A zinc porphyrin monomer and its preparation method, and a method for preparing fluorescent microspheres.
Fluorescent microspheres with uniform particle size and good dispersibility were prepared by polymerizing zinc porphyrin monomer with styrene and acrylic acid and using homogenization-microfluidics technology. This solved the problem of unstable encoded information in traditional methods and enabled efficient biological applications.
Patent Information
- Application Number
- CN202611360787.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-03
- Publication Date
- 2026-11-17
AI Technical Summary
Existing methods for preparing fluorescently encoded microspheres suffer from problems such as the encoding information being easily affected by the external environment, small encoding capacity, and uneven encoding elements.
Carboxylated polystyrene crosslinked fluorescent microspheres were prepared by polymerizing zinc porphyrin monomer with styrene and acrylic acid. Combined with homogenization-microfluidics technology, fluorescent microspheres with uniform particle size and good dispersibility were prepared.
The prepared fluorescent microspheres have uniform particle size and good dispersibility, and their surface is covered with carboxyl functional groups, which facilitates biological applications and improves coding stability and efficiency.
Smart Images

Figure CN123106689A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of polystyrene-acrylic acid-porphyrin crosslinked microsphere technology, specifically to a zinc porphyrin monomer and its preparation method, and a method for preparing fluorescent microspheres. Background Technology
[0002] Fluorescent microspheres are solid particles with diameters ranging from nanometers to micrometers, loaded with fluorescent substances, and emitting fluorescence upon stimulation by external energy. In recent years, the application of fluorescent microspheres in the biomedical field has attracted increasing attention due to their inherent morphological stability, large specific surface area, strong adsorption, significant aggregation, strong surface reactivity, and stable and efficient luminescence. Furthermore, various properties can be endowed to microspheres according to their different applications, such as biospecific binding, hollow porosity, and magnetism, leading to their wide range of applications, particularly in immunoassay, high-throughput drug screening, drug carriers, immobilized enzymes, bacterial and viral diagnostics, single nucleotide polymorphism genotyping, cytokine identification, and cell analysis. Therefore, developing various methods to prepare fluorescent biolabeled microspheres, fluorescent encoded microspheres, or fluorescent sensing microspheres with different fluorescence properties and sizes not only has significant theoretical value but also practical application value for national economic development. In addition, various properties can be endowed to microspheres according to their different uses, such as biospecific binding, hollow porosity, and magnetism, thus enabling their wide application, especially in immunoassay, high-throughput drug screening, drug carriers, immobilized enzymes, bacterial and viral diagnostics, single nucleotide polymorphism genotyping, cytokine identification, and cell analysis.
[0003] Traditional methods for preparing fluorescently encoded microspheres mainly include organic solvent swelling, layer-by-layer self-assembly, and surface cross-linking. Organic solvent swelling is simple to operate, offers large encoding capacity, and is commercially available; however, the encoded information is easily affected by external environmental factors (such as organic solvents), and the encoding of internal microsphere components is uneven. Layer-by-layer self-assembly is based on spontaneous bonding through electrostatic interactions, requires no complex equipment, and has a wide range of applications; however, the encoding process is complex, it is difficult to obtain a large encoding capacity, and the encoding elements are located on the surface of the microsphere, making them susceptible to environmental influences.
[0004] In view of this, the present invention is hereby proposed. Summary of the Invention
[0005] This application provides a zinc porphyrin monomer and its preparation method, as well as a method for preparing fluorescent microspheres. The zinc porphyrin monomer provided by this invention produces fluorescent microspheres with uniform particle size and good dispersibility, which can meet market demand.
[0006] To achieve the above objectives, the present invention employs the following technical solution: This invention provides a zinc porphyrin monomer having the following structure: ; The exact molecular weight of the zinc porphyrin monomer is 809.2253.
