A modified steel slag aggregate, an anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture, its preparation method and application
By constructing an oil-resistant and flame-retardant composite interface layer on the surface of steel slag aggregate, the problems of insufficient anti-skid degradation and flame-retardant performance of steel slag asphalt mixture in oily pollution environments are solved, achieving efficient interface stability and stable adhesion of functional components, thus improving the overall performance of asphalt mixture.
Patent Information
- Application Number
- CN202611573808.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-12
- Publication Date
- 2026-11-17
AI Technical Summary
Existing steel slag asphalt mixtures have problems during use, such as uneven distribution of asphalt film, excessive local adsorption, unstable mortar coating, fluctuating interfacial adhesion, reduced skid resistance, uneven dispersion of flame retardants, increased mortar viscosity, decreased low-temperature toughness, and poor workability. In particular, their performance is insufficient in oily polluted environments.
An oil-resistant and flame-retardant composite interface layer is constructed on the surface of steel slag aggregate, including an oil-resistant adhesive base film, a fine powder pore-filling layer, and a coarse powder embedding layer. Through the combined use of interface pre-coating material and first- and second-grade oil-resistant and flame-retardant composite functional powders, a thin-layer composite structure is formed, which improves the adhesion stability between steel slag and asphalt mortar and the stable adhesion of functional components.
It achieves oil-resistant adhesion stability and flame-retardant and smoke-suppressing functions between steel slag and asphalt mortar, and improves the anti-skid retention capacity, flame-retardant and smoke-suppressing capacity, anti-scattering capacity and water stability of the mixture. It is suitable for asphalt paving projects with high performance requirements such as tunnels, underground passages, and long downhill slopes.
Smart Images

Figure CN123106052A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of asphalt pavement materials and functional paving technology in road engineering, specifically relating to a modified steel slag aggregate, an anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture, its preparation method, and its application. Background Technology
[0002] Steel slag is a major solid waste generated by the metallurgical industry. It is characterized by its rough surface, high strength, high hardness, and good wear resistance, and can be used as an aggregate in asphalt mixtures. Using steel slag in asphalt pavements not only helps improve the resource utilization level of industrial solid waste, but also helps improve the skid resistance and wear resistance of asphalt mixtures.
[0003] However, compared to natural aggregates, steel slag differs in surface porosity, angularity, alkaline active components, water absorption rate, and adsorption characteristics. When ordinary steel slag is directly used in asphalt mixtures, problems such as uneven asphalt film distribution, excessive local adsorption, unstable adhesive coating, and interfacial adhesion fluctuations easily occur. Especially in tunnels, underground passages, service area entrances and exits, long downhill slopes, and heavy traffic sections, ordinary asphalt adhesives are prone to softening, peeling, and skid resistance reduction after vehicles leak fuel, engine oil, lubricating oil, and other oily contaminants.
[0004] Existing technologies for steel slag asphalt mixtures primarily focus on controlling the stability of steel slag, improving water stability, optimizing gradation, treating steel slag with stabilizers, and warm-mix asphalt processes. For example, existing technologies improve the stability and road performance of steel slag asphalt mixtures through steel slag stabilizers, warm-mix asphalt, modified mineral powder, and staged mixing, while specifying the particle size of the steel slag stabilizer, the modified mineral powder, and the warm-mix agent. These technologies mainly address the inherent stability and water stability of steel slag, but do not address the construction of a composite interface structure on the steel slag surface that combines oil resistance, flame retardancy, smoke suppression, anti-skid texture retention, and adhesive reinforcement.
[0005] Existing flame-retardant asphalt mixtures typically employ aluminum hydroxide, magnesium hydroxide, phosphorus-based flame retardants, expanded graphite, nanomaterials, or modified flame-retardant additives to enhance their flame-retardant properties. While these methods can improve the flame-retardant ability of asphalt mixtures to some extent, directly incorporating flame retardants can easily lead to problems such as uneven dispersion, increased viscosity of the asphalt paste, decreased low-temperature toughness, and poor workability during construction. Simply increasing the amount of flame retardant may also affect the high-temperature stability, water stability, and crack resistance of the mixture.
[0006] Existing oil-resistant asphalt materials mostly focus on modifying the binder to improve service performance in oily environments by enhancing the oil softening resistance of the asphalt binder. However, simply improving the oil resistance of the binder cannot fully address issues such as uneven asphalt film on steel slag surfaces, migration of flame-retardant powders, surface texture being covered by the binder, and insufficient anti-skid retention after oil contamination.
[0007] Existing anti-scattering asphalt mixtures mostly improve the adhesion performance of the mortar by using polymer modifiers, fibers, or anti-scattering agents. However, these methods focus on reducing scattering losses and do not integrate the rough texture of the steel slag surface, oil-resistant mortar, flame-retardant functional powder, and interfacial micro-embedded structure into a unified design.
[0008] Therefore, there is an urgent need to develop a steel slag skeleton asphalt mixture and its preparation and construction method that can fully utilize the anti-skid and wear-resistant advantages of steel slag and achieve synergistic improvement in oil resistance, flame retardancy, smoke suppression, anti-scattering and road durability performance through the control of composite interface on the steel slag surface. Summary of the Invention
[0009] To solve the above-mentioned technical problems, the present invention adopts the following technical solution: This invention provides a modified steel slag aggregate, comprising steel slag aggregate and an oil-resistant and flame-retardant composite interface layer coated on a portion of the surface of the steel slag aggregate. The oil-resistant and flame-retardant composite interface layer comprises an oil-resistant adhesive base film, a fine powder pore-filling layer, and a coarse powder embedding layer. The oil-resistant adhesive base film is formed by coating a portion of the steel slag aggregate surface with an interface pre-coating material; the fine powder pore-filling layer is formed by the first-grade oil-resistant and flame-retardant composite functional powder entering the pores, pits and oil-resistant adhesive base film on the surface of the steel slag aggregate; the coarse powder embedding layer is formed by the second-grade oil-resistant and flame-retardant composite functional powder partially embedded in the oil-resistant adhesive base film and partially exposed.
[0010] The particle size of the steel slag aggregate is 2.36 mm to 13.2 mm. For example, when the mixture is SMA-13 or SMA-10, the steel slag aggregate refers to coarse steel slag aggregate with a particle size greater than 4.75 mm. When the mixture is SMA-5, the particle size range of the steel slag aggregate is 2.36 to 4.75 mm.
[0011] The oil-resistant and flame-retardant composite interface layer coating the local surface of the steel slag aggregate means that at least part of the edges, protrusions, and rough textures of the steel slag aggregate surface are exposed. The oil-resistant and flame-retardant composite interface layer is not a thick film structure that completely covers the surface of the steel slag aggregate, but rather a thin-layer composite interface structure formed on the basis of the micropores, pits, and rough textures of the steel slag surface. This structure can both improve the adhesion stability between the steel slag and the asphalt mortar and prevent the anti-skid texture of the steel slag from being completely covered by the mortar.
