A modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings, its preparation method and application

The functionalized polyacrylamide additive with thiol-containing side chains was prepared under hydrothermal conditions, which solved the problem of poor iron selectivity in red mud magnetic separation tailings, and achieved efficient recovery of iron and improved economic value in red mud tailings.

CN123106956APending Publication Date: 2026-11-17CENT SOUTH UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611454451.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing polyacrylamide flocculants have problems with poor iron selectivity and low recovery rate in the treatment of red mud magnetic separation tailings, and cannot effectively recover iron resources in red mud.

Method used

A functionalized polyacrylamide additive with side chain containing thiol groups was used to prepare modified polyacrylamide under hydrothermal conditions via ammonia exchange reaction. The coordination effect of thiol groups with the surface of iron minerals and the enhanced affinity of nitrogen and oxygen sites of amide groups for iron were utilized to achieve specific capture and separation of iron.

Benefits of technology

It improves the recovery grade and selectivity of iron in red mud tailings, reduces preparation costs, and achieves effective separation of iron in multiple forms and enhances its economic value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106956A_ABST
    Figure CN123106956A_ABST
Patent Text Reader

Abstract

This invention discloses a modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings, its preparation method, and its application. It belongs to the field of acrylamide functionalization modification technology. The structural formula is as follows: The modified polyacrylamide additive provided by this invention for secondary magnetic separation of iron-containing red mud tailings is a functionalized polyacrylamide magnetic separation additive. It is a type of functionalized polyacrylamide polymer with side chains containing thiol groups (-SH). The thiol groups can form stable coordination with iron sites on the surface of iron-containing minerals. The oxygen and nitrogen sites of the amide groups can also assist in coordination, enhancing the specific affinity for the iron phase. Furthermore, it can cause iron-containing substances to aggregate and suspend in the solution for a longer period, which is beneficial for the magnetic field to be fully and uniformly applied during magnetic separation. This effectively improves the iron recovery grade in the secondary iron separation of red mud tailings, laying the foundation for subsequent iron beneficiation work.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polyacrylamide functionalization modification technology, and particularly relates to a modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings, its preparation method and application. Background Technology

[0002] In the Bayer process, alumina in bauxite is dissolved into the liquid phase by concentrated sodium hydroxide solution. Impurities in the ore, such as iron oxide, silica, and titanium dioxide, do not react with the alkali, or react to form insoluble sodium aluminosilicate (sodium silicate slag). These insoluble substances, after separation from the alkali solution, form red mud. Due to the extremely fine particles (micro-fine particle size), red mud has poor settling and filtration properties. Furthermore, the massive global alumina production results in staggering red mud stockpiles, containing 30%–60% Fe₂O₃, equivalent to a large, underutilized iron ore resource pool. Currently, the main treatment strategy for red mud is physical magnetic separation for iron resource recovery. However, due to the fine particle size of the magnetic separation tailings, the iron distribution rate decreases, and the viscosity of the tailings increases. This leads to severe inclusions of iron-bearing minerals with other gangue minerals in the tailings, resulting in a significant amount of iron-bearing material remaining in the tailings. Although the tailings contain a large amount of iron-bearing material, due to their poor recovery grade and low recovery rate, they are typically discarded in the traditional alumina industry. Traditional polyacrylamide has good sedimentation and separation effects as a flocculant in the treatment of tailings. However, all substances agglomerate and settle rapidly, easily encapsulating non-ferrous substances. It has poor selectivity for ferrous substances, which is not conducive to subsequent iron separation and cannot achieve secondary recovery of iron resources.