[0007] In a specific feasible implementation, the following steps are included: Add p-carbonylbenzaldehyde, benzaldehyde, and propionic acid in a mass ratio of 1:3:4, stir to dissolve, and obtain solution A. Prepare solution B by dissolving pyrrole and propionic acid. Heat solution A, and add solution B dropwise to solution A while stirring. Continue stirring and reflux. Add anhydrous ethanol and let stand. Add deionized water to adjust the pH to 7, extract with dichloromethane, evaporate to dryness, combine the crude products, and perform column chromatography separation using petroleum ether-ethyl acetate as eluent to obtain product P1. Product P1 was added to chloroform to obtain solution C. Acetic acid dihydrate was dissolved in ethanol to obtain solution D. Solution D was added dropwise to solution C. The mixture was heated under reflux, cooled, extracted with distilled water, dried, and the purple crystals were collected. The purple crystals were washed with cold methanol to obtain bright purple solid P2. Under a nitrogen protective atmosphere, potassium carbonate was dissolved in N,N-dimethylformamide to obtain solution E. Then, the above-mentioned bright purple solid P2 was also dissolved in N,N-dimethylformamide to obtain solution F. Solution F was added to solution E, heated and stirred to dissolve, and then chloromethylstyrene was added. The reaction was stirred and separated by column chromatography using petroleum ether-ethyl acetate as eluent to obtain zinc porphyrin monomer.
[0008] In one specific feasible implementation, the steps of adding p-carbonylbenzaldehyde, benzaldehyde, and propionic acid, stirring to dissolve them to obtain solution A, preparing solution B with pyrrole and propionic acid, heating solution A while stirring, uniformly adding solution B dropwise into solution A, and continuing to stir and reflux; adding anhydrous ethanol and allowing it to stand; adding deionized water to adjust the pH to 7, extracting with dichloromethane, evaporating to dryness, combining the crude products, and performing column chromatography separation using petroleum ether-ethyl acetate as eluent to obtain product P1 include the following steps: The stirring speed for dissolving is 9000-12000 rpm; The temperature of the heating solution A during stirring is 130-150℃, and the stirring speed is 200-400 rpm; The time for uniformly adding solution B to solution A is 2-4 minutes; The stirring reflux temperature is 130-141℃, the stirring speed is 200-400rpm, and the reflux time is 2-4h; The settling time is 5-8 hours; The extraction is performed 2-3 times; In the petroleum ether-ethyl acetate mixture, the ratio of petroleum ether to ethyl acetate is 10:1.
[0009] In one specific implementation scheme, the steps of adding product P1 to chloroform to obtain solution C, dissolving acetic acid dihydrate in ethanol to obtain solution D, adding solution D dropwise to solution C, heating under reflux, cooling, extracting with distilled water, drying and collecting purple crystals, and washing the purple crystals with cold methanol to obtain bright purple solid P2 include the following steps: The heating reflux temperature is 50-60℃, and the time is 8-15h; The extraction is performed 2-5 times.
[0010] In one specific implementation scheme, under a nitrogen protective atmosphere, potassium carbonate is dissolved in N,N-dimethylformamide to obtain solution E. Then, the aforementioned bright purple solid P2 is similarly dissolved in N,N-dimethylformamide to obtain solution F. Solution F is added to solution E, heated and stirred to dissolve, followed by the addition of chloromethylstyrene, stirring the reaction, and column chromatography separation using petroleum ether-ethyl acetate as eluent to obtain the zinc porphyrin monomer. This includes the following steps: During the heating, stirring, and dissolving process, the heating temperature is 60-70℃, and the stirring rate is 200-400 rpm. The temperature of the stirring reaction is 70-90℃, and the stirring speed is 200-400 rpm; In the petroleum ether-ethyl acetate mixture, the ratio of petroleum ether to ethyl acetate is 20:1.
[0011] This invention also provides a method for preparing fluorescent microspheres, comprising the following steps: An initiator, acrylic acid, and the zinc porphyrin monomer of claim 1 are added to styrene and mixed to form a dispersed phase solution; Add an emulsifier to deionized water, mix, and divide into two portions to serve as a continuous phase solution; Stir one portion of the continuous phase solution, add the dispersible solution dropwise to the continuous phase solution, pre-emulsify, and obtain the pre-emulsion; The pre-emulsion and the remaining continuous phase solution were ultrasonically dispersed to obtain nanosphere droplets; After heating and solidifying the nanosphere droplets, followed by washing and purification, monodisperse fluorescent microspheres were obtained.
