A method for preparing pozzolanic composite materials by synergistic modification of coal gasification slag and limestone powder
By using a synergistic modification method of coal gasification slag and limestone powder, the problems of high cost and secondary pollution in the resource utilization of coal gasification slag are solved, and a highly active pozzolanic composite material is prepared, which is suitable for cement, mortar and concrete.
Patent Information
- Application Number
- CN202611404816.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-10
- Publication Date
- 2026-11-17
AI Technical Summary
The resource utilization of coal gasification slag is subject to high costs, long process flow and secondary pollution risks. In addition, the chemical composition and particle size distribution of different coal gasification slags vary greatly, which limits their large-scale utilization.
A highly active pozzolanic composite material was prepared by using a synergistic modification method of coal gasification slag and limestone powder, including steps such as preheating and dehydration, crushing and screening, heating and melting, water quenching and rapid cooling, iron selection and impurity removal, and mechanical grinding.
It realizes the resource utilization of coal gasification slag, reduces secondary pollution, adapts to the differences of different coal gasification slags, and prepares highly active pozzolanic composite materials to meet the requirements of cement, mortar and concrete.
Smart Images

Figure CN123106047A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of solid waste resource utilization, specifically relating to a method for preparing pozzolanic composite materials by synergistic modification of coal gasification slag and limestone powder. Background Technology
[0002] The rapid development and application of coal gasification technology has provided a solid guarantee for the clean and efficient utilization of coal in my country. However, the inorganic minerals and unconverted carbon in coal generate a large amount of coal gasification slag after being oxidized at high temperatures in the gasifier. Coal gasification enterprises typically dispose of this slag through landfill or open-air storage, which is costly, occupies a large amount of land resources, and poses potential pollution to surrounding water bodies, soil, and the atmosphere. Therefore, the safe disposal and resource utilization of coal gasification slag has become a key issue restricting the green development of the coal gasification industry.
[0003] Current research, including patent literature, indicates that the main pathways for the resource utilization of coal gasification slag are carbon-ash separation, preparation of cementitious materials, and recovery of valuable components. However, existing processes all suffer from high costs, long process flows, and high risks of secondary pollution. Furthermore, due to the influence of coal quality, fluxing agents, and gasification processes, the chemical composition, particle size distribution, and residual carbon content of different coal gasification slags vary significantly, which also greatly limits their large-scale utilization. Summary of the Invention
[0004] To address the aforementioned technical problems, this invention proposes a method for preparing pozzolanic composite materials by synergistic modification of coal gasification slag and limestone powder.
[0005] The technical solution adopted in this invention is: A method for preparing pozzolanic composite materials by synergistic modification of coal gasification slag and limestone powder includes the following steps: a. Preheat, dehydrate, crush, and screen the coal gasification slag to obtain coal gasification slag with the target particle size; b. Mix the coal gasification slag of the target particle size with limestone powder to obtain a mixture; c. The mixture is heated and melted to reconstruct the components, thus obtaining the modified product; d. The modified product is rapidly cooled by water quenching, then dehydrated, and then separated by iron selection and impurity removal to obtain iron-rich material and iron-removed material respectively. e. Mechanically grind and activate the iron-removed material to obtain a pozzolanic composite material.
[0006] Preferably, step a includes the following steps: a1. The coal gasification slag is fed into the preheater via a belt conveyor. The preheater removes moisture from the coal gasification slag, and the moisture content of the dehydrated coal gasification slag is controlled to be ≤5%. a2. After being dehydrated by the preheater, the coal gasification slag is then screened by a grading screen. The material under the screen is the coal gasification slag of the target particle size. The material over the screen is fed into a high-pressure roller mill to be crushed into small particles. The crushed small particles are then returned to the grading screen by a bucket elevator for screening again.
[0007] Preferably, step b includes the following steps: coal gasification slag of the target particle size is fed into the mixer through a first belt scale, and limestone powder is fed into the mixer simultaneously as a component regulator through a second belt scale to obtain a mixture; the mass ratio of limestone powder to coal gasification slag in the mixture is 1:9 to 7:3.
[0008] Preferably, step c includes the following steps: the uniformly mixed material is fed into a rotary kiln for high-temperature melting and component reconstruction; the temperature of the core area of the rotary kiln is controlled at 1200~1600℃, preferably 1400~1500℃; and the residence time of the mixture in the rotary kiln is controlled at 20~60min, preferably 30~40min.
