A high color rendering white light phosphor-glass composite material excited by violet light and its preparation method
By introducing stannous oxide and a specific type of phosphor into a low-melting-point phosphate matrix glass, combined with a low-temperature stirring process, the problem of oxidation and decomposition of phosphor-glass composite materials at high temperatures was solved, achieving high color rendering and efficient white light emission under violet light excitation, which is suitable for high-power laser driving.
Patent Information
- Application Number
- CN202611579424.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-13
- Publication Date
- 2026-11-17
AI Technical Summary
Existing phosphor-glass composite materials are prone to oxidation and decomposition during high-temperature sintering, resulting in a decrease in luminescence efficiency. Furthermore, there is a lack of high color rendering phosphor-glass composite materials suitable for violet light excitation, making it difficult to meet the application requirements of high stability and long lifespan.
A phosphor-glass composite material was prepared by combining low-melting-point phosphate matrix glass with white phosphor. By introducing tin oxide into the glass to form a mixed valence intermediate energy level trap state, free electrons generated by photoionization were captured. Combined with specific phosphor types and ratios, a low-temperature stirring process was used to prepare the phosphor-glass composite material.
It achieves white light emission with high color rendering index and high internal quantum efficiency under violet light excitation, improves the laser saturation threshold and thermal stability of the material, and adapts to high-power laser driving.
Smart Images

Figure CN123105983A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of laser lighting technology, specifically relating to a high color rendering white phosphor-glass composite material excited by violet light and its preparation method. Background Technology
[0002] With the rapid development of solid-state lighting and laser display technologies towards higher brightness, wider color gamut, higher color rendering index, and eye-friendly features, white light conversion systems based on violet light excitation have attracted much attention in the high-end lighting and display fields due to their advantages such as continuous spectrum, ability to reduce the high-intensity blue light component caused by direct blue light pumping, and easy improvement of color rendering index. Photon conversion materials, as core optical functional components, directly determine the brightness, color gamut, stability, and lifespan of devices.
[0003] Traditional optoelectronic devices often use organic polymers to encapsulate phosphors to fabricate photon converters. This process is simple and versatile, but organic substrates suffer from problems such as easy aging at high temperatures, irreversible degradation under strong ultraviolet / blue light irradiation, and low thermal conductivity. Under high-power laser driving conditions, the thermal accumulation effect is significant, leading to a sharp decline in phosphor quantum efficiency and structural failure, which cannot meet the requirements for high stability and long lifespan applications.
[0004] Phosphor-glass composites, using inorganic glass as a matrix, possess excellent thermal stability, chemical stability, and radiation resistance. With a wide range of material choices and relatively economical preparation, they are considered an ideal alternative to organic encapsulation. However, existing phosphor-glass composites still face key bottlenecks: conventional high-temperature sintering (typically above 1000 °C) easily causes oxidation, decomposition, or interfacial reactions of the phosphor, leading to decreased luminous efficiency and deteriorated color rendering performance. In particular, they exhibit poor compatibility with sensitive high-color-rendering phosphors such as nitrides. Furthermore, most systems are only compatible with blue light excitation; specialized, high-color-rendering, and highly stable phosphor-glass composites for violet light excitation are still lacking, hindering the industrial application of high-quality violet-excited white light devices.
[0005] Existing technologies already have a basis There are reports of ultra-low melting point glass composites with phosphors (such as CN120923144A), but their glass components do not contain phosphors. The phosphor loading is low (0.5-4 wt%), mainly used for narrowband emission and laser display color gamut expansion. This technology prioritizes narrowband color gamut rather than wideband high color rendering white light. This system fails to address the efficiency decrease caused by phosphor reabsorption under high loading conditions, and it does not optimize the glass composition or match the phosphor system for violet excitation. Furthermore, existing technologies also employ borosilicate glass through a lamination softening method to prepare luminescent glass (e.g., EP2481572A1), but its preparation mechanism is completely different from the melt-stirring method of this application, and it does not involve high color rendering white light emission under violet excitation.
[0006] Therefore, developing a novel phosphor-glass composite material that can be efficiently excited by violet light, has a high color rendering index, and excellent thermal stability is of great practical significance. Summary of the Invention
[0007] This invention addresses the problems of high color rendering index (CRI) white light bulk materials in existing laser lighting technologies, such as high difficulty in preparation, low quantum efficiency, and difficulty in being excited by violet light (common blue light excitation poses blue light hazards). It proposes a violet-excited high CRI white light phosphor-glass composite material and its preparation method.