[0012] Similarly, the oil-resistant adhesive base film formed by coating the local surface of the steel slag aggregate with an interfacial pre-coating material refers to the oil-resistant adhesive base film penetrating into some open pores, pits, and microcracks on the steel slag surface, forming a thin adhesive film on the steel slag surface. This thin adhesive film is used to reduce the disordered adsorption of steel slag to subsequent asphalt mortar and improve the interfacial stability between steel slag and asphalt mortar.
[0013] The steel slag aggregate is steel slag aggregate that has passed aging, iron removal, crushing, screening, shaping, and stability testing. The preferred steel slag aggregate has a particle size of 4.75mm to 13.2mm, and more preferably consists of steel slag particles of 4.75mm to 9.5mm and steel slag particles of 9.5mm to 13.2mm.
[0014] Preferably, the steel slag aggregate has a crushing value of no more than 20%, a Los Angeles abrasion loss of no more than 20%, a needle-like particle content of no more than 8%, a weak particle content of no more than 3%, a free calcium oxide content of no more than 3.0%, a water immersion expansion rate that meets the stability requirements for steel slag aggregate for road use, and an adhesion to asphalt of no less than level 5.
[0015] The steel slag aggregate is used as the main anti-skid skeleton aggregate in this invention. Its rough surface, multi-faceted shape, and high wear resistance are used to improve the long-term anti-skid ability of the road surface. The oil-resistant and flame-retardant composite interface layer is used to improve the oil-resistant adhesion stability and flame-retardant and smoke-suppressing function between the steel slag surface and the asphalt mortar.
[0016] Preferably, the interface pre-coating material includes oil-resistant and low-smoke modified asphalt, oil-resistant toughening component, interface reinforcement component and anti-stripping component, in parts by weight: 100 parts oil-resistant and low-smoke modified asphalt, 5-20 parts oil-resistant toughening component, 0.5-3 parts interface reinforcement component and 0.2-1.0 parts anti-stripping component.
[0017] Furthermore, the oil-resistant, low-smoke modified asphalt is an asphalt binder obtained by oil-resistant toughening and low-smoke warm-mix modification of road petroleum asphalt. The road petroleum asphalt is No. 70 or No. 90 road petroleum asphalt.
[0018] Furthermore, the oil-resistant toughening component is one or more of petroleum resin, terpene resin, polyurethane prepolymer, epoxy modifying component, and rubber powder modifying component.
[0019] Furthermore, the interface enhancement component is one or more of silane coupling agents, titanate coupling agents, and aluminate coupling agents.
[0020] Furthermore, the anti-stripping component is one or more of amine anti-stripping agents, phosphate ester anti-stripping agents, hydrated lime, and cement.
[0021] Preferably, the thickness of the oil-resistant adhesive base film is 2μm to 6μm. When the thickness of the oil-resistant adhesive base film is less than 2μm, it is difficult to form a stable interface; when the thickness of the oil-resistant adhesive base film is greater than 6μm, it easily covers the edges and rough textures of the steel slag surface, which is not conducive to maintaining the anti-slip performance.
[0022] Preferably, the oil-resistant and flame-retardant composite functional powder comprises mineral carrier powder, flame-retardant and smoke-suppressing powder, oil-resistant regulating powder, and coupling modifier. The oil-resistant and flame-retardant composite functional powder serves both as a functional powder for the composite interface layer on the steel slag surface and as a functional filler in asphalt mixtures, replacing part or all of the ordinary mineral powder. By weight, it comprises 100 parts mineral carrier powder, 20-60 parts flame-retardant and smoke-suppressing powder, 10-35 parts oil-resistant regulating powder, and 0.5-3 parts coupling modifier.
[0023] Furthermore, the mineral carrier powder is one or more of the following: zeolite powder, diatomaceous earth, attapulgite, modified bentonite, basalt powder, steel slag powder, and limestone powder.
[0024] Furthermore, the flame-retardant and smoke-suppressing powder is one or more of magnesium hydroxide, layered double hydroxide, zinc borate, expanded graphite, and modified montmorillonite.
[0025] Furthermore, the oil-resistant regulating powder is one or more of the following: organic modified zeolite powder, activated silicate, porous carbonaceous micro powder, modified bentonite, and oleophobic mineral powder.
[0026] Furthermore, the coupling modifier is one or more of silane coupling agents, titanate coupling agents, aluminate coupling agents, and composite coupling agents.
[0027] The oil-resistant and flame-retardant composite functional powder includes a first-size oil-resistant and flame-retardant composite functional powder and a second-size oil-resistant and flame-retardant composite functional powder. Preferably, the first-size oil-resistant and flame-retardant composite functional powder has a particle size of less than 0.075 mm, and is used to enter the micropores, pits, and oil-resistant adhesive base film on the surface of the steel slag aggregate to form a fine powder pore-filling layer. The second-size oil-resistant and flame-retardant composite functional powder has a particle size of 0.075 mm to 0.30 mm, and is used to form a coarse powder embedding layer on the outside of the oil-resistant adhesive base film.
[0028] The preparation method of the oil-resistant and flame-retardant composite functional powder is as follows: mineral carrier powder, flame-retardant and smoke-suppressing powder and oil-resistant regulating powder are premixed evenly and then silane coupling agent is added for surface modification to obtain modified mixed powder. One portion of the modified mixed powder is ground and sieved to produce a first-grade oil-resistant and flame-retardant composite functional powder with a particle size of less than 0.075 mm; the other portion uses 0.075-0.30 mm porous zeolite particles as carrier particles, and the modified mixed powder is loaded onto the surface of the carrier particles and some open pores. After drying and sieving, a second-grade oil-resistant and flame-retardant composite functional powder with a particle size of 0.075-0.30 mm is obtained.
[0029] Preferably, the mass ratio of the first-grade oil-resistant and flame-retardant composite functional powder to the second-grade oil-resistant and flame-retardant composite functional powder is 3:7 to 7:3, more preferably 4:6 to 6:4.
[0030] This invention also discloses a method for preparing the above-mentioned modified steel slag aggregate, comprising the following steps: Step 1: Preheating and dust removal of steel slag aggregate The steel slag aggregate, after aging, iron removal, crushing, screening and shaping, is heated to 135℃~160℃, and the surface dust of the steel slag is removed by hot air, screening or mechanical stirring, so that the moisture content of the steel slag aggregate is no more than 0.3%.
[0031] Step 2: Preparation of the oil-resistant adhesive base film An interface pre-coating material is added to the preheated steel slag aggregate. The amount of the interface pre-coating material is 0.20% to 0.80% of the mass of the steel slag aggregate, preferably 0.35% to 0.60%.