[0009] Preferably, step c further includes the following step: maintaining a weak oxidizing atmosphere in the rotary kiln at all times.
[0010] Preferably, step d includes the following steps: d1. The modified product after component reconstruction in the rotary kiln is subjected to rapid cooling by water quenching to suppress melt crystallization and form a water-quenched modified product mainly composed of amorphous glass. At the same time, the thermal energy is converted into chemical energy and stored in the molecular structure of the modified product, thereby improving the pozzolanic activity of the modified product. d2. After water quenching, the modified product is dehydrated using a dewatering screen. The screen aperture size of the dewatering screen is 0.08~0.15 mm, preferably 0.10~0.12 mm. The material on the dewatering screen is fed into the iron removal and impurity removal device for further processing via a third belt scale. d3. Control the magnetic field strength of the iron separation and impurity removal device to 1000~4000 Gs, preferably 2000~3000 Gs; after separation by the iron separation and impurity removal device, iron-rich materials with iron grade ≥90% and iron-removed materials with iron grade ≤1.5% are obtained respectively, while removing hard particles with low activity and poor grinding ability from the modified products.
[0011] Preferably, step e includes the following steps: The iron-removed material discharged from the iron separation and impurity removal device is mechanically ground and activated by a vertical mill. Before the iron-removed material is fed into the vertical mill, the grinding aid is evenly sprayed onto the surface of the iron-removed material in the form of atomization. The vertical mill is equipped with a powder separation system, which can collect the activated products that meet the particle size requirements as a highly active pozzolanic mixture into a temporary storage bin in a timely manner. The vertical mill is also used in conjunction with an iron separator to remove iron-containing materials from the material. The resulting iron-containing material is incorporated into the iron-rich material produced in step d. The iron-removed material is returned to the vertical mill for re-grinding.
[0012] Preferably, the grinding aid is a combination of one or more of triethanolamine, triisopropanolamine, and aminosilane coupling agent, and its addition amount is 0.2‰ to 1.0‰ of the mass of the iron-removing material, preferably 0.4‰ to 0.6‰.
[0013] The water content of the above-mentioned activated products does not exceed 1%, and the specific surface area reaches 500 m². 2 The activity index of granulated blast furnace slag powder is above 95% and 105% at 7 days and 28 days, respectively, meeting the requirements for use in cement, mortar and concrete.
[0014] The beneficial technical effects of the present invention are as follows: (1) This invention combines coal gasification slag and limestone powder, and combines them through high-temperature component reconstruction, water quenching and rapid cooling, grinding and activation processes to obtain highly active pozzolanic mixed material and iron-rich material. This effectively realizes the resource-environmental utilization of coal gasification slag and the recovery of valuable components. Moreover, the process is low-cost and has little secondary pollution. Furthermore, the processing technology of this invention is not affected by the differences in the chemical composition of coal gasification slag, and can realize the resource-based and large-scale utilization of coal gasification slag.
[0015] (2) This invention constructs a synergistic component reconstruction system of coal gasification slag and limestone powder, and proposes a resource utilization process of “synergistic component reconstruction-water quenching-iron selection and impurity removal-mechanical grinding and activation” suitable for multi-source solid waste, realizing the multi-effect integration of coal gasification slag residual carbon removal, iron-containing material recovery and high-activity pozzolanic mixture preparation.
[0016] (3) The present invention uses limestone powder rich in CaO as a component regulator. By adjusting the ratio of coal gasification slag and limestone powder, the chemical composition of the modified product is optimized and adjusted under high temperature melting state.
[0017] (4) This invention uses a high-temperature, weakly oxidizing atmosphere to convert the residual carbon in the coal gasification slag into CO with reducing properties, and converts the iron-containing materials in the coal gasification slag into iron-rich materials with an iron grade of ≥90% for recycling.