[0008] To achieve the above objectives, the present invention adopts the following technical solution: A high-color-rendering phosphor-glass composite material excited by violet light, comprising a white phosphor and a low-melting-point phosphate matrix glass; wherein the white phosphor is uniformly dispersed in the low-melting-point phosphate matrix glass; and wherein the low-melting-point phosphate matrix glass comprises at least the following components, in molar percentage: Tin fluoride: 40~55 mol% Tin oxide: 5~10 mol%. Sodium fluoride: 5~15 mol% Phosphorus pentoxide: 30~40 mol% The white phosphor accounts for 5-15 wt% of the mass percentage in the phosphor-glass composite material; The phosphor-glass composite material emits white light when excited by a 405nm violet laser.
[0009] Furthermore, the white phosphor comprises a variety selected from... , , , , At least two of them.
[0010] Furthermore, the white phosphor contains .
[0011] Furthermore, the white phosphor contains , , , , Five types of fluorescent powder.
[0012] Furthermore, the mass ratio of the five phosphors is as follows: .
[0013] Furthermore, the composition of the low-melting-point phosphate matrix glass is: 48 mol% stannous fluoride, 7 mol% stannous oxide, 10 mol% sodium fluoride, and 35 mol% phosphorus pentoxide.
[0014] This invention also provides a method for preparing a phosphor-glass composite material, characterized by comprising the following steps: (1) Provide a low melting point phosphate matrix glass raw material, wherein the low melting point phosphate matrix glass raw material contains at least stannous fluoride, stannous oxide, sodium fluoride and phosphate precursor, and the components are mixed in molar percentage, ground and then heated and melted at 35~550℃ for 10~30 minutes to obtain glass melt; (2) Add the prepared white phosphor to the glass melt and stir at a speed of 1-5 rpm for 3-15 seconds to make the phosphor evenly dispersed; (3) The mixed melt is quickly poured into a preheated mold and cooled in air to obtain the phosphor-glass composite material.
[0015] Further, the mixing in step (1) includes grinding each component together with anhydrous ethanol into a slurry, followed by thorough drying.
[0016] Furthermore, the heating and melting temperature in step (1) is 400~550℃ and the time is 10~20 minutes.
[0017] Furthermore, the stirring speed in step (2) is 3~5 rpm and the stirring time is 3~10 seconds.
[0018] Compared with the prior art, the present invention has the following advantages and beneficial effects: This invention is in Introduce 5~10 mol% into the system , Under 405nm violet light (3.06eV) irradiation, photoionization is likely to occur. If the free electrons generated are not captured, they will combine with glass defects to form color centers, leading to photo-blackening and thermal quenching. After introduction, Mixed valence states form intermediate energy level trap states in the glass band gap, which can quickly capture free electrons generated by photoionization, blocking the formation path of color centers, thereby lowering the laser saturation threshold from a state without valence. The power output was increased from 0.5W to 1.5W, making the material compatible with high-power violet laser drive.
[0019] Furthermore, the present invention employs , , , , Five phosphors were blended in a mass ratio of 6:5:4:2:1. The emission peaks of each phosphor (~450nm, ~515nm, ~530nm, ~570nm, ~650nm) formed a relatively continuous coverage in the visible spectrum, which helps to obtain broadband white light emission while taking into account both color rendering performance and internal quantum efficiency. Attached Figure Description
[0020] Figure 1 The excitation and emission spectra of the white phosphor prepared in Example 1 and the phosphor-glass composite material in Example 4 are shown. Figure 2 shows the quantum efficiency of the phosphor-glass composite material prepared in Example 4; Figure 3 is a schematic diagram of the 405nm laser test in Examples 3 to 5; Figure 4 shows the emission spectrum of the phosphor-glass composite material prepared in Example 2 under 405nm laser excitation; Figure 5 shows the emission spectrum of the phosphor-glass composite material prepared in Example 5 under 405nm laser excitation; Figure 6 shows the emission spectrum of the phosphor-glass composite material prepared in Example 4 under 405nm laser excitation; Figure 7 is a schematic diagram of the lumen output and lumen efficiency of the phosphor-glass composite materials prepared in Examples 3-5 under 405nm laser excitation. Detailed Implementation
[0021] To better understand the present invention, the following embodiments are provided for further explanation, but the scope of protection of the present invention is not limited thereto.