[0003] For example, Chinese patent CN104724808A discloses a polyacrylamide composite flocculant and its preparation method. This method involves combining an inorganic polymeric flocculant with cationic polyacrylamide, modifying the surface of the inorganic polymeric flocculant with a reactive coupling agent, and grafting inorganic polymeric flocculant molecules onto polyacrylamide molecules through the participation of the coupling agent molecules in the acrylamide polymerization reaction. This enhances the interfacial interaction between the inorganic polymeric flocculant and polyacrylamide molecules, as well as the adsorption, neutralization, and sweeping-and-capture effects on pollutants in wastewater. However, due to its good adsorption and sedimentation effect but lack of specific selectivity, it cannot specifically capture iron-containing substances, thus failing to achieve the goal of secondary iron resource recovery. Summary of the Invention

[0004] To address the shortcomings of existing polyacrylamide flocculants, this invention proposes a modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings, along with its preparation method and application. The modified polyacrylamide additive provided by this invention is a functionalized polyacrylamide magnetic separation additive. It is a type of functionalized polyacrylamide polymer with side chains containing thiol groups (-SH). The thiol groups can form stable coordination with iron sites on the surface of iron-containing minerals, and the oxygen and nitrogen sites of the amide groups can also assist in coordination, enhancing the specific affinity for the iron phase. Furthermore, it can cause iron-containing substances to aggregate and remain suspended in the solution for a longer period, which is beneficial for the magnetic field to be fully and uniformly applied during magnetic separation. This effectively improves the iron recovery grade in the secondary iron separation of red mud tailings, laying the foundation for subsequent iron beneficiation work.

[0005] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings, having the structural formula shown in Formula I: Formula I Where n ranges from 10000 to 14940; R is selected from , , , , , , or R is preferred. .

[0006] This invention relates to a modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings. This modified polyacrylamide, prepared via ammonia exchange reaction, contains thiol groups and is a functionalized polyacrylamide polymer with side chains containing thiol groups (-SH). Its flocculation and iron selectivity advantages are achieved through the synergistic effect of the main polymer backbone, side chain amide groups, and thiol groups. In terms of flocculation and sedimentation, the long-chain backbone can simultaneously adsorb multiple suspended particles, colloids, and iron-containing microparticles through bridging effects, promoting the formation of larger aggregates, accelerating the aggregation of iron-containing substances, and enhancing the sedimentation rate. The side chain amide groups can enhance the adsorption of iron-containing particles through hydrogen bonding and dipole interactions to promote particle destabilization, while the thiol groups can further capture iron-containing microparticles through chemical coordination, achieving specific capture of iron-containing microparticles. Regarding iron selectivity, the thiol groups can form stable coordination with iron sites on the surface of iron-containing minerals, and the oxygen and nitrogen sites of the amide groups can also assist in coordination, enhancing the specific affinity for the iron phase. Furthermore, Al... 3+ Mg 2+ Na + Ca 2+Alkali metals and alkaline earth metals have a weak affinity for thiol groups, which makes the polymer exhibit good selectivity for iron in high hardness and high salt backgrounds. It can also act on both dissolved and particulate iron, achieving effective separation of iron in multiple forms.

[0007] This invention also provides a method for preparing the above-mentioned modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings. The method involves reacting polyacrylamide with a compound having the structural formula R-NH2 under hydrothermal conditions via ammonia exchange to obtain the modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings. The reaction route is as follows: ; Where R is , , , or The range of n is 10000~14940.

[0008] This invention proposes an innovative initiator-free preparation process that utilizes the thermodynamic driving force of the conversion from "small-volume amide" to "large-volume amide" in the ammonia exchange reaction via a hydrothermal method to efficiently modify the R group onto the polyacrylamide backbone, thereby obtaining functionalized modified polyacrylamide. This preparation method not only features a fast reaction rate and simple operation, but also produces a product that can be directly used. Furthermore, it offers significant advantages over previously published high-temperature melting methods in terms of maintaining product molecular weight and controlling crosslinking degree, thus significantly reducing preparation costs.

[0009] The preparation method of the present invention does not require the participation of an initiator, and has the advantages of fast reaction rate, simple operation and direct use of product. It also effectively avoids the generation of irrelevant by-products, and has good effects in maintaining product molecular weight (Z-average molecular weight of 500,000~1,000,000 and polydispersity index of 1.1~1.2) and controlling crosslinking degree, and significantly reduces preparation cost.