[0018] (5) This invention uses water quenching to suppress melt crystallization and transforms the modified product into a highly active pozzolanic composite material with a significant glassy phase separation structure through reconstruction of the aluminosilicate network and mechanical grinding activation. This composite material meets the technical requirements of S105 grade blast furnace slag powder in "Granulated blast furnace slag powder for use in cement, mortar and concrete (GB / T 18046-2017)", and can be used as an admixture for cement, mortar and concrete, or can be prepared into a cementitious material that meets the requirements of mine cementitious filling by chemical activation. Attached Figure Description
[0019] Figure 1 This is a schematic diagram of the process flow for preparing pozzolanic composite materials by synergistic modification of coal gasification slag and limestone powder according to the present invention. Figure 2 This is a schematic diagram showing the connections of the various devices involved in the process of this invention; Figure 3 The image shows the modified product obtained after water quenching and rapid cooling in a specific application example of the present invention. Figure 4 The image shows the iron-removed material obtained after magnetic separation in a specific application example of the present invention. Figure 5 The image shows an example of iron-rich material obtained through magnetic processing in a specific application example of the present invention. Figure 6 The image shows a highly active pozzolanic composite material obtained in a specific application example of the present invention. Detailed Implementation
[0020] Coal gasification slag possesses a typical glassy phase-separated structure, with its chemical composition primarily consisting of SiO2, Al2O3, Fe2O3, and CaO, demonstrating its potential as a pozzolanic admixture. However, the excessively high residual carbon content and the difficulty of mechanical grinding and activation result in a low activity index for the raw coal gasification slag, making it unsuitable for direct use as a pozzolanic admixture. Furthermore, the CaO content in coal gasification slag is only around 10%, far lower than that of pozzolanic admixtures such as "granulated blast furnace slag powder for use in cement, mortar, and concrete (GB / T 18046-2017)". Therefore, this invention proposes using limestone powder with high CaO content as a component modifier, and through chemical composition reconstruction and mechanical grinding and activation, co-modifying coal gasification slag and limestone powder to prepare a highly active pozzolanic admixture, achieving synergistic and efficient resource utilization of multi-source solid waste. This admixture can be used as an admixture in cement, mortar, and concrete, or it can be chemically activated to prepare a cementitious material that meets the requirements for mine cementitious filling.
[0021] like Figure 1 , Figure 2 As shown, a method for preparing pozzolanic composite materials by synergistic modification of coal gasification slag and limestone powder includes the following steps: a. The coal gasification slag is preheated, dehydrated, crushed, and screened to obtain coal gasification slag of the target particle size.
[0022] Specifically, the following steps are included: a1. Preheating and dehydration; The coal gasification slag is first fed into the preheater 2 via belt conveyor 1. The function of the preheater 2 is to remove moisture from the coal gasification slag, thereby reducing energy consumption in subsequent modification processes. The moisture content of the dehydrated coal gasification slag is ≤10%, preferably ≤5%.
[0023] a2. Crushing and screening; The gasification slag, after being dehydrated by preheater 2, is then screened by grading screen 3. The undersize material is the gasification slag with the target particle size. The oversize material is fed into high-pressure roller mill 6 and crushed into small particles. The crushed small particles are then returned to grading screen 3 via bucket elevator 7 for further screening. To balance material throughput and crushing efficiency, grading screen 3 uses a 3 mm × 5 mm screen surface.
[0024] b. Mix the coal gasification slag of the target particle size with limestone powder to obtain a mixture.
[0025] The target particle size of the coal gasification slag is fed into the mixer 5 via the first belt scale 4, while limestone powder, as a component regulator, is simultaneously fed into the mixer 5 via the second belt scale 8, resulting in a mixture. The mass ratio of limestone powder to coal gasification slag in the mixture is 1:9 to 7:3, preferably 4:6 to 6:4. The limestone powder is mainly used to supplement the CaO component and adjust the relative proportions of chemical components such as SiO2, Al2O3, and CaO in the mixture, providing a prerequisite for improving the activity index of the modified product.
[0026] c. The mixture is heated and melted to reconstruct the components, thus obtaining the modified product.
[0027] The uniformly mixed material from mixer 5 is fed into rotary kiln 9 for high-temperature melting and component reconstruction. The temperature in the core zone of rotary kiln 9 is controlled at 1200~1600℃, preferably 1400~1500℃. The residence time of the mixture in the rotary kiln is controlled at 20~60min, preferably 30~40min.
[0028] During the synergistic component reconstruction and modification process of coal gasification slag and limestone powder, a weak oxidizing atmosphere is maintained throughout the rotary kiln 9. This allows the residual carbon in the coal gasification slag to generate reducing CO under high temperature, reducing the iron oxides in the mixture to elemental iron or magnetic iron oxides, so that the iron-rich materials generated can be recovered by magnetic separation in the subsequent process.
[0029] Furthermore, the waste heat of the rotary kiln can be used as a heat source for the preheater 2, the iron ore removal device 12, and the vertical mill 13.