[0032] Mixing at 130℃~155℃ for 20s~50s allows the interface pre-coating material to form an oil-resistant and adhesive bottom film on the surface of the steel slag aggregate.
[0033] The pre-coating material penetrates into some of the open pores, pits, and microcracks on the surface of the steel slag, forming a thin adhesive film on the steel slag surface. This thin adhesive film reduces the disordered adsorption of steel slag onto subsequent asphalt mortar, improving the interfacial stability between the steel slag and the asphalt mortar.
[0034] Step 3: Preparation of the fine powder pore-filling layer (first-stage functional powder pore filling) A first-stage oil-resistant and flame-retardant composite functional powder is added to the steel slag aggregate that has formed an oil-resistant and adhesive base film. The first-stage oil-resistant and flame-retardant composite functional powder has a particle size of less than 0.075 mm and is used at a rate of 0.15% to 0.60% of the mass of the steel slag aggregate.
[0035] Mixing at 120℃~150℃ for 15s~35s allows the first-stage oil-resistant and flame-retardant composite functional powder to enter the pores, pits and oil-resistant adhesive bottom film on the steel slag surface, forming a fine powder pore-filling layer.
[0036] The fine powder filling layer is used to reduce the disordered adsorption of asphalt on the steel slag surface and to make the flame-retardant, smoke-suppressing and oil-resistant functional components preferentially and stably adhere to the interface area of the steel slag surface.
[0037] Step 4: Preparation of the coarse powder embedding layer (second-stage functional powder embedding) A second-grade oil-resistant and flame-retardant composite functional powder is added to the steel slag aggregate after fine powder filling. The particle size of the second-grade oil-resistant and flame-retardant composite functional powder is 0.075mm to 0.30mm, and the dosage is 0.20% to 0.80% of the mass of the steel slag aggregate.
[0038] Mixing at 120℃~145℃ for 10s~30s causes the second-stage oil-resistant and flame-retardant composite functional powder to partially embed into the oil-resistant adhesive base film and partially expose on the surface of the steel slag aggregate, forming a coarse powder adhering layer.
[0039] The coarse powder intercalation layer is used to improve the mechanical bonding between the subsequent asphalt mortar and the steel slag surface, and to improve the flame retardant, smoke suppression and oil resistance functions at the interface of the steel slag skeleton.
[0040] Step 5: Interface Stability The steel slag aggregate that forms the oil-resistant and flame-retardant composite interface layer is kept at 110℃~140℃ for 3min~10min to ensure stable bonding of the oil-resistant adhesive base film, the fine powder pore-filling layer and the coarse powder embedding layer.
[0041] The total amount of the interface pre-coating material, the first-sized oil-resistant and flame-retardant composite functional powder, and the second-sized oil-resistant and flame-retardant composite functional powder is 0.55% to 2.20% of the mass of the steel slag aggregate. When the total amount is less than 0.55%, the interface modification effect is insufficient; when the total amount is greater than 2.20%, it is easy to cover the edges and rough texture of the steel slag surface, affecting the anti-slip performance.
[0042] This invention also discloses an anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture, comprising aggregates, oil-resistant and low-smoke modified asphalt, fiber stabilizers, and anti-stripping agents. By mass, the mineral material includes 35-70 parts of modified steel slag aggregate, 0-30 parts of auxiliary coarse aggregate, 15-35 parts of fine aggregate, and 8-12 parts of filler, with the sum of the mass parts of each mineral material component being 100 parts. The filler comprises 50% to 100% of oil-resistant and flame-retardant composite functional powder by mass and 0% to 50% of mineral powder by mass, wherein the mineral powder is ordinary mineral powder.
[0043] Preferably, the preparation method of the oil-resistant and flame-retardant composite functional powder in the anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture is as follows: After the mineral carrier powder, flame retardant and smoke suppressant powder and oil-resistant control powder are premixed evenly, a silane coupling agent is added for surface modification to obtain a modified mixed powder. After grinding, the modified mixed powder that meets the requirements of a 0.15 mm sieve passing rate of not less than 90% and a 0.075 mm sieve passing rate of not less than 80% is the oil-resistant and flame-retardant composite functional powder required for the preparation of the mixture. It is preferred to use the fine particles below 0.075 mm as the functional filler of the mixture.
[0044] Preferably, the amount of oil-resistant and low-smoke modified asphalt is 5.5% to 7.0% of the total mass of the aggregate, the amount of fiber stabilizer is 0.25% to 0.40% of the total mass of the anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture, and the amount of anti-stripping agent is 0.20% to 0.50% of the mass of the oil-resistant and low-smoke modified asphalt.
[0045] Preferably, the auxiliary coarse aggregate is one or more of basalt, diabase, and andesite. The auxiliary coarse aggregate is used to improve the continuity of the steel slag skeleton gradation, the workability of the mixture during construction, and the uniformity of compaction.
[0046] Preferably, the fine aggregate is one or more of basalt manufactured sand, diabase manufactured sand, andesite manufactured sand, or limestone manufactured sand. The fine aggregate has a sand equivalent of not less than 70% and a methylene blue value of not more than 3.0 g / kg.
[0047] The steel slag aggregate accounts for 50% to 85% of the total mass of coarse aggregate with a thickness of 4.75mm or more (modified steel slag aggregate + auxiliary coarse aggregate), preferably 60% to 75%. This proportion can ensure that the steel slag forms an effective anti-skid skeleton, while avoiding excessive steel slag content, which would lead to excessive mixture density, uneven asphalt adsorption, and reduced workability.
[0048] Preferably, the oil-resistant and low-smoke modified asphalt is composed of road petroleum asphalt, oil-resistant toughening component, low-smoke warm mix component, stabilizing component, and anti-aging component. By weight, 100 parts of road petroleum asphalt, 8-15 parts of oil-resistant toughening component, 1.5-4 parts of low-smoke warm mix component, 0.2-1.0 parts of stabilizing component, and 0.2-0.8 parts of anti-aging component.
[0049] The road petroleum asphalt is No. 70 or No. 90 road petroleum asphalt; the oil-resistant toughening component is one or more of petroleum resin, terpene resin, rubber powder, polyurethane prepolymer, and epoxy modified component; the low-smoke warm mix component is one or more of organic viscosity-reducing warm mix agent, surfactant-type warm mix agent, or foaming-type warm mix agent; the stabilizing component is one or more of compatibilizer, stabilizer, or antioxidant; the anti-aging component is preferably a compound system of hindered phenolic antioxidant and phosphite antioxidant.
[0050] When the oil-resistant, low-smoke modified asphalt is used in subsequent asphalt mixture mixing, it should form a continuous but not excessively thick asphalt film on the surface of the aggregate. Preferably, the equivalent film thickness of the oil-resistant, low-smoke modified asphalt on the surface of the aggregate is 6 μm to 11 μm, and more preferably 7 μm to 10 μm.