[0012] In one specific implementation, the stirring of one portion of the continuous phase solution, the dropwise addition of the dispersible solution to the continuous phase solution, and the pre-emulsification to obtain the pre-emulsion include the following steps: The stirring speed is 9000-12000 rpm; The pre-emulsification time is 3-6 minutes.
[0013] In one specific implementation, the step of ultrasonically dispersing the pre-emulsion and the remaining continuous phase solution to obtain nanosphere droplets includes the following steps: The ultrasonic dispersion frequency is 28-31%; The ultrasonic dispersion time is 3-6 minutes; The flow rate of the ultrasonically dispersed phase solution is 120-480 μL / min; The flow rate of the ultrasonically dispersed continuous phase solution is 950-970 μL / min.
[0014] In one specific implementation, the step of heating and solidifying the nanosphere droplets, washing and purifying them to obtain monodisperse fluorescent microspheres includes the following steps: The heating and curing temperature is 70-90℃, and the heating and curing time is 0.5-2h.
[0015] In one specific implementation, the fluorescent microspheres are made from raw materials comprising the following components, by mass parts: 100 parts styrene, 5-6 parts initiator, 0.0001-0.001 parts zinc porphyrin monomer, 19-20 parts emulsifier and 1-10 parts acrylic acid.
[0016] Compared with the prior art, this application has at least the following advantages: 1. This invention uses zinc porphyrin monomer as a fluorescent dye and prepares carboxylated polystyrene crosslinked fluorescent microspheres by polymerization of styrene, acrylic acid, and zinc porphyrin monomer. The morphology and spectral properties of the microspheres were studied. In this experiment, styrene-based photosensitive groups with polymerizable groups were directly polymerized with styrene and acrylic acid. The prepared carboxylated polystyrene copolymer fluorescent microspheres have a stable and wide spectral range, and the surface of the microspheres has carboxyl functional groups, which facilitates subsequent biological applications. Attached Figure Description
[0017] Various other advantages and benefits will become apparent to those skilled in the art upon reading the following detailed description of preferred embodiments. The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings:
[0018] Figure 1 Here is a SEM image of the fluorescent microspheres prepared in Example 2 of this invention; Figure 2 This is a SEM image of the fluorescent microspheres prepared in Comparative Example 2 of this invention; Figure 3 This is a SEM image of the fluorescent microspheres prepared in Comparative Example 3 of this invention; Figure 4 The fluorescence emission spectra of the fluorescent microspheres prepared in Example 2 and the zinc porphyrin monomer prepared in Example 1 at an excitation wavelength of 420 nm are shown. Figure 5 These are particle size distribution diagrams of fluorescent microspheres prepared at different dispersed phase flow rates. Among them, a is the particle size distribution diagram of Example 2, b is the particle size distribution diagram of Example 9, c is the particle size distribution diagram of Example 10, d is the particle size distribution diagram of Example 11, and e is a particle size histogram at different dispersed phase flow rates. Detailed Implementation
[0020] The technical solution of the present invention will be clearly and completely described below with reference to the accompanying drawings and specific embodiments. However, those skilled in the art will understand that the embodiments described below are some embodiments of the present invention, but not all embodiments, and are only used to illustrate the present invention, and should not be regarded as limiting the scope of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall be followed. Where the manufacturers of reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0021] In the description of this invention, it should be noted that the terms "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing the invention and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the invention. Furthermore, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.
[0022] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installed," "connected," and "connected" should be interpreted broadly. For example, they can refer to fixed connection, detachable connection, or integral connection; they can refer to mechanical connection or electrical connection; they can refer to direct connection or indirect connection through an intermediate medium; and they can refer to the connection within two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.
[0023] To more clearly illustrate the technical solutions in this invention, specific embodiments are described below.
[0024] Example 1 This embodiment provides a zinc porphyrin monomer with a precise molecular weight of 809.2253 and its structural formula is as follows: .