[0022] First, this invention provides a phosphor-glass composite material. This composite material uses a stannous fluoride-stannous oxide-sodium fluoride-phosphorus pentoxide system as a low-melting-point phosphate matrix glass. Stannous fluoride, sodium fluoride, and phosphorus pentoxide together form the glass network framework, lowering the glass melting temperature to 350°C to 550°C and preventing thermal degradation of the phosphor during the composite process. Stannous oxide is then introduced at an addition amount of 5 mol% to 10 mol%. The mechanism of action of stannous oxide is as follows: Under continuous irradiation with 405 nm ultraviolet light, divalent tin ions in the glass are prone to photoionization, generating free electrons. These free electrons combine with glass defects to form color centers, leading to photoblackening and attenuation of luminous intensity. After the introduction of stannous oxide, divalent and tetravalent tin ions form a mixed valence system, generating intermediate energy level trap states in the glass band gap. These trap states can quickly capture the free electrons generated by photoionization, blocking the color center formation path and thus significantly improving the laser saturation threshold of the material. Simultaneously, the phosphor loading in this composite material is limited to 5% to 15% by weight. Below this range, the phosphor concentration is insufficient to completely absorb the 405nm excitation light, resulting in a large amount of violet light transmission and a low color rendering index; above this range, the phosphor particle spacing is too small, leading to increased reabsorption between different phosphors and a decrease in internal quantum efficiency. This loading range achieves the optimal balance between complete absorption and efficient conversion of the excitation light.
[0023] Furthermore, the white phosphor in this composite material is selected from at least two of the aluminate, silicate, and nitride phosphor systems. A single phosphor is insufficient to provide broadband emission; white light can only be formed through the complementarity of at least two phosphors, either blue and yellow or blue and red. This provides a material basis for further improving the color rendering index and covering a wider spectral band.
[0024] Furthermore, the white phosphor in this composite material includes a calcium-based nitride red phosphor. This phosphor is currently the only red phosphor that can be efficiently excited under 405nm violet light and possesses excellent thermal stability. Its emission peak is located in the deep red region at 650nm, making it irreplaceable for improving the color rendering index. The use of calcium-based nitride red phosphor ensures sufficient deep red components in the white light spectrum, maintaining a high level of saturated red light value in the color rendering index.
[0025] Furthermore, the white phosphor in this composite material is a mixture of five phosphors. The emission peaks of the five phosphors are located at 450 nm, 515 nm, 530 nm, 570 nm and 650 nm, respectively, forming an equally spaced continuous coverage in the visible spectrum range of 400 to 700 nm without significant spectral gaps, thus achieving spectral continuity and integrity.
[0026] Furthermore, the five phosphors in this composite material are compounded in a mass ratio of 6:5:4:2:1. This ratio ensures that the emission spectra of each phosphor form a continuous coverage in the visible light range, while minimizing the spectral overlap integral between the excitation spectrum of each phosphor and the emission spectrum of adjacent phosphors. This physically suppresses reabsorption between different phosphors, enabling the composite material to achieve broadband white light emission while maintaining high internal quantum efficiency.
[0027] Furthermore, the low-melting-point phosphate matrix glass in this composite material is composed of 4 mol% stannous fluoride, 7 mol% stannous oxide, 10 mol% sodium fluoride, and 35 mol% phosphorus pentoxide. At this ratio, the viscosity and surface tension of the glass melt are optimal for the uniform dispersion of the phosphor, and the glass transition temperature matches the phosphor's coefficient of thermal expansion to the highest degree. The composite material also exhibits the lowest interfacial stress and the highest light transmittance.