[0051] The oil-resistant and flame-retardant composite functional filler can replace 50% to 100% of the mass of ordinary mineral powder. When the project has high requirements for flame retardancy and oil resistance, the replacement ratio is preferably 70% to 100%; when the project has high requirements for low-temperature crack resistance and workability, the replacement ratio is preferably 50% to 80%.
[0052] The preferred type of anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture is a dense skeleton gradation.
[0053] When the mixture is SMA-13, the total mass of coarse aggregates larger than 4.75mm (modified steel slag aggregate + auxiliary coarse aggregate) accounts for 65% to 82% of the total mass of the aggregate. When the mixture is SMA-10, the total mass of coarse aggregate (modified steel slag aggregate + auxiliary coarse aggregate) larger than 4.75mm accounts for 60% to 78% of the total mass of the aggregate. When the mixture is SMA-5, the modified steel slag aggregate of 2.36mm to 4.75mm accounts for 55% to 70% of the aggregate mass, and the fine aggregate of 0mm to 3mm accounts for 20% to 35% of the aggregate mass. The present invention also discloses a method for preparing anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture as described above, comprising the following steps.
[0054] Step 1: Prepare modified steel slag aggregate using the above-described method. Step 2: Oil-resistant and low-smoke modified asphalt The road petroleum asphalt is heated to 160–170°C and kept in a fluid state; an oil-resistant toughening component is added, and premixed at 1000–1500 r / min for 20 min to allow the oil-resistant toughening component to be fully wetted and swollen; then it is sheared at 3500–4500 r / min at 165–175°C for 30 min; the temperature is lowered to 150–160°C, and a low-smoke temperature-mixing component, a stabilizing component, and an anti-aging component are added, and stirring is continued at 800–1200 r / min for 15–20 min; finally, it is kept at 150–160°C for 20–30 min to obtain oil-resistant low-smoke modified asphalt.
[0055] Step 3: Dry mixing of the skeleton The steel slag aggregate that forms the oil-resistant and flame-retardant composite interface layer is put into the mixing equipment along with auxiliary coarse aggregate, fine aggregate and fiber stabilizer for dry mixing for 20s to 50s.
[0056] Step 4: Wet mixing of oil-resistant and low-smoke modified asphalt Add oil-resistant and low-smoke modified asphalt to the dry-mixed aggregate and wet mix at 145℃~165℃ for 60s~100s to make the oil-resistant and low-smoke modified asphalt evenly coat the aggregate and form a stable mortar.
[0057] Step 5: Disperse and mix the remaining functional fillers. Add the remaining oil-resistant and flame-retardant composite functional filler and anti-stripping agent to the wet-mixed mixture, and continue mixing for 50s to 90s to obtain anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture.
[0058] The remaining oil-resistant and flame-retardant composite functional filler is added later in a dispersed manner, which can reduce the local dryness or agglomeration of the mortar caused by premature adsorption of asphalt by all functional fillers in the early stage, and improve the dispersion uniformity of functional fillers in the mixed mortar.
[0059] The preferred discharge temperature of the mixture is 145℃~160℃.
[0060] This invention also discloses the application of any of the aforementioned anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixtures. These mixtures are suitable for tunnels, underground passages, long downhill slopes, heavy-duty lanes, bridge-tunnel connection sections, service area entrances and exits, toll plazas, and other asphalt paving projects requiring high anti-skid, flame-retardant, oil-resistant, and anti-scattering properties. Preferably, SMA-13 and SMA-1 skeleton dense gradations are suitable for tunnel mainlines, heavy-duty lanes, long downhill slopes, and bridge-tunnel connection sections; SMA-5 skeleton dense gradation is suitable for thin-layer anti-skid functional overlays on existing pavements.
[0061] By adopting the above technical solution, the beneficial effects of the present invention are as follows: This invention constructs an oil-resistant and flame-retardant composite interface layer on the surface of steel slag aggregate, consisting of an oil-resistant adhesive base film, a fine powder pore-filling layer, and a coarse powder embedding layer. This enables the steel slag aggregate to not only serve as a skeleton aggregate in asphalt mixtures, playing a role in load-bearing and anti-skid functions, but also as a functional interface carrier, playing roles in oil resistance, flame retardancy, smoke suppression, interface reinforcement, and anti-scattering.
[0062] Compared with the direct mixing method of steel slag aggregate, the present invention first forms an oil-resistant adhesive base film on the surface of steel slag, which can reduce the disordered adsorption of asphalt on the surface of steel slag, improve the problem of uneven local asphalt film thickness on the surface of steel slag, and improve the bonding stability between steel slag and asphalt mortar.
[0063] Compared with the conventional method of directly adding mineral powder, this invention uses first-size functional powder to fill pores and second-size functional powder to embed, so that the oil-resistant and flame-retardant composite functional powder is preferentially and stably attached to the surface of steel slag, thereby reducing the agglomeration and migration of functional powder in the mixture and improving the effective utilization rate of functional components at the interface of steel slag skeleton.
[0064] Compared with ordinary thick film coating methods, the present invention controls the thickness of the oil-resistant adhesive base film and the amount of functional powder embedded, so that the edges and rough textures of the steel slag surface are partially exposed, avoiding the reduction of anti-slip performance due to the excessive thickness of the adhesive covering the steel slag texture.
[0065] Compared with ordinary flame-retardant asphalt mixtures, this invention does not simply rely on the external addition of flame retardants to improve flame retardant performance, but introduces flame-retardant, smoke-suppressing and oil-resistant functional components into the steel slag aggregate interface and asphalt mastic, so as to achieve synergistic functionalization of the skeleton interface and the mastic.
[0066] Compared with ordinary oil-resistant asphalt mixtures, this invention not only improves the oil resistance of the binder, but also enhances the interfacial stability and anti-skid texture retention in oily environments through the steel slag aggregate composite interface layer.
[0067] This invention can improve the anti-skid retention, flame retardant and smoke suppression, anti-scattering, water stability and high temperature stability of asphalt paving materials after being affected by oil. It is suitable for tunnels, underground passages, long downhill slopes, heavy-duty lanes and other asphalt paving projects with high requirements for anti-skid, flame retardant and oil resistance. Attached Figure Description
[0068] Figure 1 This is a flowchart illustrating the preparation process of the anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture of the present invention. Figure 2 This is a schematic diagram of the modified steel slag aggregate structure of the present invention. Detailed Implementation
[0069] Example 1: SMA-13 Anti-skid, Flame-retardant, and Oil-resistant Steel Slag Skeleton Asphalt Mixture This embodiment provides an SMA-13 anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture suitable for tunnel mainline carriageways, long downhill sections, and heavy traffic sections.