[0025] This embodiment also provides a method for preparing the above-mentioned zinc porphyrin monomer, which includes the following steps: 1. In a three-necked flask equipped with a reflux condenser and a constant pressure funnel, add 1.02 g of p-carbonylbenzaldehyde, 2.4 mL of benzaldehyde and 100 mL of propionic acid, and stir at 10000 rpm to dissolve, to obtain solution A. Dissolve 2.09 mL of pyrrole in 3 mL of propionic acid to obtain solution B. Place solution B in a constant pressure funnel. Heat solution A in the three-necked flask to 140°C. While stirring at 300 rpm, add solution B dropwise into solution A over 3 minutes. Continue stirring and refluxing at 300 rpm for 3 hours at 140°C. After the reaction was completed, 100 mL of anhydrous ethanol was added, and the mixture was allowed to stand at 15 °C for 6 h. Add 200 mL of deionized water, adjust the pH to 7 with sodium bicarbonate, extract three times with dichloromethane, evaporate to dryness, and combine the crude products; Column chromatography was performed with petroleum ether-ethyl acetate (10:1) as the eluent to obtain product P1; 2. Dissolve 63 mg of product P1 obtained in step (1) in 30 mL of chloroform to obtain solution C; Dissolve 66 mg of zinc acetate dihydrate in 3 mL of methanol to obtain a saturated solution, solution D. Solution D was added dropwise to solution C to obtain a reaction mixture. The reaction mixture was heated to 55°C and refluxed for 10 h, then cooled to room temperature and extracted three times with distilled water to obtain an organic layer. The organic layer was dried with anhydrous sodium sulfate and then filtered. Purple crystals were collected and washed with cold methanol to obtain a bright purple solid P2. 3. Add 7.4 mg of potassium carbonate to the flask, purge with nitrogen, dissolve in 10 mL of N,N-dimethylformamide solvent to obtain solution E, then dissolve 18.5 mg of the bright purple solid P2 obtained in step (2) in 10 mL of N,N-dimethylformamide to obtain solution F, inject solution F into solution E in the flask system with a syringe, heat to 60°C, and stir at 300 rpm to dissolve; 4.9 mg of chloromethylstyrene was added and the mixture was stirred at 80 °C. After the reaction was completed, column chromatography was performed with petroleum ether-ethyl acetate (20:1) as the eluent to obtain the product P3-zinc porphyrin monomer.
[0026] Example 2 This embodiment provides a method for preparing fluorescent microspheres, which includes the following steps: 1. Selecting raw materials: Select 0.001 parts of the zinc porphyrin monomer proposed in Example 1, 100 parts of styrene, 5 parts of initiator, 4 parts of acrylic acid and 19 parts of emulsifier, wherein the initiator is selected as azobisisobutyronitrile and the emulsifier is selected as polyvinylpyrrolidone. 2. Preparation of dispersed phase solution: An initiator, acrylic acid, and zinc porphyrin monomer are added to styrene and mixed to form a dispersed phase solution. 3. Preparation of continuous phase solution: Add deionized water to the emulsifier and mix to form a continuous phase solution. Divide the continuous phase solution into two portions. 4. Preparation of pre-emulsion: The dispersed phase solution prepared in step (2) of stirring and descending in a homogenizer at 10000 rpm is added dropwise to one of the continuous phase solutions prepared in step (3), and pre-emulsified for 5 min to obtain a pre-emulsion. 5. Preparation of monodisperse nanosphere droplets: The pre-emulsion obtained in step (4) and the remaining continuous phase solution in step (3) were respectively input into the ultrasonic microfluidic channel through two injection ports. The ultrasonic microfluidic frequency was set to 30% and the time was 5 min. Monodisperse nanosphere droplets were prepared at a flow rate of 120 μL / min for the dispersed phase solution and 960 μL / min for the continuous phase solution. 6. Preparation of fluorescent microspheres: The monodisperse nanosphere droplets obtained in step (5) were heated and solidified at 80°C for 1 hour, and then washed and purified to obtain monodisperse fluorescent microspheres.
[0027] Examples 3-4 The specific implementation method is the same as that in Example 1, with the differences shown in Table 1 below: Table 1 Different preparation conditions Examples 5-6 The specific implementation method is the same as that in Example 2, with the differences shown in Table 2 below: Table 2 Different component mass fractions Examples 7-8 The specific implementation method is the same as that in Example 2, with the differences shown in Table 3 below: Table 3 Different preparation conditions Examples 9-11 The specific implementation method is the same as that in Example 1, with the only difference shown in the following 4: Table 4 Different flow rates of dispersed phase solutions Comparative Example 1 Dissolve 0.1 mg of zinc porphyrin P2 in 1 mL of dichloromethane to obtain a mixed solution with a concentration of 0.1 mg / mL.