[0028] Furthermore, this invention provides a method for preparing a phosphor-glass composite material. The method first involves heating and melting the glass raw material at 350°C to 550°C for 10 to 30 minutes to form a homogeneous glass melt. Then, the phosphor is added, and the mixture is stirred at a speed of 1 to 5 rpm for 3 to 15 seconds to ensure uniform dispersion. Finally, the mixture is poured and cooled to form the final shape. This process sequence avoids the high-temperature process and acidic atmosphere that would otherwise require the phosphor to undergo raw material decomposition. The phosphor is added only after the glass melt has formed, and its exposure time in the high-temperature melt is only 3 to 15 seconds. This controls the interfacial reaction at the nanoscale, allowing the phosphor's crystalline structure to be fully preserved. Simultaneously, the use of a low-melting-point phosphate glass matrix results in a melting temperature far lower than that of traditional high-temperature sintering processes, suppressing the interfacial reaction between the phosphor and the glass matrix from both thermodynamic and kinetic perspectives.
[0029] Furthermore, in this method, the components of the glass raw material are co-ground with anhydrous ethanol to a slurry state, and then thoroughly dried. Ethanol grinding allows the raw materials to be uniformly mixed at the microscale. After drying, the uniformity of the distribution of each component directly affects the uniformity of the glass melt, and thus affects the uniformity of phosphor dispersion.
[0030] Furthermore, the heating and melting temperature is further controlled to 400°C to 550°C and the time to 10 to 20 minutes. This preferred range ensures that the glass raw material is completely melted while minimizing the exposure time of the phosphor at high temperatures, making it suitable for phosphor systems that are more sensitive to temperature.
[0031] Furthermore, in this method, the stirring speed is further controlled to 3 to 5 rpm and the stirring time to 3 to 10 seconds. This preferred range further shortens the exposure time of the phosphor in the high-temperature melt while ensuring uniform dispersion of the phosphor, thereby further reducing the thermal erosion of the phosphor.
[0032] In summary, this invention achieves a breakthrough in violet light irradiation stability by introducing stannous oxide into the glass composition; it achieves a synergistic effect of high color rendering and high quantum efficiency through the selection of specific phosphor types, compounding ratios, and loading control; and it ensures the complete preservation of the phosphor's luminescent properties through a pre-melting and post-addition process with low-temperature rapid stirring. These technical features work synergistically and progressively, collectively achieving white light emission with high color rendering index and high internal quantum efficiency under violet light excitation.
[0033] Test Method Description The phosphor-glass composite materials prepared in the following examples and comparative examples were all tested using the following methods and equipment.
[0034] Color rendering index (CRI) and color temperature (CCT) were measured using a high-precision, rapid spectroradiometer equipped with a 300mm integrating sphere. The sample was placed in the optical path of a 405nm semiconductor laser with a power of 1.5W and a spot diameter of 3mm. The integrating sphere collected the emitted light, and the spectroradiometer recorded the spectral power distribution from 380nm to 780nm. The CRI Ra and CCT were calculated using a standard illuminant, D65, as the reference light source.
[0035] The internal quantum efficiency was measured using an absolute quantum efficiency testing system with an integrating sphere. A 405nm laser was used as the excitation source. .
[0036] Luminous flux and lumen efficiency were measured using a spectroradiometer with an integrating sphere. The sample was excited by a 1.5W laser, and the absolute luminous flux was calculated. .
[0037] The laser saturation threshold test used a 405nm semiconductor laser with a maximum output power of 5W, along with a power meter and a spectroradiometer. Starting from 0.5W, the laser power was gradually increased, and the critical power value at which the luminous intensity decreased sharply was recorded.
[0038] Example 1 Will , , , , The five phosphors were accurately weighed according to a mass ratio of 6:5:4:2:1, and the masses of the five phosphors were as follows: , , , , Total The weighed phosphor was placed in an agate mortar, 20 mL of anhydrous ethanol was added, and the mixture was ground for 30 minutes until it was fully mixed and formed a slurry. The slurry was then dried in a 60 °C oven for 12 hours. After drying, it was ground again for 10 minutes and then vacuum-sealed for later use. The excitation and emission spectra of the white phosphor prepared in Example 1 are as follows: Figure 1 As shown.
[0039] Example 2 The target composition of the matrix glass is 40 mol%. 5 mol% 15 mol% 40 mol% Weigh , , , ,total Weigh accurately to three decimal places.