[0070] In this embodiment, the asphalt mixture uses modified steel slag aggregate as one of the aggregate components: The modified steel slag aggregate includes coarse steel slag aggregate and an oil-resistant and flame-retardant composite interface layer covering a portion of the surface of the coarse steel slag aggregate. The oil-resistant and flame-retardant composite interface layer includes an oil-resistant bonding base film, a fine powder pore-filling layer, and a coarse powder embedding layer. The oil-resistant bonding base film is formed by an interface pre-coating material covering a portion of the surface of the coarse steel slag aggregate. The fine powder pore-filling layer is formed by first-grade oil-resistant and flame-retardant composite functional powder entering the pores, pits, and oil-resistant bonding base film on the surface of the coarse steel slag aggregate. The coarse powder embedding layer is formed by second-grade oil-resistant and flame-retardant composite functional powder partially embedded in the oil-resistant bonding base film and partially exposed.
[0071] The modified steel slag aggregate uses 9.5mm~13.2mm and 4.75mm~9.5mm steel slag coarse aggregate. The steel slag coarse aggregate undergoes aging, iron removal, crushing, shaping, and screening. Its crushing value is no greater than 18%, its Los Angeles abrasion loss is no greater than 18%, its needle-like and flaky particle content is no greater than 6%, its free calcium oxide content is no greater than 2.5%, its water immersion expansion rate meets the stability requirements for road steel slag aggregate, and its adhesion to asphalt is no lower than level 5.
[0072] The interface pre-coating material comprises, by weight, 100 parts of oil-resistant and low-smoke modified asphalt, 10 parts of petroleum resin, 1.5 parts of KH-550 silane coupling agent, and 0.5 parts of high-temperature resistant polyamide amine liquid anti-stripping agent.
[0073] By weight, the oil-resistant and low-smoke modified asphalt comprises 100 parts of No. 70 road petroleum asphalt, 6 parts of C9 petroleum resin (softening point 100-120℃), 4 parts of nitrile rubber powder (acrylonitrile content preferably 30%-36%, particle size 40-80 mesh), 2.5 parts of Fischer-Tropsch wax-type organic viscosity-reducing temperature mixing agent, 0.5 parts of maleic anhydride grafted polyolefin compatibilizer, 0.2 parts of antioxidant 1010, and 0.2 parts of antioxidant 168. The oil-resistant and flame-retardant composite functional powder comprises, by weight, 60 parts of clinoptilolite powder, 40 parts of limestone powder (CaCO3 mass fraction not less than 90%), 25 parts of magnesium hydroxide (purity not less than 95%), 10 parts of zinc borate (2ZnO·3B2O3·3.5H2O type zinc borate), 8 parts of expanded graphite (initial expansion temperature not less than 200℃), 15 parts of activated silicate (porous activated calcium silicate powder), and 1.5 parts of KH-550 silane coupling agent.
[0074] The preparation method of the oil-resistant and flame-retardant composite functional powder is as follows: clinoptilolite powder, limestone mineral powder, magnesium hydroxide, zinc borate, expanded graphite and activated silicate are premixed evenly and then KH-550 silane coupling agent is added for surface modification to obtain modified mixed powder; a portion of the modified mixed powder is ground and sieved to form first-grade functional powder with a particle size of less than 0.075 mm; another portion of the modified mixed powder is attached to the surface of 0.075-0.30 mm porous zeolite particles, and after drying, it forms second-grade composite functional particles with a particle size of 0.075-0.30 mm.
[0075] The SMA-13 anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture in this embodiment includes aggregates, oil-resistant and low-smoke modified asphalt, fiber stabilizers, and anti-stripping agents: By weight, the aggregate comprises 52 parts of the modified steel slag aggregate, 22 parts of 4.75–9.5 mm basalt auxiliary coarse aggregate, 16 parts of 0–3 mm basalt manufactured sand, and 10 parts of oil-resistant and flame-retardant composite functional filler. The modified steel slag aggregate accounts for 70% of the total mass of the coarse aggregate (4.75 mm and above), and the oil-resistant and flame-retardant composite functional filler replaces all ordinary mineral powder.
[0076] The amount of oil-resistant and low-smoke modified asphalt is 6.2% of the aggregate mass. The fiber stabilizer is lignin fiber, with a dosage of 0.35% of the total mass of the asphalt mixture. The anti-stripping agent is a high-temperature resistant polyamide amine liquid anti-stripping agent, with a dosage of 0.30% of the oil-resistant and low-smoke modified asphalt mass.
[0077] like Figure 1 As shown in the figure, the preparation method of the anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture in this embodiment is as follows: First, modified steel slag aggregate is prepared: The steel slag coarse aggregate was heated to 155°C and dust removed to ensure a moisture content of no more than 0.3%. 0.5% (by weight of the steel slag coarse aggregate) of an interface pre-coating material was added to the steel slag coarse aggregate (either by mixing the raw materials of the interface pre-coating material and adding them to the steel slag coarse aggregate, or by directly adding the raw materials of the interface pre-coating material to the steel slag coarse aggregate). The mixture was stirred at 145°C for 30 seconds to form an oil-resistant adhesive base film on the surface of the steel slag. In this embodiment, the thickness of the oil-resistant adhesive base film was 4 μm.
[0078] Subsequently, 0.35% of the mass of the steel slag coarse aggregate is added as the first-grade oil-resistant and flame-retardant composite functional powder, the first-grade oil-resistant and flame-retardant composite functional powder having a particle size of less than 0.075 mm. The mixture is stirred at 135°C for 25 seconds to allow it to enter the pores, pits and oil-resistant adhesive bottom film on the surface of the steel slag, forming a fine powder filling layer.
[0079] Then, 0.55% of the mass of steel slag coarse aggregate is added as the second-grade oil-resistant and flame-retardant composite functional powder. The particle size of the second-grade oil-resistant and flame-retardant composite functional powder is 0.075mm to 0.30mm. The mixture is stirred at 130℃ for 20 seconds to partially embed it into the oil-resistant adhesive base film and partially expose it to form a coarse powder embedding layer.
[0080] The steel slag coarse aggregate that forms the oil-resistant and flame-retardant composite interface layer is kept at 125℃ for 5 minutes to ensure stable bonding of the oil-resistant adhesive base film, the fine powder filling layer and the coarse powder embedding layer.
[0081] Figure 2 This is a schematic diagram of the modified steel slag aggregate structure prepared in this embodiment. Figure 2 In this process, an oil-resistant bonding base film, a fine powder pore-filling layer, and a coarse powder embedding layer are sequentially formed on the surface of the steel slag coarse aggregate. The oil-resistant bonding base film is used to improve the oil-resistant adhesion stability between the steel slag and the asphalt mastic; the fine powder pore-filling layer is used to fill the pores and pits on the surface of the steel slag; the coarse powder embedding layer is used to improve the mechanical interlocking and flame-retardant oil-resistant properties of the subsequent mastic; and the edges and rough texture of the steel slag surface are at least partially exposed to maintain anti-skid performance.