[0030] d. The modified product is rapidly cooled by water quenching, then dehydrated, and then separated by iron selection and impurity removal to obtain iron-rich material and iron-removed material respectively.
[0031] Specifically, the following steps are included: d1. Water quenching and rapid cooling; The modified product, whose composition has been reconstructed by rotary kiln 9, is subjected to rapid cooling by water quenching to suppress melt crystallization and form a water-quenched modified product mainly composed of amorphous glass phase. At the same time, thermal energy is converted into chemical energy and stored in the molecular structure of the modified product, thereby improving the pozzolanic activity of the modified product.
[0032] d2, Dehydration; The modified product is dehydrated using a dewatering screen 10 after water quenching. The screen aperture size of the dewatering screen 10 is 0.08~0.15 mm, preferably 0.10~0.12 mm. The water under the dewatering screen 10 is reused, and the material over the dewatering screen 10 is fed into the iron removal and impurity removal device 12 via a third belt scale 11 for further processing.
[0033] d3. Iron-rich material recovery; The dehydrated modified product is conveyed by the third belt scale 11 to the iron separation and impurity removal device 12. After separation by the iron separation and impurity removal device 12, iron-rich material with an iron grade ≥90% and iron-removed material with an iron grade ≤1.5% are obtained respectively. At the same time, hard particles with low activity and poor grinding properties are removed from the modified product. The magnetic field strength of the iron separation and impurity removal device 12 is 1000~4000 Gs, preferably 2000~3000 Gs.
[0034] Furthermore, the iron separation and impurity removal device 12 is connected to a hot air duct, which can realize the pre-dehydration of materials. After the modified product is separated by the iron separation and impurity removal device 12, the separation and enrichment of iron-rich materials can realize the recovery and utilization of iron elements in coal gasification slag, and at the same time improve the grindability of the iron-removed materials, providing a prerequisite for the mechanical grinding and activation of the iron-removed materials.
[0035] e. Mechanically grind and activate the iron-removed material to obtain a pozzolanic composite material.
[0036] The iron-removed material discharged from the iron removal device 12 is mechanically ground and activated by a vertical mill 13. Before the iron-removed material is fed into the vertical mill 13, the grinding aid is evenly sprayed onto the surface of the iron-removed material in an atomized form by the grinding aid addition device 14. The grinding aid is a complex composed of one or more of triethanolamine, triisopropanolamine, and aminosilane coupling agent, and its addition amount is 0.2‰~1.0‰ of the mass of the iron-removed material, preferably 0.4‰~0.6‰. The vertical mill 13 is equipped with a powder classification system, which can promptly collect the activation products that meet the particle size requirements as a highly active pozzolanic mixture into a temporary storage bin to improve the mechanical grinding and activation efficiency of the iron-removed material. In addition, the vertical mill 13, in conjunction with the iron separator 14, completes the removal of iron-containing materials from the material. The resulting iron-containing material is incorporated into the iron-rich material produced in step d, and the iron-removed material is returned to the vertical mill 13 for re-grinding. The waste heat of the vertical mill 13 is introduced into the preheater 2 through pipelines for utilization.
[0037] After mechanical grinding and activation, the water content of the activated product does not exceed 1%, and the specific surface area reaches 500 m². 2 The activity index of slag powder is above 95% and 105% at 7 days and 28 days, respectively, meeting the technical requirements of S105 grade slag powder in "Granulated blast furnace slag powder for use in cement, mortar and concrete (GB / T 18046-2017)".
[0038] The following uses coal gasification coarse slag as an example to illustrate the specific application of the present invention in more detail.
[0039] Table 1 shows the main chemical composition of coal gasification coarse slag; Table 1
[0040] Table 2 shows the main chemical composition of limestone powder; Table 2
[0041] The specific steps are as follows: (1) Crushing and screening of coarse slag from coal gasification; The coarse slag from coal gasification has a moisture content of 12.56% and is fed into preheater 2 by belt conveyor 1 at a feed rate of 10 t / h. Preheater 2 utilizes the waste heat from the tail gas of rotary kiln 9 to heat the coal gasification slag, with a residence time of 15-20 min. After preheating and dehydration, the moisture content of the coal gasification slag is reduced to 4.50%. The dehydrated coal gasification slag is then screened by grading screen 3 with a 3mm × 5mm screen surface. The wet basis mass of the undersize material is 8.44 t / h, and the dry basis mass is 8.06 t / h, which is fed into mixer 5 by first belt scale 4. The oversize material is rolled by high-pressure roller mill 6 and then returned to grading screen 3 by bucket elevator 7 to form a closed-loop circulation with a circulation rate of 2.29 t / h.