[0040] Place the weighed raw materials in an agate mortar, add 8 mL of anhydrous ethanol, and grind for 30 minutes until a slurry forms. Transfer the slurry to a glass petri dish and dry in a 60°C oven for 12 hours. Grind the dried mixture into a fine powder, transfer it all to a corundum crucible, and place it in a muffle furnace heated to 350°C. Hold the furnace at this temperature for 15 minutes to allow the raw materials to fully decompose and melt. Remove the crucible and observe that the glass melt is transparent and homogeneous.
[0041] Quickly weigh the white phosphor prepared in Example 1 The molten glass was added to the surface of the crucible in one go. The mixture was stirred for 3 seconds at 3 rpm using a 3mm diameter corundum stirring rod. The phosphor was observed to be incorporated into the melt and uniformly dispersed to the naked eye. The molten mixture was then quickly poured into a preheated brass mold (20mm diameter, 5mm deep cylindrical groove) at 200℃. After natural cooling to room temperature in air, the sample was demolded to obtain a circular sample approximately 18mm in diameter and 3mm thick. The sample was then successively polished with 400, 800, and 1500 grit silicon carbide sandpaper until the surface was smooth, and then polished to a mirror finish with cerium oxide polishing solution. The final sample dimensions were 18mm in diameter and 2.5mm thick. The test results are shown in Table 1.
[0042] Example 3 The target composition of the matrix glass is 48 mol%. 7 mol% 10 mol% 35 mol% Weigh , , , ,total .
[0043] The grinding and drying steps are the same as in Example 2. The dried mixed raw materials are ground into a fine powder, and all of it is transferred to a corundum crucible. The crucible is then placed in a muffle furnace heated to 480°C and held for 20 minutes. The crucible is then removed, and the glass melt is observed to be transparent and uniform.
[0044] Quickly weigh the white phosphor prepared in Example 1 Add the mixture to the crucible all at once. Stir with a 3mm diameter corundum stirring rod at 3 rpm for 9 seconds. Quickly pour into a brass mold preheated to 200℃, cool, demold, cut, grind, and polish, following the same steps as in Example 2. Test results are shown in Table 1.
[0045] Example 4 The target composition of the matrix glass is 55 mol%. 10 mol% 5 mol% 30 mol% Weigh , , , ,total .
[0046] The grinding and drying steps are the same as in Example 2. The dried mixed raw materials are ground into a fine powder, and all of it is transferred to a corundum crucible, which is then placed in a muffle furnace heated to 550°C and held for 30 minutes. The crucible is then removed, and the glass melt is observed to be transparent and uniform.
[0047] Quickly weigh the white phosphor prepared in Example 1 Add the mixture to the crucible all at once. Stir with a 3mm diameter corundum stirring rod at 5 rpm for 15 seconds. Quickly pour into a brass mold preheated to 200℃, cool, demold, cut, grind, and polish, following the same steps as in Example 2. Test results are shown in Table 1.
[0048] Example 5 The target composition of the matrix glass is 48 mol%. 7 mol% 10 mol% 35 mol% The amount of raw materials used is the same as in Example 3, that is... , , , ,total The grinding and drying steps are the same as in Example 2.
[0049] The dried mixed raw materials were ground into a fine powder and transferred entirely into a corundum crucible. The crucible was then placed in a muffle furnace heated to 550°C and held for 10 minutes. The crucible was removed, and the glass melt was observed to be transparent and homogeneous.
[0050] Quickly weigh the white phosphor prepared in Example 1 Add the powder to the crucible all at once. Stir with a 3mm diameter corundum stirring rod at 5 rpm for 15 seconds. Quickly pour into a brass mold preheated to 200℃, cool, demold, cut, grind, and polish, following the same steps as in Example 2. A photograph of the phosphor-glass composite material sample prepared in Example 5 is shown, and its emission spectrum under 405nm violet laser excitation is as follows. Figure 5 As shown, the internal quantum efficiency test results are as follows: Figure 2 As shown in Table 1, the test results are as follows.
[0051] Example 6 Remix the phosphor according to the same mass ratio: , , , , each ,total The mixture was placed in an agate mortar, 20 mL of anhydrous ethanol was added, and it was ground for 30 minutes to mix thoroughly. The mixture was then dried at 60°C for 12 hours. The glass composition, preparation conditions, and total phosphor loading were the same as in Example 5. The test results are shown in Table 1.