[0010] Furthermore, the hydrothermal temperature is 70~90℃ and the time is 11~13h; preferably, the hydrothermal temperature is 80℃ and the time is 12h.

[0011] Furthermore, the molar ratio of the polyacrylamide to the compound with the structural formula R-NH2 is 1:1.

[0012] Furthermore, before the ammonia exchange reaction, the sample is subjected to several cycles of shaking and sonication to ensure uniform mixing and avoid localized violent reactions that could produce unusable byproducts.

[0013] Furthermore, after the ammonia exchange, extraction is performed to remove excess compounds with the structural formula R-NH2.

[0014] The reaction product of this invention requires no further processing; the synthesized product is a functionalized modified polyacrylamide aqueous solution that can be directly used. Compared to the high-temperature melting method, the hydrothermal method has specific advantages in terms of maintaining the molecular weight of the product and controlling the degree of crosslinking.

[0015] The present invention also provides an application of the above-mentioned modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings in the iron / silicon ore separation of solid waste red mud recovery.

[0016] The modified polyacrylamide additive of the present invention can be used as a magnetic separation additive in the secondary magnetic separation process of red mud tailings for iron resource recovery and separation, and has a good selective enrichment effect on iron.

[0017] Compared with the prior art, the present invention has the following advantages and technical effects: 1) The cross-linked functionalized polyacrylamide of the present invention is a type of functionalized polyacrylamide polymer with side chain containing thiol groups (-SH). This compound has a stable linear structure and abundant coordination sites. Therefore, it exhibits good iron capture ability during flocculation and sedimentation. It can significantly increase the flocculation stability and selectivity of iron in synergy with the polyacrylamide host unit. The flocculation speed is moderate, which can avoid the inclusion of non-iron substances during flocculation and reduce the iron selection grade. It exhibits good selectivity for iron and can act on dissolved iron and particulate iron at the same time to achieve effective separation of multiple forms of iron.

[0018] 2) No initiator is involved in the reaction process, which avoids the generation of other by-products. The reaction rate is fast, the operation process is simple, and the product can be used directly. It has good effects in maintaining the molecular weight of the product and controlling the degree of crosslinking, and significantly reduces the preparation cost.

[0019] 3) In terms of product efficacy, the functionalized polyacrylamide of this invention can effectively improve the recovery effect of red mud tailings and give red mud tailings certain economic value. Attached Figure Description

[0020] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 This is a scanning electron microscope (SEM) image of a lyophilized polyacrylamide sample. Figure 2 SEM image of PAM-P1 lyophilized sample; Figure 3 For PAM-P1 lyophilized samples 1 H NMR spectrum; Figure 4 For PAM-P1 lyophilized samples and PAM lyophilized samples1 H NMR comparison spectrum; Figure 5 The graph shows the molecular weight distribution of PAM-P1. The blue line represents the relationship between the fitted molecular weight and the logarithm of the molecular weight (dw / dLogM), and the red line represents the relationship between the fitted molecular weight and the cumulative height. Figure 6 A comparison chart of the settlement performance of PAM, PAM-P1, and PAM-K1; Figure 7 The images show SEM images and EDS analysis of the red mud after settling. (a) and (c) are scanning electron microscope-energy dispersive spectroscopy (SEM) images of the red mud after settling of PAM-L1 and PAM, respectively. (b) and (d) are SEM images of the surface of the red mud after settling of PAM-P1 and PAM, respectively. Detailed Implementation

[0021] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0022] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.

[0023] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.

[0024] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be apparent to those skilled in the art. This specification and embodiments are merely exemplary.

[0025] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.

[0026] Embodiments of the present invention provide a modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings, having the structural formula shown in Formula I: Formula I Where n ranges from 10000 to 14940; R is selected from , , , , , , or R is preferred. .

[0027] The embodiments of the present invention also provide a method for preparing the above-mentioned modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings. The method involves exchanging polyacrylamide with a compound having the structural formula R-NH2 under hydrothermal conditions to obtain the modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings. The reaction route is as follows: ; Where R is , , , or The range of n is 10000~14940.

