20-35 wt%.
3. The low-melting-point phosphate magnetic sealing glass according to claim 1, characterized in that, The softening point of the phosphate magnetic sealing glass is in the range of 460-480℃.
4. The low-melting-point phosphate magnetic sealing glass according to claim 1, characterized in that, The magnetic crystals in the phosphate magnetic sealing glass have a particle size of 200-600 nm and are uniformly dispersed.
5. The low-melting-point phosphate magnetic sealing glass according to claim 1, characterized in that, The saturation magnetization of the phosphate magnetic sealing glass is 4.5-22.5 emu / g, and the coercivity is greater than 500 Oe.
6. The method for preparing low-melting-point phosphate magnetic sealing glass according to any one of claims 1-5, characterized in that, Includes the following steps: (1) Weigh the raw materials containing each component according to the stated weight percentage; (2) Place the weighed raw materials in a ball mill jar and mix them evenly to obtain the batch material; (3) The batch material is loaded into a crucible and melted; (4) The molten glass is poured or water-quenched to form a glass block; (5) The glass block is annealed at 400°C for 1-3 hours and then cooled to obtain the low melting point phosphate magnetic sealing glass.
7. The preparation method according to claim 6, characterized in that, The raw material containing P2O5 is ammonium dihydrogen phosphate, the raw material containing B2O3 is boric acid, and the raw material containing Na2O is sodium carbonate.
8. The preparation method according to claim 6, characterized in that, In step (2), ethanol solvent is added for grinding, and the mass ratio of raw material, ethanol solvent and zirconium oxide balls is 1:2:1, and the grinding time is 1-3h.
9. The preparation method according to claim 6, characterized in that, In step (3), the temperature is increased to 1200-1400℃ at a rate of 3-5℃ / min, and the temperature is maintained for melting for 1-4 hours.
10. The preparation method according to claim 6, characterized in that, In step (5), the cooling rate is controlled at 1-2℃ / min.