[0052] Example 7 By mass ratio The phosphors were remixed, and the masses of the five phosphors were respectively... , , , , ,total The grinding and mixing method was the same as in Example 1. The glass composition, preparation conditions, and total phosphor loading were the same as in Example 5. The test results are shown in Table 1.
[0053] Example 8 By mass ratio The phosphors were remixed, and the masses of the two phosphors were respectively... and ,total The grinding and mixing method was the same as in Example 1. The glass composition, preparation conditions, and total phosphor loading were the same as in Example 5. The test results are shown in Table 1.
[0054] Comparative Example 1 The target composition of the matrix glass is 48 mol%. 0 mol% 10 mol% 42 mol% Weigh , , ,total The glass melting temperature was 550℃, and the holding time was 10 minutes. The phosphor used was the white phosphor prepared in Example 1, with a loading of 10 wt%. All other preparation conditions were the same as in Example 5. The test results are shown in Table 1.
[0055] Comparative Example 2 The matrix glass composition and preparation conditions were the same as in Example 5. Only the amount of white phosphor prepared in Example 1 was changed; the following was weighed... The phosphor was added to the glass melt, resulting in a phosphor loading of 3 wt%. The remaining preparation and testing methods were the same as in Example 5. The test results are shown in Table 1.
[0056] Comparative Example 3 The matrix glass composition and preparation conditions were the same as in Example 5. Only the amount of white phosphor prepared in Example 1 was changed; the following was weighed... The phosphor was added to the glass melt, resulting in a phosphor loading of 20 wt%. The remaining preparation and testing methods were the same as in Example 5. The test results are shown in Table 1.
[0057] Comparative Example 4 The matrix glass composition and phosphor were the same as in Example 5. The dried mixture was placed in a muffle furnace heated to 600°C and held for 10 minutes. After removal, it was added... The white phosphor prepared in Example 1 was stirred at 5 rpm for 15 seconds. The remaining preparation and testing methods were the same as in Example 5. The test results are shown in Table 1.
[0058] Comparative Example 5 The matrix glass composition, melting conditions, and phosphor were the same as in Example 5. Added... After preparing the white phosphor in Example 1, it was stirred at 5 rpm for 60 seconds. The remaining preparation and testing methods were the same as in Example 5. Due to the excessive stirring time, the melt had significantly solidified, resulting in poor sample formation and an uneven surface. After grinding and polishing, a test sample was barely obtained. The test results are shown in Table 1.
[0059] The performance test results of each embodiment and comparative example are shown in Table 1. The comparison of lumen output and lumen efficiency of the phosphor-glass composite materials prepared in Examples 2 to 5 under 405nm violet laser excitation is shown in Table 1. Figure 7 A schematic diagram of the test results showing the emission of white light from a phosphor-glass composite material excited by a 405nm violet laser is shown below. Figure 3As shown, all embodiments and comparative examples used the same testing apparatus and conditions.
[0060] Table 1 shows the performance test results for each embodiment and comparative example: Table 1
[0061] Comparative Example 1 (excluding) A comparison with Example 5 shows that the color rendering index and internal quantum efficiency of the two are not significantly different in the initial state, but the laser saturation threshold of the former is only 0.5W, far lower than the latter's 1.5W. This is because it does not contain... At that time, under 405nm violet light excitation, the glass in The free electrons generated by photoionization cannot be effectively captured and combine with glass defects to form color centers, leading to premature photo-blackening and thermal quenching. back, Mixed valence states form intermediate energy level trap states, rapidly capturing free electrons and blocking the color center formation path. This proves that SnO is a necessary component for realizing high-power violet light excitation.
[0062] Comparative Example 2, with a phosphor loading of 3 wt%, had a color rendering index of only 82.1, indicating insufficient excitation light absorption and spectral conversion at a lower loading. Comparative Example 3, with a phosphor loading of 20 wt%, saw its internal quantum efficiency drop to 62.5%, because the phosphor particle spacing was too small, causing repeated absorption of emitted light by adjacent particles, especially blue light being absorbed by red phosphor, resulting in significant energy loss. Examples 2 to 5, with phosphor loadings ranging from 5 to 15 wt%, exhibited superior color rendering index and quantum efficiency, demonstrating the rationality of the 5-15 wt% range.