[0082] Preparation of asphalt mixture: Basalt auxiliary coarse aggregate, basalt manufactured sand, and lignin fiber were added to the modified steel slag aggregate prepared above and dry-mixed for 30 seconds. Then, oil-resistant and low-smoke modified asphalt was added and wet-mixed at 155℃ for 80 seconds. Finally, oil-resistant and flame-retardant composite functional powder (meeting a 0.15 mm sieve passing rate of not less than 90% and a 0.075 mm sieve passing rate of not less than 80%) and anti-stripping agent were added and mixed for another 80 seconds. The discharge temperature of the mixture was controlled at 150℃~160℃. This yields SMA-13 anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture.
[0083] During construction, the paving temperature should be controlled at 140℃~150℃, the initial compaction temperature should not be lower than 125℃, the secondary compaction temperature should not be lower than 110℃, and the final compaction temperature should not be lower than 90℃.
[0084] Example 2: SMA-10 Anti-skid, Flame-retardant, and Oil-resistant Steel Slag Skeleton Asphalt Mixture This embodiment provides an SMA-10 anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture suitable for tunnel entrances and exits, bridge-tunnel connection sections, and wet transition sections.
[0085] The mixture in this embodiment includes mineral aggregates, oil-resistant and low-smoke modified asphalt, lignin fibers, and anti-stripping agents.
[0086] By weight, the mineral materials comprise 46.8 parts modified steel slag aggregate, 25.2 parts 4.75–9.5 mm diabase auxiliary coarse aggregate, 18.4 parts 0–3 mm basalt manufactured sand, 7.7 parts oil-resistant and flame-retardant composite functional powder, and 1.9 parts ordinary limestone mineral powder. The amount of oil-resistant and low-smoke modified asphalt is 6.0% of the aggregate mass; the amount of lignin fiber is 0.30% of the total mass of the mixture; and the amount of anti-stripping agent is 0.30% of the asphalt mass.
[0087] The preparation method of the mixture in this embodiment is as follows: First, modified steel slag aggregate is prepared: Preheat the steel slag coarse aggregate to 150℃; add 0.4% of the steel slag coarse aggregate mass of interface pre-coating material to the steel slag coarse aggregate, and mix at 140℃ for 30s to form an oil-resistant adhesive base film on the surface of the steel slag. Since the particle size of SMA-10 is small, in order to avoid the steel slag texture being overly covered by the mortar, control the thickness of the oil-resistant adhesive base film to be no more than 5μm during the mixing process, and avoid over-compaction during the rolling process.
[0088] Subsequently, 0.30% of the first-stage oil-resistant and flame-retardant composite functional powder by weight of steel slag coarse aggregate is added and mixed at 130℃ for 25 seconds, so that it enters the pores, pits and oil-resistant adhesive bottom film on the surface of steel slag to form a fine powder filling layer.
[0089] Then, 0.45% of the second-grade oil-resistant and flame-retardant composite functional powder by weight of steel slag coarse aggregate is added and mixed at 125℃ for 20 seconds, so that it is partially embedded in the oil-resistant adhesive base film and partially exposed, forming a coarse powder embedded layer.
[0090] Then, it is kept at 120℃ for 5 minutes to allow the oil-resistant adhesive base film, fine powder filling layer and coarse powder embedding layer to bond stably.
[0091] Next, prepare the mixture: Add diabase auxiliary coarse aggregate, basalt manufactured sand and lignin fiber to the modified steel slag aggregate prepared above and dry mix for 30s. Add oil-resistant and low-smoke modified asphalt at 155℃ and wet mix for 80s. Then add oil-resistant and flame-retardant composite functional filler, ordinary mineral powder and anti-stripping agent and continue mixing for 70s. The discharge temperature is controlled at 150-158℃.
[0092] The remaining undisclosed raw materials and preparation methods are the same as in Example 1.
[0093] This embodiment is applicable to road sections with high requirements for surface texture uniformity, wet slip safety, and anti-skid retention after oil stains.
[0094] Example 3: SMA-5 thin-layer anti-slip flame-retardant and oil-resistant steel slag overlay mixture This embodiment provides an SMA-5 thin-layer overlay compound suitable for skid-resistant repair of existing tunnel pavements, underground passages, and heavy-duty lanes.
[0095] The mixture in this embodiment includes mineral aggregates, oil-resistant and low-smoke modified asphalt, lignin fibers, and anti-stripping agents.
[0096] By weight, the mineral material includes 60 parts modified steel slag aggregate, 30 parts basalt manufactured sand of 0mm to 2.36mm, and 10 parts oil-resistant and flame-retardant composite functional powder.
[0097] The amount of oil-resistant and low-smoke modified asphalt is 6.5% of the aggregate mass, the amount of fiber stabilizer is 0.35% of the total mass of the mixture, and the anti-stripping agent is a high-temperature resistant polyamide amine anti-stripping agent, with a dosage of 0.30% of the oil-resistant and low-smoke modified asphalt mass.
[0098] The preparation method of the mixture in this embodiment is as follows: First, modified steel slag aggregate is prepared: Steel slag aggregate with a thickness of 2.36mm to 4.75mm was heated to 150℃, and 0.35% (by weight) of interface pre-coating material was added and mixed for 25 seconds to form an oil-resistant adhesive base film. In this embodiment, the thickness (equivalent average thickness) of the oil-resistant adhesive base film was controlled to be 3μm. 0.25% (by weight) of the first-grade oil-resistant and flame-retardant composite functional powder was added and mixed for 20 seconds to form a fine powder pore-filling layer. 0.35% (by weight) of the second-grade oil-resistant and flame-retardant composite functional powder was added and mixed for 15 seconds to form a coarse powder embedding layer. The mixture was then held at 120℃ for 5 minutes to allow the oil-resistant adhesive base film, fine powder pore-filling layer, and coarse powder embedding layer to bond stably.
[0099] Next, prepare the mixture: Then, dry-mix basalt manufactured sand and fiber stabilizer are added, followed by wet-mixing with oil-resistant and low-smoke modified asphalt. Finally, oil-resistant and flame-retardant composite functional powder and anti-stripping agent are added and mixed evenly.
[0100] The remaining undisclosed raw materials and preparation methods are the same as in Example 1.
[0101] In this embodiment, when used for thin overlays, the construction thickness is 1.5cm to 2.5cm. Before construction, the original road surface should be swept, roughened, or sandblasted, and an oil-resistant, high-viscosity bonding layer should be applied. After paving, a light steel wheel roller should be used for stabilization and final compaction to prevent thin-layer displacement, slurry bleeding, and the steel slag surface texture from being covered by adhesive slurry.
[0102] Comparative Example 1: The ordinary steel slag SMA-13 reference group uses unmodified steel slag aggregate with the same particle size and dosage. No oil-resistant adhesive bottom film, fine powder pore-filling layer and coarse powder embedding layer are set. The oil-resistant and flame-retardant composite functional filler in the aggregate is replaced by ordinary mineral powder of equal mass, and conventional modified asphalt is used. The remaining gradation and preparation conditions are the same as in Example 1.