[0028] 8 mg of polyvinylpyrrolidone (PVP, molecular weight 40,000) was dissolved in 10 mL of deionized water to obtain a PVP aqueous solution. 10 mg of surface-carboxylated polystyrene-acrylic acid crosslinked microspheres (particle size 200 nm, carboxyl density 200 μmol / g) were dispersed in 10 mL of the PVP aqueous solution to obtain a microsphere suspension.
[0029] Under continuous stirring, the mixed solution was added dropwise to the microsphere suspension. The mass ratio of microspheres to zinc porphyrin P2 was 100:1, and the volume ratio of aqueous phase to organic phase was 10:1. The mixture was stirred at 45℃ for 6 hours. After the reaction was completed, the microspheres were washed sequentially with ethanol and deionized water by centrifugation (12000 rpm, 15 min) until no fluorescent residue was found in the supernatant. The microspheres were then freeze-dried to obtain polymeric fluorescent microspheres encapsulated with photosensitizers.
[0030] Experimental Example 1 The stability of the fluorescent microspheres obtained in Example 2 and Comparative Example 1 was tested. It can be seen that compared with Comparative Example 1, the stability of Example 2 was greatly improved, and the uniformity and batch repeatability of the microsphere system were better.
[0031] Experiment Example 2 First, 0.1 g of polyvinylpyrrolidone (PVP) was weighed using an electronic balance and dissolved in 10 mL of deionized water to form the aqueous phase. 575 μL of styrene monomer and 0.4 mg of zinc porphyrin monomer were mixed to form the oil phase. The oil phase was added dropwise to the aqueous phase under ultrasonic conditions for pre-emulsification, followed by ultrasonic emulsification at 300 W for 10 min. The resulting fine emulsion was then transferred to a flask. Next, 0.03 g of azobisisobutyronitrile (AIBN) was added to the system and stirred for 15 min to ensure complete dissolution. Then, 35 μL of acrylic acid was added and stirred until homogeneous. Nitrogen gas was introduced, and the mixture was heated to 80 °C and reacted for 20 h. After the reaction was complete, the emulsion was broken, centrifuged, and the product was collected. The product was washed six times with deionized water and finally dried to obtain the solid product, which is fluorescent microsphere I.
[0032] The effect of the fluorescent microsphere preparation method on the microsphere particle size was determined in Comparative Example 1 and Example 2. The SEM image of the fluorescent microspheres prepared by mechanically stirred emulsion polymerization in the former is shown below. Figure 2 As shown, from Figure 2It can be seen that fluorescent microspheres prepared by traditional emulsification methods (such as mechanical stirring) have inconsistent sizes and poor dispersibility. The fluorescent microspheres prepared by the "homogenization-microfluidics" combined method provided by this invention have uniform particle size and good dispersibility.
[0033] Experimental Example 3 First, 0.1 g of sodium dodecyl sulfate (SDS) was weighed using an electronic balance and dissolved in 10 mL of deionized water to form the aqueous phase. 575 μL of styrene monomer and 0.004 mg of zinc porphyrin monomer were mixed to form the oil phase. The oil phase was added dropwise to the aqueous phase under ultrasonic conditions for pre-emulsification, followed by ultrasonic emulsification at 300 W for 10 min. The resulting fine emulsion was then transferred to a flask. Subsequently, 0.03 g of potassium persulfate (KPS) was added to the system and stirred for 15 min to ensure complete dissolution. Then, 35 μL of acrylic acid was added and stirred until homogeneous. Nitrogen gas was introduced, and the mixture was heated to 80 °C and reacted for 20 h. After the reaction was complete, the emulsion was broken, centrifuged, and the product was collected. The product was washed six times with deionized water and finally dried to obtain the solid product, which is fluorescent microsphere I.
[0034] The effect of the preparation method of fluorescent microspheres in Comparative Example 2 and Example 2 on the microspheres was determined. The SEM image of the fluorescent microspheres prepared by mechanically stirred emulsion polymerization in the former is shown below. Figure 3 As shown, from Figure 3 It can be seen that fluorescent microspheres prepared by traditional emulsification methods (such as mechanical stirring) have inconsistent sizes and poor dispersibility. The fluorescent microspheres prepared by the "homogenization-microfluidics" combined method provided by this invention have uniform particle size and good dispersibility.