[0063] A comparison of Examples 5 and 6 shows that the internal quantum efficiency is only 71.2% when mixed in equal proportions, while it reaches 81.1% with a 6:5:4:2:1 ratio, and the color rendering index also increases from 90.5 to 94.1. This is because the red powder is relatively excessive when mixed in equal proportions, significantly increasing its reabsorption of blue and green light, while the blue light component is relatively insufficient, causing the spectral white balance to deviate from the optimal point. Example 7 uses... Alternative The color rendering index dropped to 90.2, and the R9 value decreased from 85.3 to 68.7 because... The emission peak is located near 620nm, and the red light saturation is lower than... It emits a deep red light at 650nm. Example 8 uses only blue and red phosphors, with a color rendering index of only 85.3, because it lacks emission in the green and yellow light bands, resulting in a discontinuous spectrum.
[0064] When the melting temperature of Comparative Example 4 was increased to 600℃, the internal quantum efficiency decreased to 68.0% because... Nitride phosphors begin to oxidize and denitrify on their surface above 600°C, reducing the number of luminescent centers. In Comparative Example 5, with the stirring time extended to 60 seconds, the internal quantum efficiency dropped to 65.0% because prolonged exposure of the phosphor in the high-temperature melt intensified interfacial reactions and caused the phosphor surface to be eroded by the glass components. In Examples 2 to 5, with melting temperatures of 350–550°C and stirring times of 3–15 seconds, the quantum efficiency remained between 76.5% and 81.1%, demonstrating that this process window effectively protected the phosphor.
[0065] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.
Claims
1. A high color rendering phosphor-glass composite material excited by violet light, characterized in that, The product comprises white phosphor and low-melting-point phosphate matrix glass; the white phosphor is uniformly dispersed in the low-melting-point phosphate matrix glass; the low-melting-point phosphate matrix glass contains at least the following components, in mole percentage: Tin fluoride: 40~55 mol% Tin oxide: 5~10 mol%. Sodium fluoride: 5~15 mol% Phosphorus pentoxide: 30~40 mol% The white phosphor accounts for 5-15 wt% of the mass percentage in the phosphor-glass composite material; The phosphor-glass composite material emits white light when excited by a 405nm violet laser.
2. The phosphor-glass composite material according to claim 1, characterized in that, The white phosphor contains components selected from... , , , , At least two of them.
3. The phosphor-glass composite material according to claim 2, characterized in that, The white phosphor contains .
4. The phosphor-glass composite material according to claim 2, characterized in that, The white phosphor contains , , , , Five types of fluorescent powder.
5. The phosphor-glass composite material according to claim 4, characterized in that, The mass ratio of the five phosphors is: .
6. The phosphor-glass composite material according to claim 1, characterized in that, The low-melting-point phosphate matrix glass has the following composition: 48 mol% stannous fluoride, 7 mol% stannous oxide, 10 mol% sodium fluoride, and 35 mol% phosphorus pentoxide.
7. A method for preparing a phosphor-glass composite material as described in any one of claims 1 to 6, characterized in that, Includes the following steps: (1) Provide a low melting point phosphate matrix glass raw material, wherein the low melting point phosphate matrix glass raw material contains at least stannous fluoride, stannous oxide, sodium fluoride and phosphate precursor, and the components are mixed in molar percentage, ground and then heated and melted at 350~550℃ for 10~30 minutes to obtain glass melt; (2) Add the prepared white phosphor to the glass melt and stir at a speed of 1-5 rpm for 3-15 seconds to make the phosphor evenly dispersed; (3) The mixed melt is quickly poured into a preheated mold and cooled in air to obtain the phosphor-glass composite material.
8. The preparation method according to claim 7, characterized in that, The mixing described in step (1) involves grinding each component together with anhydrous ethanol into a slurry, followed by thorough drying.
9. The preparation method according to claim 7, characterized in that, The heating and melting temperature in step (1) is 400~550℃ and the time is 10~20 minutes.
10. The preparation method according to claim 7, characterized in that, The stirring speed in step (2) is 3~5 rpm and the stirring time is 3~10 seconds.
Citation Information
Patent Citations
Narrow-band emission fluorescent powder-glass composite material for laser fluorescent display as well as preparation method and application thereof
CN120923144A
Luminescent glass, producing method thereof and luminescent device
EP2481572A1