[0042] (2) Batching and mixing of coal gasification slag; The limestone powder, with a moisture content of 0.50%, is simultaneously fed into the mixer 5 after being weighed by the second belt scale 8. The dry basis mass ratio of limestone powder to coal gasification slag is 5:5. Considering that the dry basis mass of the coal gasification slag entering the mixer 5 in the previous step was 8.06 t / h, the amount of limestone powder added here is 8.10 t / h. The mixer 5 uses a twin-shaft gravity-free mixer with a rotation speed of 45 r / min and a material residence time of 2-3 min. The mass of the mixed material is 16.54 t / h, and the dry basis mass is 16.12 t / h.
[0043] (3) High-temperature melting component reconstruction of coal gasification slag and limestone powder; The uniformly mixed material from mixer 5 is continuously fed into rotary kiln 9. The molten product discharged from rotary kiln 9 is then rapidly cooled by water and dehydrated by dewatering screen 10 to obtain a modified product, such as... Figure 3 As shown. The wet basis mass of the modified product is 12.41 t / h, with a moisture content of 8.80%, corresponding to a dry basis mass of 11.32 t / h. The mass loss in this process is mainly caused by the release of CO2 from the decomposition of limestone powder and the decarburization of coal gasification slag. The kiln tail exhaust gas is directed to the preheater 2, the iron ore removal device 12, and the vertical mill 13, respectively. The underflow water from the dewatering screen 10 is returned to the water quenching tank for recycling, and the water temperature in the water quenching tank is controlled below 50℃.
[0044] (4) Magnetic separation for iron removal; The dehydrated modified product is uniformly fed into the iron separation and impurity removal device 12 by the third belt scale 11. The iron separation and impurity removal device 12 is equipped with a permanent magnet drum separator with a magnetic field strength of 3000 Gs and a drum rotation speed of 35 r / min. After magnetic separation, iron-rich material, iron-removed material, and low-activity hard particles are obtained. The iron-removed material is as follows: Figure 4 As shown, iron-rich materials such as Figure 5As shown in the figure, the iron-rich material has a mass of 0.94 t / h and a total iron grade of 91.20%; the iron-removed material has a mass of 10.44 t / h and a total iron grade of 1.42%; and the low-activity hard particles have a mass of 0.05 t / h.
[0045] (5) Preparation of highly active pozzolanic composite material (mechanical grinding, activation and drying of iron-free materials); The iron-removed material is fed into the vertical mill 13 at a rate of 10.44 t / h. After being ground in the vertical mill 13, the iron-removed material is separated by the mill's built-in classifier system, yielding a highly active pozzolanic mixture, such as... Figure 6 As shown, the mass of the highly reactive pozzolanic composite material is 10.34 t / h, with a moisture content of 0.02% and a specific surface area of 523 m². 2 / kg, the activity indices at 3 days, 7 days and 28 days reached 83.40%, 99.94% and 110.49% respectively, meeting the technical requirements of S105 grade slag powder in "Granulated Blast Furnace Slag Powder for Cement, Mortar and Concrete (GB / T 18046-2017)". The external circulating material of the vertical mill 13 undergoes secondary iron removal by the iron separator 14, with a secondary iron removal material mass of 0.04 t / h, which is combined with the iron-rich material obtained by the iron separation and impurity removal device.
[0046] In summary, using coal gasification slag with a moisture content of 12.56% as raw material, and with a feed rate of 10 t / h, the co-processing capacity of limestone powder can reach 8.10 t / h. After modification, both materials can produce 10.34 t of highly active pozzolanic composite material meeting the technical requirements of S105 grade slag powder and 0.98 t of iron-rich material with a total iron content ≥90% per hour.
Claims
1. A method for preparing pozzolanic composite materials by synergistic modification of coal gasification slag and limestone powder, characterized in that... Includes the following steps: a. Preheat, dehydrate, crush, and screen the coal gasification slag to obtain coal gasification slag of the target particle size; b. Mix the coal gasification slag of the target particle size with limestone powder to obtain a mixture; c. The mixture is heated and melted to reconstruct the components, thereby obtaining the modified product; d. The modified product is rapidly cooled by water quenching, then dehydrated, and then separated by iron selection and impurity removal to obtain iron-rich material and iron-removed material respectively. e. Mechanically grind and activate the iron-removed material to obtain a pozzolanic composite material.