[0028] In a preferred embodiment of the present invention, the hydrothermal temperature is 70~90°C and the time is 11~13h; preferably, the reaction temperature is 80°C and the time is 12h.

[0029] In a preferred embodiment of the present invention, the molar ratio of polyacrylamide to the compound with the structural formula R-NH2 is 1:1.

[0030] In a preferred embodiment of the present invention, the sample is oscillated and sonicated several times before the ammonia exchange reaction to ensure uniform mixing and avoid localized violent reactions that could produce unusable byproducts.

[0031] In a preferred embodiment of the present invention, after ammonia exchange, extraction is performed to remove excess compounds with the structural formula R-NH2.

[0032] The reaction product of this invention requires no further processing; the synthesized product is a functionalized modified polyacrylamide aqueous solution that can be directly used. Compared to the high-temperature melting method, the hydrothermal method has specific advantages in terms of maintaining the molecular weight of the product and controlling the degree of crosslinking.

[0033] Embodiments of the present invention also provide an application of the modified polyacrylamide additive described above for secondary magnetic separation of iron-containing red mud tailings in the iron / silicon ore separation of solid waste red mud recovery.

[0034] The modified polyacrylamide additive of the present invention can be used as a magnetic separation additive in the secondary magnetic separation process of red mud tailings for iron resource recovery and separation, and has a good selective enrichment effect on iron.

[0035] This invention achieves the specific selection of fine-grained iron minerals by polyacrylamide in the treatment of red mud tailings, and applies it as a magnetic separation additive for the secondary magnetic separation and recovery of iron resources in red mud tailings. It also develops an iron / silicon mineral separation technology based on the selective agglomeration of fine-grained iron minerals, thereby giving red mud tailings economic value.

[0036] Unless otherwise specified, the room temperature in this invention is 25±2℃.

[0037] All raw materials used in the embodiments and comparative examples of this invention were purchased commercially. For example, the polyacrylamide used in the following embodiments and comparative examples of this invention was purchased from Shanghai Bied Pharmaceutical Co., Ltd., catalog number BD01131191, with an average molecular weight of 2,000,000 to 14,000,000.

[0038] It should be noted that any aspects not described in detail in this invention are conventional practices in the field and are not the focus of this invention.

[0039] The technical solution of the present invention will be further illustrated by the following embodiments.

[0040] Example 1 A method for preparing a modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings, comprising the following steps: Add 10 mL of water, 0.05 g of polyacrylamide (0.7 mmol, molar amount based on monomer content), and 0.055 g of 2-mercaptoethylamine (0.7 mmol, molar amount based on monomer content) to a 15 mL reactor liner. After repeated shaking and ultrasonic cycles to ensure homogeneous mixing and avoid vigorous localized reactions that could generate byproducts, place the reactor liner in a steel reactor and place it in an oven at a pre-set temperature (80°C) for 12 hours. After the reaction time, cool the reactor to room temperature to obtain a directly usable functionalized modified polyacrylamide aqueous solution (i.e., a modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings), denoted as PAM-P1. The structural formula of its active ingredient is as follows: .

[0041] Example 2 A method for preparing a modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings, comprising the following steps: Water (10 mL), polyacrylamide (0.1 g, 1.4 mmol), and 2-mercaptoethylamine (0.11 g, 1.4 mmol) were added to a 15 mL reaction vessel liner. The mixture was repeatedly oscillated and sonicated to ensure homogeneous mixing and prevent vigorous localized reactions that could generate byproducts. The liner was then placed in a steel reaction vessel and placed in an oven pre-set at 80°C for 12 hours. After the reaction time, the reaction vessel was cooled to room temperature to obtain a directly usable functionalized modified polyacrylamide aqueous solution, denoted as PAM-P2. The structural formula of its active ingredient is as follows: .