[0103] Comparative Example 2: The types and total amount of functional materials used are the same as in Example 1, but the graded composite interface construction on the steel slag surface is not carried out. That is, the oil-resistant adhesive base film, the fine powder pore-filling layer and the coarse powder embedding layer are not formed separately. Instead, the corresponding interface pre-coating materials, the first-grade functional powder and the second-grade functional powder are directly added to the mixture in the same total amount and mixed together. The other conditions are the same as in Example 1.
[0104] Comparative Example 3: Based on Example 2, steel slag aggregate of the same grade without composite interface treatment was used, and the corresponding interface modification materials were directly added to the mixture in the same total amount. No graded interface construction was carried out, and the other conditions were the same as in Example 2.
[0105] Comparative Example 4 is based on Example 3, using the same graded steel slag aggregate without composite interface treatment. The corresponding interface modification materials are directly added to the mixture in the same total amount, without graded interface construction. The other conditions are the same as in Example 3.
[0106] To verify the road performance, anti-skid and oil-resistant properties, and flame-retardant and smoke-suppressing properties of the technical solution of the present invention, performance tests were conducted on Examples 1-3 and the corresponding comparative examples. The test indicators included dynamic stability, freeze-thaw splitting strength ratio, Kentaburg scattering loss, initial swing value, anti-skid retention rate after oil contamination, splitting strength retention rate after oil contamination, peak heat release rate, and total smoke production.
[0107] Performance Evaluation To evaluate the road performance and functional properties of the anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture of the present invention, performance tests were conducted on the embodiments and corresponding comparative examples. Dynamic stability, freeze-thaw splitting strength ratio, and Kentenberg scattering loss were tested according to the corresponding test methods in JTG3410—2025 "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering"; the initial pendulum value was tested using the pendulum tester method for testing the road surface friction coefficient in JTG 3450—2019 "Field Test Procedures for Highway Subgrade and Pavement"; the peak heat release rate and total smoke production were tested using the cone calorimeter method in GB / T 16172—2026 "Test Methods for Heat Release Rate and Smoke Production Rate of Building Materials".
[0108] Oil resistance was evaluated using the performance retention rate before and after oil contamination. Diesel-based oil contaminants, commonly used in road vehicle operation, were selected as the medium for treating molded asphalt mixture specimens under uniform conditions. The same oil contaminant, treatment method, treatment time, and post-treatment conditions were used in both the example and comparative examples for the same test item. After the oil contamination treatment, free oil contaminants were removed from the specimen surface and the specimens were conditioned. Subsequently, the pendulum value and splitting tensile strength of the specimens were tested and compared with the corresponding test results of the same batch of untreated specimens.
[0109] The anti-slip retention rate after oil contamination is calculated using the following formula: R_BPN = (BPN_oil / BPN_0) × 100% Where: R_BPN—anti-slip retention rate after oil contamination, %; BPN_oil—pendulum value of the specimen after oil contamination; BPN_0—pendulum value of the specimen before oil contamination.
[0110] The splitting strength retention rate after oil contamination is calculated using the following formula: R_ITS = (ITS_oil / ITS_0) × 100% Where: R_ITS—Splitting strength retention rate after oil contamination, %; ITS_oil—Splitting strength of specimen after oil contamination; ITS_0—Splitting strength of specimens in the same batch that have not been contaminated with oil.
[0111] Table 1. Road performance, anti-skid properties, and oil resistance of Example 1 and Comparative Examples
[0112] As shown in Table 1, the dynamic stability and freeze-thaw splitting strength ratio of Example 1 reached 7820 cycles / mm and 92.3%, respectively, which are higher than those of Comparative Example 1 and Comparative Example 2. Meanwhile, the Kentenberg spalling loss was reduced to 4.6%, indicating that the composite interface structure of this invention can maintain good high-temperature stability, water stability, and anti-spilling performance. The initial pendulum value of Example 1 was 82, a relatively small increase compared to the comparative examples. However, the anti-slip retention rate after oil contamination reached 91.4%, significantly higher than the 73.8% of Comparative Example 1 and 82.7% of Comparative Example 2; the splitting strength retention rate after oil contamination reached 89.2%, also significantly higher than the comparative examples. These results indicate that the main advantage of this invention is not simply improving the initial anti-slip level, but rather improving the stability of the steel slag skeleton interface and the ability to retain anti-slip performance after oil contamination.
[0113] Table 2 Flame retardant and smoke suppression performance of Example 1 and comparative examples
[0114] As shown in Table 2, compared with Comparative Example 1, the peak heat release rate of Example 1 decreased from 420 kW / m² to 320 kW / m², a reduction of approximately 23.8%; the total smoke production decreased from 11.2 m² / m² to 7.3 m² / m², a reduction of approximately 34.8%. Compared with Comparative Example 2, which used the same functional materials but did not construct a hierarchical composite interface, the peak heat release rate and total smoke production of Example 1 were further reduced. The results indicate that the oil-resistant and flame-retardant functional components can not only improve the flame-retardant and smoke-suppressing performance of the mixture, but also further enhance their effectiveness by preferentially configuring the functional components in the interface region of the steel slag skeleton.
[0115] Table 3 Road Performance of Mixtures
[0116] As shown in Table 3, the SMA-10 and SMA-5 mixtures prepared using the interface modification method of this invention exhibit better initial pendulum value, anti-slip retention rate after oil contamination, and anti-scattering performance than the corresponding comparative examples without composite interface construction. Simultaneously, the peak heat release rate is reduced. This indicates that the oil-resistant and flame-retardant composite interface construction method proposed in this invention is not only applicable to SMA-13 mixtures but also provides oil resistance, anti-slip properties, anti-scattering effects, and flame retardancy in mixtures with different nominal maximum particle sizes and thin-layer coatings.
[0117] The above embodiments are only preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical aspects of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.
Claims
1. A modified steel slag aggregate, characterized in that, It includes steel slag aggregate, and an oil-resistant and flame-retardant composite interface layer coating a portion of the surface of the steel slag aggregate. The oil-resistant and flame-retardant composite interface layer includes an oil-resistant adhesive base film, a fine powder pore-filling layer, and a coarse powder embedding layer. The oil-resistant adhesive base film is formed by coating a local surface of the steel slag aggregate with an interface pre-coating material; The fine powder filling layer is formed by the first-grade oil-resistant and flame-retardant composite functional powder entering the pores, pits and oil-resistant adhesive base film on the surface of the steel slag aggregate. The coarse powder embedding layer is formed by partially embedding the second-grade oil-resistant and flame-retardant composite functional powder into an oil-resistant adhesive base film and partially exposing it. The particle size of the steel slag aggregate is 2.36~13.2mm.