[0035] Experiment Example 4 The fluorescence emission spectra of the fluorescent microspheres prepared in Examples 2 and 9-11 were tested using a fluorescence spectrometer, wherein... Figure 1 As shown, it is a SEM image of the fluorescent microspheres prepared in Example 2. Figure 4 As shown, it is the fluorescence emission spectrum of the fluorescent microspheres prepared in Example 2 and the zinc porphyrin monomer in Example 1 at an excitation wavelength of 420 nm. Figure 1 , Figure 4 As can be seen, the fluorescent microspheres prepared in Example 2 have uniform particle size and smooth surface. Under 420nm ultraviolet light excitation, they exhibit obvious red fluorescence, with emission wavelength peaks at 615nm and 665nm. like Figure 5 As shown in Table 5, the particle size distribution of fluorescent microspheres prepared at different dispersed phase flow rates is as follows: a is the particle size distribution of Example 2, b is the particle size distribution of Example 9, c is the particle size distribution of Example 10, d is the particle size distribution of Example 11, and e is a bar chart of particle size at different dispersed phase flow rates. The table below shows the particle size and polydispersity coefficient of the fluorescent microspheres prepared at different dispersed phase solution flow rates. Table 5. Particle size and polydispersity coefficient of fluorescent microspheres pass Figure 5 As can be seen from the description in Table 5: the average particle size of the fluorescent microspheres prepared in a is 216.2 nm, and the PDI is 0.032; the average particle size in b is 219.2 nm, and the PDI is 0.027; the average particle size in c is 222.6 nm, and the PDI is 0.036; and the average particle size in d is 227.2 nm, and the PDI is 0.047. This indicates that the fluorescent microspheres prepared by the method provided in this invention all have good monodispersity, relatively uniform particle size, and the surface morphology of the microspheres is relatively smooth as observed by high-magnification SEM electron microscopy.
[0036] The above embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit it. This application is not limited to the exact structures described above and illustrated in the accompanying drawings, and it should not be considered that the specific implementation of this application is limited to these descriptions. For those skilled in the art, various changes and modifications made without departing from the concept of this application should be considered to fall within the protection scope of this application.
Claims
1. A zinc porphyrin monomer, characterized in that, It has the following structure: ; The exact molecular weight of the zinc porphyrin monomer is 809.2253.
2. The method for preparing the zinc porphyrin monomer according to claim 1, characterized in that, Includes the following steps: Add p-carbonylbenzaldehyde, benzaldehyde, and propionic acid in a mass ratio of 1:3:4, stir to dissolve, and obtain solution A. Prepare solution B by dissolving pyrrole and propionic acid. Heat solution A, and add solution B dropwise to solution A while stirring. Continue stirring and reflux. Add anhydrous ethanol and let stand. Add deionized water to adjust the pH to 7, extract with dichloromethane, evaporate to dryness, combine the crude products, and perform column chromatography separation using petroleum ether-ethyl acetate as eluent to obtain product P1. Product P1 was added to chloroform to obtain solution C. Acetic acid dihydrate was dissolved in ethanol to obtain solution D. Solution D was added dropwise to solution C. The mixture was heated under reflux, cooled, extracted with distilled water, dried, and the purple crystals were collected. The purple crystals were washed with cold methanol to obtain bright purple solid P2. Under a nitrogen protective atmosphere, potassium carbonate was dissolved in N,N-dimethylformamide to obtain solution E. Then, the above-mentioned bright purple solid P2 was also dissolved in N,N-dimethylformamide to obtain solution F. Solution F was added to solution E, heated and stirred to dissolve, and then chloromethylstyrene was added and stirred to react. Column chromatography was performed with petroleum ether-ethyl acetate as eluent to obtain zinc porphyrin monomer.