[0042] Example 3 A method for preparing a modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings, comprising the following steps: Water (10 mL), polyacrylamide (0.5 g, 7 mmol), and 2-mercaptoethylamine (0.55 g, 7 mmol) were added to a 15 mL reaction vessel liner. The mixture was repeatedly shaken and sonicated to ensure homogeneous mixing and prevent vigorous localized reactions that could generate byproducts. The reaction vessel liner was then placed in a steel reaction vessel and placed in an oven at a pre-set temperature (80 °C) for 12 hours. After the reaction time, the reaction vessel was cooled to room temperature to obtain a directly usable functionalized modified polyacrylamide aqueous solution, denoted as PAM-P3. The structural formula of its active ingredient is as follows: .

[0043] The raw material usage for Examples 1-3 is shown in Table 1.

[0044] Table 1 Comparative Example 1 Water (10 mL), polyacrylamide (0.05 g, 0.7 mmol), and 2-aminomethylpyridine (0.076 g, 0.7 mmol) were added to a 15 mL reaction vessel liner. After repeated shaking and ultrasonic circulation to ensure homogeneous mixing and avoid vigorous localized reactions that could generate byproducts, the reaction vessel liner was placed in a steel reaction vessel and then placed in an oven at a pre-set temperature (80 °C) for 12 hours. After the reaction time was up, the reaction vessel was removed and cooled to room temperature to obtain a functionalized polyacrylamide aqueous solution, denoted as PAM-K1. The structural formula of its active ingredient is as follows: .

[0045] The surface morphology of the polymer was characterized using a field emission scanning electron microscope (FESEM) from JEOL Ltd., Japan. The results are shown in the figure. Figure 1 and Figure 2 ,in Figure 1 This is a scanning electron microscope image of a lyophilized polyacrylamide sample. Figure 2 The scanning electron microscope (SEM) images of the PAM-P1 lyophilized sample show that the polyacrylamide sample has a continuous and uniform film morphology with no obvious doping or defects on the surface. While the PAM-P1 sample also exhibits a film-like morphology, it contains numerous porous defects, and the film surface is relatively rough, uniformly coated with a small number of particles. Comparison of the two SEM images reveals that the macroscopic morphology of the product changes after the hydrothermal functionalization modification reaction of the polyacrylamide raw material. This also macroscopically demonstrates the successful execution of the ammonia exchange reaction in this invention.

[0046] To further verify the feasibility of the synthesis method of this invention and to determine the extent of 2-mercaptoethylamine introduction, this invention uses an AVANCE III 400MHz fully digital superconducting nuclear magnetic resonance spectrometer from Bruker, Switzerland, to analyze the PAM-P1 lyophilized sample and polyacrylamide. 1 1H NMR analysis. PAM-P1 lyophilized sample. 1 H NMR spectrum as shown Figure 3 As shown, the PAM-P1 chemical shift value (δ) exhibits a distinct chemical signal peak in the range of 2–4, which is a characteristic signal peak of the hydrogen atoms on the carbon chain of 2-mercaptoethylamine and the hydrogen atoms bonded to S. Furthermore, due to… Figure 4 The NMR comparison image shows that PAM-P1 still retains the structural framework of polyacrylamide, and the peak in the δ range of 5.5~6.0 of the PAM-P1 sample disappears. The peak in this range is the characteristic signal peak of the hydrogen atom connected to N in the amide before modification. This is because the amide is changed to imide after modification, and the chemical shift value of the hydrogen atom connected to N shifts to a higher field.

[0047] The molecular weight distribution of PAM-P1 was determined using Cirrus GPC gel permeation chromatography, and the results are as follows: Figure 5 As shown in the figure. The results indicate that the Z-average molecular weight of PAM-P1 is 657,690 g / mol, the Z+1 average molecular weight is 714,902 g / mol, and the polydispersity index is 1.15324. This demonstrates that the flocculant prepared by the hydrothermal method maintains a high molecular weight even without removing the additive monomers and solution, further validating the feasibility of this synthesis method.

[0048] Application Examples The sedimentation performance of PAM-P1 prepared in Example 1 of this invention, PAM-K1 prepared in Comparative Example 1, and flocculants prepared from unmodified polyacrylamide (PAM) were tested.