2. The modified steel slag aggregate according to claim 1, characterized in that, It also includes one or more of the following technical features: By weight, the interface pre-coating material comprises 100 parts of oil-resistant and low-smoke modified asphalt, 5 to 20 parts of oil-resistant toughening component, 0.5 to 3 parts of interface reinforcing component, and 0.2 to 1.0 parts of anti-stripping component. The thickness of the oil-resistant adhesive base film is 2μm~6μm.
3. The modified steel slag aggregate according to claim 1, characterized in that, It also includes one or more of the following technical features: By weight, the oil-resistant and flame-retardant composite functional powder comprises 100 parts of mineral carrier powder, 20-60 parts of flame-retardant and smoke-suppressing powder, 10-35 parts of oil-resistant regulating powder, and 0.5-3 parts of coupling modifier. The particle size of the first-grade oil-resistant and flame-retardant composite functional powder is less than 0.075 mm; The particle size of the second-grade oil-resistant and flame-retardant composite functional powder is 0.075 mm to 0.30 mm.
4. A method for preparing the modified steel slag aggregate according to any one of claims 1 to 3, characterized in that, Includes the following steps: Step 1: Preheating and dust removal treatment of steel slag aggregate; Step 2: Preparation of the oil-resistant adhesive base film: Add an interface pre-coating material to the steel slag aggregate after step one. The amount of the interface pre-coating material is 0.20% to 0.80% of the mass of the steel slag aggregate. Mix at 130℃ to 155℃ for 20s to 50s to form an oil-resistant adhesive base film on the surface of the steel slag aggregate. Step 3: Preparation of the fine powder pore-filling layer: Add the first-grade oil-resistant and flame-retardant composite functional powder to the steel slag aggregate after step two. The amount of the first-grade oil-resistant and flame-retardant composite functional powder is 0.15% to 0.60% of the mass of the steel slag aggregate. Mix at 120℃ to 150℃ for 15s to 35s to allow the first-grade oil-resistant and flame-retardant composite functional powder to enter the pores, pits and oil-resistant adhesive bottom film on the surface of the steel slag, forming a fine powder pore-filling layer. Step 4: Preparation of the coarse powder embedding layer: Add a second-sized oil-resistant and flame-retardant composite functional powder to the steel slag aggregate after step three. The amount of the second-sized oil-resistant and flame-retardant composite functional powder is 0.20% to 0.80% of the mass of the steel slag aggregate. Mix at 120℃ to 145℃ for 10s to 30s to make the second-sized oil-resistant and flame-retardant composite functional powder partially embedded in the oil-resistant adhesive bottom film and partially exposed on the surface of the steel slag aggregate, forming a coarse powder adhering layer. Step 5: Interface Stability: The steel slag aggregate treated in step four is kept at 110℃~140℃ for 3min~10min to ensure stable bonding of the oil-resistant adhesive base film, the fine powder filling layer and the coarse powder embedding layer.
5. A skid-resistant, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture, characterized in that, This includes mineral aggregates, oil-resistant and low-smoke modified asphalt, fiber stabilizers, and anti-stripping agents. By mass, the mineral material includes 35-70 parts of modified steel slag aggregate as described in any one of claims 1 to 3, 0-30 parts of auxiliary coarse aggregate, 15-35 parts of fine aggregate, and 8-12 parts of filler, and the sum of the mass parts of each mineral material component is 100 parts. The filler comprises 50% to 100% oil-resistant and flame-retardant composite functional powder and 0% to 50% mineral powder.
6. The anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture according to claim 5, characterized in that, It also includes one or more of the following technical features: The auxiliary coarse aggregate is one or more of basalt, diabase and andesite; The fine aggregate is one or more of the following: basalt manufactured sand, diabase manufactured sand, andesite manufactured sand, and limestone manufactured sand. By weight, the oil-resistant and low-smoke modified asphalt comprises 100 parts of road petroleum asphalt, 8-15 parts of oil-resistant toughening component, 1.5-4 parts of low-smoke warm mix component, 0.2-1.0 parts of stabilizing component and 0.2-0.8 parts of anti-aging component.
7. The anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture according to claim 5, characterized in that, The amount of the oil-resistant and low-smoke modified asphalt is 5.5% to 7.0% of the total mass of the aggregate; the amount of the fiber stabilizer is 0.25% to 0.40% of the total mass of the anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture; and the amount of the anti-stripping agent is 0.20% to 0.50% of the mass of the oil-resistant and low-smoke modified asphalt. And / or, the oil-resistant and flame-retardant composite functional powder selected in the filler is an oil-resistant and flame-retardant composite functional powder that meets the following requirements: a 0.15 mm sieve passing rate of not less than 90% and a 0.075 mm sieve passing rate of not less than 80%.
8. A method for preparing the anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture according to any one of claims 5 to 7, characterized in that, Includes the following steps: Step 1: Prepare modified steel slag aggregate using the method described in claim 4; Step 2: Preparation of oil-resistant, low-smoke modified asphalt Road petroleum asphalt is heated to 160-170℃ and kept in a fluid state. Oil-resistant toughening components are added for premixing, followed by high-speed shearing at 3500-4500 r / min at 165-175℃. The temperature is then lowered to 150-160℃, and low-smoke warm mix components, stabilizing components, and anti-aging components are added. Stirring continues for 15-20 min, and finally, the mixture is kept at 150-160℃ for 20-30 min to obtain oil-resistant low-smoke modified asphalt. Step 3: Dry mixing of the skeleton The modified steel slag aggregate, along with auxiliary coarse aggregate, fine aggregate, and fiber stabilizer, is put into a mixing equipment for dry mixing. Step 4: Wet mixing of oil-resistant and low-smoke modified asphalt Add oil-resistant and low-smoke modified asphalt to the dry-mixed aggregate, then wet-mix to ensure that the oil-resistant and low-smoke modified asphalt evenly coats the aggregate and forms a stable mortar. Step 5: Disperse and mix the remaining functional fillers. Add oil-resistant and flame-retardant composite functional filler and anti-stripping agent to the wet-mixed mixture, and continue mixing to obtain anti-skid, flame-retardant and oil-resistant steel slag skeleton asphalt mixture.
9. A method for preparing the anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture according to claim 8, characterized in that, It also includes one or more of the following technical features: Step (3) Dry mixing time is 20~50 s; Step (iv): The wet mixing temperature is 145~165℃, and the wet mixing time is 60~100s; Step (5) The mixing temperature is 50s to 90s, and the discharge temperature of the anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture is 145℃ to 160℃.
10. The application of the anti-skid, flame-retardant, and oil-resistant steel slag skeleton asphalt mixture according to any one of claims 5 to 7, characterized in that, Used for asphalt paving projects with high requirements for anti-skid, flame retardancy, oil resistance and anti-dispersion properties.