2. The method for preparing pozzolanic composite materials by synergistic modification of coal gasification slag and limestone powder according to claim 1, characterized in that, Step a includes the following steps: a1. The coal gasification slag is fed into the preheater via a belt conveyor. The preheater removes moisture from the coal gasification slag, and the moisture content of the dehydrated coal gasification slag is controlled to be ≤5%. a2. After being dehydrated by the preheater, the coal gasification slag is then screened by a grading screen. The material under the screen is the coal gasification slag of the target particle size. The material over the screen is fed into a high-pressure roller mill to be crushed into small particles. The crushed small particles are then returned to the grading screen by a bucket elevator for screening again.
3. The method for preparing pozzolanic composite materials by synergistic modification of coal gasification slag and limestone powder according to claim 2, characterized in that, Step b includes the following steps: the target particle size of the coal gasification slag is fed into the mixer through the first belt scale, and limestone powder, as a component regulator, is simultaneously fed into the mixer through the second belt scale to obtain a mixture; the mass ratio of limestone powder to coal gasification slag in the mixture is 1:9~7:
3.
4. The method for preparing pozzolanic composite material by synergistic modification of coal gasification slag and limestone powder according to claim 3, characterized in that, Step c includes the following steps: the uniformly mixed material is fed into a rotary kiln for high-temperature melting and component reconstruction; the temperature of the core area of the rotary kiln is controlled at 1200~1600℃, and the residence time of the mixture in the rotary kiln is controlled at 20~60min.
5. The method for preparing pozzolanic composite materials by synergistic modification of coal gasification slag and limestone powder according to claim 4, characterized in that, Step c also includes the following step: maintaining a weak oxidizing atmosphere in the rotary kiln at all times.
6. The method for preparing pozzolanic composite materials by synergistic modification of coal gasification slag and limestone powder according to claim 5, characterized in that, Step d includes the following steps: d1. The modified product after component reconstruction in the rotary kiln is subjected to rapid cooling by water quenching to suppress melt crystallization and form a water-quenched modified product mainly composed of amorphous glass. At the same time, the thermal energy is converted into chemical energy and stored in the molecular structure of the modified product, thereby improving the pozzolanic activity of the modified product. d2. After water quenching, the modified product is dehydrated using a dewatering screen. The screen aperture size of the dewatering screen is 0.08~0.15 mm. The material on the dewatering screen is fed into the iron ore removal device for further processing via a third belt scale. d3. Control the magnetic field strength of the iron separation and impurity removal device to 1000~4000 Gs. After separation by the iron separation and impurity removal device, iron-rich materials with iron grade ≥90% and iron-removed materials with iron grade ≤1.5% are obtained respectively. At the same time, hard particles with low activity and difficult grinding are removed from the modified products.
7. The method for preparing pozzolanic composite materials by synergistic modification of coal gasification slag and limestone powder according to claim 6, characterized in that, Step e includes the following steps: The iron-removed material discharged from the iron separation and impurity removal device is mechanically ground and activated by a vertical mill. Before the iron-removed material is fed into the vertical mill, the grinding aid is evenly sprayed onto the surface of the iron-removed material in the form of atomization. The vertical mill is equipped with a powder separation system, which can collect the activated products that meet the particle size requirements as a highly active pozzolanic mixture into a temporary storage bin in a timely manner. The vertical mill is also used in conjunction with an iron separator to remove iron-containing materials from the material. The resulting iron-containing material is incorporated into the iron-rich material produced in step d. The iron-removed material is returned to the vertical mill for re-grinding.
8. The method for preparing pozzolanic composite material by synergistic modification of coal gasification slag and limestone powder according to claim 7, characterized in that: The grinding aid is a combination of one or more of triethanolamine, triisopropanolamine, and aminosilane coupling agent, and its addition amount is 0.2‰~1.0‰ of the mass of the iron-removing material.
9. A method for preparing pozzolanic composite materials by synergistic modification of coal gasification slag and limestone powder according to claim 8, characterized in that: The activated product has a water content of not more than 1%, a specific surface area of 500 m 2 2 / g or more, and an activity index of 95% or more at 7 d and 105% or more at 28 d, meeting the requirements of granulated blast furnace slag powder used in cement, mortar and concrete.