[0049] The settling performance experiment used tailings from the red mud vertical ring magnetic separation process as the research object (hereinafter referred to as "vertical ring sample," mineral types and contents are shown in Table 4). The samples were collected from the Guangxi Branch of China Aluminum Corporation (located in Pingguo City, Guangxi, China). After collection, the samples underwent pretreatment: a Buchner funnel with a vacuum pump was used for solid-liquid separation to remove free water from the tailings; subsequently, the separated solid samples were placed in a constant-temperature oven and dried to constant weight at 80℃. This operation completely eliminated the interference of moisture on the subsequent solution concentration, ensuring consistent experimental standards. The dried samples were sealed and stored in a desiccator for later use to avoid moisture absorption affecting experimental accuracy.

[0050] In the experimental solution preparation stage, the dried sample of the liposome was accurately weighed using a 0.1 g electronic balance, and tailings suspensions with a solid content of 200 g / L were prepared in 500 mL volumetric flasks. During preparation, a small amount of deionized water was first added to moisten the sample, then the mixture was continuously stirred with a magnetic stirrer for 30 minutes to ensure complete dispersion of solid particles and no obvious agglomeration. Finally, the volume was adjusted to the mark and shaken well, and the mixture was allowed to stand for 5 minutes before use.

[0051] The flocculation and sedimentation experiment was conducted strictly according to the single variable principle: 250 mL of the vertical ring suspension was transferred into three identical 250 mL graduated sedimentation tubes (three vertical ring samples, corresponding to three flocculants). Then, 2.5 mL of PAM-P1, PAM-K1, and PAM flocculant solutions were slowly added dropwise to each sedimentation tube in sequence.

[0052] Solution mixing was performed using a self-made stainless steel mesh stirrer. The stirrer was held and pulled up and down at a constant speed 5-8 times, with the lifting height controlled 2-3 cm above the liquid surface. This ensured thorough mixing of the flocculant and tailings suspension while avoiding excessive air bubbles that could interfere with interface observation. The stopwatch was started the instant stirring ended, and the corresponding scale value at the solid-liquid interface was read and recorded.

[0053] Settlement results as follows Figure 5 As shown, among the three flocculants, PAM-P1 exhibits a sedimentation effect similar to that of the unmodified PAM flocculant. Its moderate sedimentation performance allows iron-containing substances to agglomerate and remain suspended in the solution for a relatively long time, which is beneficial for the uniform and sufficient application of the magnetic field during magnetic separation and subsequent iron separation. PAM-K1 flocculant, however, has an excessively good sedimentation effect, causing all substances to rapidly agglomerate and settle to the bottom of the measuring cylinder, which is detrimental to subsequent iron separation.

[0054] The secondary magnetic separation performance of PAM-P1 prepared in Example 1 of the present invention, PAM-K1 prepared in Comparative Example 1, and flocculants prepared by unmodified polyacrylamide (PAM) were tested.

[0055] The secondary magnetic separation performance experiment used vertical ring samples as the research object. The samples required pretreatment: a Buchner funnel with a vacuum pump was used for solid-liquid separation by filtration to remove free water from the tailings; subsequently, the separated solid samples were placed in a constant-temperature oven and dried to constant weight at 80℃. This operation completely eliminated the interference of moisture on the subsequent solution concentration, ensuring consistent experimental standards. The dried samples were then sealed and stored in a desiccator for later use to prevent moisture absorption from affecting experimental accuracy.

[0056] In the experimental solution preparation stage, the dried sample of the liposome was accurately weighed using a 0.1 g electronic balance, and tailings suspensions with a solid content of 200 g / L were prepared in 500 mL volumetric flasks. During preparation, a small amount of deionized water was first added to moisten the sample, then the mixture was continuously stirred with a magnetic stirrer for 30 minutes to ensure complete dispersion of solid particles and no obvious agglomeration. Finally, the volume was adjusted to the mark and shaken well, and the mixture was allowed to stand for 5 minutes before use.

[0057] The secondary magnetic separation performance test strictly followed the single variable principle: 250 mL of the vertical ring suspension was transferred into three identical 500 mL beakers (three vertical ring samples, corresponding to three flocculants). Then, 2.5 mL of PAM-P1, PAM-K1, and PAM flocculant solutions were slowly added dropwise to each settling tube in sequence.