3. The preparation method according to claim 2, characterized in that, The steps of adding p-carbonylbenzaldehyde, benzaldehyde, and propionic acid, stirring to dissolve, and obtaining solution A; preparing solution B with pyrrole and propionic acid; heating and stirring solution A; uniformly adding solution B dropwise into solution A; and continuing to stir and reflux; adding anhydrous ethanol and allowing to stand; adding deionized water to adjust the pH to 7; extracting with dichloromethane; evaporating to dryness; combining the crude products; and performing column chromatography separation using petroleum ether-ethyl acetate as eluent to obtain product P1 include the following steps: The stirring speed for dissolving is 9000-12000 rpm; The temperature of the heating solution A during stirring is 130-150℃, and the stirring speed is 200-400 rpm; The time for uniformly adding solution B to solution A is 2-4 minutes; The stirring reflux temperature is 130-141℃, the stirring speed is 200-400rpm, and the reflux time is 2-4h; The settling time is 5-8 hours; The extraction is performed 2-3 times; In the petroleum ether-ethyl acetate mixture, the ratio of petroleum ether to ethyl acetate is 10:
1.
4. The preparation method according to claim 2, characterized in that, The process of adding product P1 to chloroform to obtain solution C, dissolving acetic acid dihydrate in ethanol to obtain solution D, adding solution D dropwise to solution C, heating under reflux, cooling, extracting with distilled water, drying, collecting purple crystals, washing the purple crystals with cold methanol to obtain bright purple solid P2 includes the following steps: The heating reflux temperature is 50-60℃, and the time is 8-15h; The extraction is performed 2-5 times.
5. The preparation method according to claim 2, characterized in that, Under a nitrogen protective atmosphere, potassium carbonate is dissolved in N,N-dimethylformamide to obtain solution E. Then, the bright purple solid P2 is similarly dissolved in N,N-dimethylformamide to obtain solution F. Solution F is added to solution E, heated and stirred to dissolve, followed by the addition of chloromethylstyrene, stirring, and column chromatography separation using petroleum ether-ethyl acetate as eluent to obtain the zinc porphyrin monomer. The process includes the following steps: During the heating, stirring, and dissolving process, the heating temperature is 60-70℃, and the stirring rate is 200-400 rpm. The temperature of the stirring reaction is 70-90℃, and the stirring speed is 200-400 rpm; In the petroleum ether-ethyl acetate mixture, the ratio of petroleum ether to ethyl acetate is 20:
1.
6. A method for preparing fluorescent microspheres, characterized in that, Includes the following steps: An initiator, acrylic acid, and the zinc porphyrin monomer of claim 1 are added to styrene and mixed to form a dispersed phase solution; Add an emulsifier to deionized water, mix, and divide into two portions to serve as a continuous phase solution; Stir one portion of the continuous phase solution, add the dispersible solution dropwise to the continuous phase solution, pre-emulsify, and obtain the pre-emulsion; The pre-emulsion and the remaining continuous phase solution were ultrasonically dispersed to obtain nanosphere droplets; After heating and solidifying the nanosphere droplets, followed by washing and purification, monodisperse fluorescent microspheres were obtained.
7. The preparation method according to claim 6, characterized in that, The process of stirring one portion of the continuous phase solution, adding the dispersible solution dropwise to the continuous phase solution, and pre-emulsifying to obtain the pre-emulsion includes the following steps: The stirring speed is 9000-12000 rpm; The pre-emulsification time is 3-6 minutes.
8. The preparation method according to claim 6, characterized in that, The step of ultrasonically dispersing the pre-emulsion and the remaining continuous phase solution to obtain nanosphere droplets includes the following steps: The ultrasonic dispersion frequency is 28-31%; The ultrasonic dispersion time is 3-6 minutes; The flow rate of the ultrasonically dispersed phase solution is 120-480 μL / min; The flow rate of the ultrasonically dispersed continuous phase solution is 950-970 μL / min.
9. The preparation method according to claim 6, characterized in that, The process of heating and solidifying the nanosphere droplets, followed by washing and purification to obtain monodisperse fluorescent microspheres includes the following steps: The heating and curing temperature is 70-90℃, and the heating and curing time is 0.5-2h.
10. The preparation method according to claim 6, characterized in that, The fluorescent microspheres are made from the following raw materials, in parts by mass: 100 parts styrene, 5-6 parts initiator, 0.0001-0.001 parts zinc porphyrin monomer, 19-20 parts emulsifier and 1-10 parts acrylic acid.