[0058] The solution was mixed using a self-made stainless steel mesh stirrer. The stirrer was held and pulled up and down at a constant speed 5 to 8 times, with the height of the pull controlled 2 to 3 cm above the liquid surface, to ensure that the flocculant and tailings suspension were fully mixed.

[0059] Magnetic separation of the vertical ring samples was performed using a magnetic rod (magnetic field strength of 10000 Gauss) with the three types of flocculants (PAM-P1, PAM-K1, and PAM). The magnetic concentrate and tailings obtained from the magnetic separation were separated by solid-liquid separation via filtration and dried to constant weight, and the weights were recorded. Elemental content (oxide form) of the samples was tested using XRF. The test results (Tables 2-4) show that PAM-P1 has a significant selective effect on iron-containing substances in the samples (XRF data show that the iron content in the concentrate increased after magnetic separation, while the iron content in the tailings decreased, proving its selectivity for iron). The Fe content in its magnetic concentrate was significantly higher than that of the vertical ring samples, and the iron recovery rate of PAM-P1 reached 65%. In contrast, PAM-K1 and PAM showed no significant selectivity, and the Fe content in the tailings was significantly reduced. Therefore, the polyacrylamide flocculants prepared using the functionalization modification strategy have a good recovery effect on the red mud tailings of the Pingguo bauxite mine in Guangxi.

[0060] Table 2 XRF test of iron concentrate content in vertical ring samples Table 3. XRF test of iron tailings content in vertical ring samples. Table 4. XRF test of cyclohexane content in samples. This invention analyzes the morphology of red mud after sedimentation using a field emission scanning electron microscope (FESEM) from Japan Electron Microscopy Co., Ltd. (JEOL). Figure 7 As shown, the red mud morphology described above mostly presents as irregular blocky particles. After PAM-P1 sedimentation, the Fe / Si mass fraction ratio is around 3 / 1, while after PAM sedimentation, the Fe / Si mass fraction ratio is less than 2 / 1. Careful observation of the EDS images clearly shows that the Fe element in the red mud obtained from PAM-P1 sedimentation exhibits a certain degree of aggregation, while the Fe / Si element in the red mud obtained from PAM sedimentation is more uniformly dispersed, with no aggregation of Fe element. Therefore, it can be seen that the polyacrylamide-based iron beneficiation additive prepared using the thiohydroxyl functionalization modification strategy has a good iron beneficiation effect on the red mud tailings of the Pingguo bauxite mine.

[0061] The above are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.

Claims

1. A modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings, characterized in that, It has the structural formula shown in Equation I: Formula I Where n ranges from 10000 to 14940; R is selected from , , , , , , or .

2. The modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings according to claim 1, characterized in that, R is .

3. A method for preparing a modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings as described in any one of claims 1 to 2, characterized in that, Polyacrylamide was subjected to ammonia exchange with a compound with the structural formula R-NH2 under hydrothermal conditions to obtain the modified polyacrylamide additive used for secondary magnetic separation of iron-containing red mud tailings. Where R is , , , or .

4. The method for preparing the modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings according to claim 3, characterized in that, The hydrothermal temperature is 70~90℃, and the time is 11~13h.

5. The method for preparing the modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings according to claim 3, characterized in that, The molar ratio of the polyacrylamide to the compound with the structural formula R-NH2 is 1:

1.

6. The method for preparing the modified polyacrylamide additive for secondary magnetic separation of iron-containing red mud tailings according to claim 3, characterized in that, Before the ammonia exchange reaction, the sample is mixed evenly by shaking and ultrasonic circulation.

7. The application of a modified polyacrylamide additive as described in any one of claims 1 to 2 for secondary magnetic separation of iron-containing red mud tailings in the iron / silicon ore separation of solid waste red mud recovery.

Citation Information

Patent Citations

  • Polyacrylamide composite flocculant and preparation method thereof

    CN104724808A