Random copolymers containing dihydroacrylidine phosphonate and their preparation methods; perovskite solar cells

By using a random copolymer containing dihydroacrylamide phosphonate as an interface modification material in perovskite solar cells, the problems of film uniformity and weak interfacial bonding of self-assembled monolayer materials were solved, achieving efficient photoelectric conversion and improved stability.

CN123107047APending Publication Date: 2026-11-17JIUYAO OPTOELECTRONICS
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611625203.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing perovskite solar cells, the self-assembled monolayer materials have poor film uniformity, weak interfacial bonding, and are prone to diffusion and desorption, leading to an increase in interfacial defects and affecting device stability and efficiency.

Method used

A random copolymer containing dihydroacrylidine phosphonate is used as an interface modification material. Through the synergistic anchoring effect of multiple phosphonic acid side groups on the polymer chain, a uniform and dense interface modification layer is formed. The ratio of structural units is adjusted to achieve step-level matching with the perovskite layer and reduce the hole injection barrier.

Benefits of technology

It improves the photoelectric conversion efficiency and operational stability of perovskite solar cells, overcomes the problems of poor film uniformity and weak interfacial bonding of traditional small molecule self-assembled monolayer materials, and has good prospects for industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107047A_ABST
    Figure CN123107047A_ABST
Patent Text Reader

Abstract

This invention discloses a random copolymer containing dihydroacrylidine phosphonate, its preparation method, and a perovskite solar cell. Addressing the technical deficiency of insufficient solubility in homopolymers containing dihydroacrylidine phosphonate, alkoxybenzene copolymer units are introduced for random copolymerization, enabling the resulting copolymer to be completely soluble in solvents and meeting spin-coating requirements. Utilizing the synergistic anchoring effect of multiple phosphonic acid side groups on the polymer chain, a uniform, dense, and stable interface modification layer is formed, overcoming the defects of traditional small-molecule self-assembled monolayer materials such as poor film uniformity, weak interfacial bonding, and easy diffusion desorption. By adjusting the copolymerization ratio of structural units, the energy level characteristics of the material are controlled, achieving step-level matching with the perovskite layer, reducing the hole injection barrier, and suppressing interfacial nonradiative recombination. Applying this copolymer as an interface modification layer in perovskite solar cells can significantly improve photoelectric conversion efficiency and operational stability, showing promising prospects for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of solar cells, and more specifically, relates to a random copolymer containing dihydroacrylidine phosphonate and its preparation method, and a perovskite solar cell. Background Technology

[0002] Inverted perovskite solar cells have attracted much attention due to their advantages such as low-temperature processing and ease of fabrication of tandem devices. In the selection of the hole transport layer, PEDOT:PSS is widely used due to its good film formation and solution processability. However, the acidic nature and hygroscopicity of PEDOT:PSS can induce unfavorable reactions at the perovskite interface, especially in tin-based or tin-lead mixed perovskite systems, where the acidic environment on the surface accelerates Sn... 2+ Oxidation severely damages the stability and efficiency of devices.

[0003] In recent years, self-assembled monolayer (SAM) materials, especially small molecules based on phosphonic carbazole, have become important interface modification materials in perovskite solar cells due to their tunable energy levels and good solution processability. For example, patent document CN118870943A discloses a method for preparing perovskite solar cells, in which the self-assembled monolayer materials include various carbazole / acriminyl phosphonic acid compounds such as [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid, [4-(9H-carbazole-9-yl)butyl]phosphonic acid, and (4-(2,7-dibromo-9,9-dimethylacrimin-10(9H)-yl)butyl)phosphonic acid. These small molecules can be anchored to metal oxides (such as NiO) through phosphonic acid groups. x Small molecule SAMs (SAMs) are applied to ITO (IonO) or PEDOT:PSS surfaces to optimize interfacial contact and promote hole extraction. However, these small molecule SAMs have significant drawbacks in practical applications. First, they exhibit poor film uniformity. During solution processing, small molecule phosphonic carbazole easily aggregates, forming uneven multilayer or island structures, increasing the resistance to hole extraction and leading to more interfacial defects. Second, they suffer from insufficient interfacial stability. The adhesion between small molecule SAMs and the substrate is weak, especially on rough, acidic surfaces like PEDOT:PSS, where the anchoring force is limited. During subsequent spin-coating of perovskite precursor solutions, the SAM layer is easily washed away, failing to effectively cover the interface and causing localized leakage. Furthermore, they are prone to diffusion and desorption. Under photothermal aging conditions, small molecule phosphonic carbazole easily desorbs from the substrate surface and diffuses into the perovskite active layer, triggering interfacial failure and further accelerating perovskite decomposition and device performance degradation.

[0004] To address the stability issues of small-molecule SAMs, researchers have attempted to develop polymeric phosphonate-carbazole materials. For example, patent document CN119504858A discloses the application of carbazole phosphate materials as self-assembled hole transport monolayers; furthermore, patent document CN111509128A provides a perovskite solar cell based on a composite hole transport layer, wherein the hole transport layer includes a PEDOT:PSS layer and a hole modification layer disposed thereon. This modification layer is prepared from amphiphilic molecules, which can improve interfacial energy level matching and suppress interfacial defects. However, existing polymeric phosphonate materials generally suffer from poor solubility and poor wettability in perovskite precursor solutions, resulting in a significant reduction in interfacial modification effects and hole transport efficiency, making it difficult to meet the requirements of high-performance devices. Summary of the Invention

[0005] To address the aforementioned deficiencies or improvement needs of existing technologies, this invention provides a random copolymer containing dihydroacrylidine phosphonate, its preparation method, and a perovskite solar cell. Addressing the technical deficiency of insufficient solubility in homopolymers containing dihydroacrylidine phosphonate, alkoxybenzene copolymer units are introduced for random copolymerization, enabling the resulting copolymer to be completely soluble in solvents and meeting spin-coating requirements. Utilizing the synergistic anchoring effect of multiple phosphonic acid side groups on the polymer chain, a uniform, dense, and stable interface modification layer is formed, overcoming the defects of traditional small-molecule self-assembled monolayer materials such as poor film uniformity, weak interfacial bonding, and easy diffusion desorption. By adjusting the copolymerization ratio of structural units, the energy level characteristics of the material are controlled, achieving step-level matching with the perovskite layer, reducing the hole injection barrier, and suppressing interfacial nonradiative recombination. Applying this copolymer as an interface modification layer in perovskite solar cells can significantly improve photoelectric conversion efficiency and operational stability, demonstrating promising prospects for industrial application.

[0006] To achieve the above objectives, according to one aspect of the present invention, a random copolymer containing dihydroacrylamide phosphonate is provided, wherein the random copolymer containing dihydroacrylamide phosphonate contains structural unit A and structural unit B, wherein structural unit A and structural unit B are randomly distributed in the copolymer backbone, wherein structural unit A has the structure shown in Formula I, and structural unit B has the structure shown in Formula II or Formula III; Equation I: or ; Formula II: ; Formula III: ; The side chain lengths m, n, and x in the structures of Formula I, Formula II, or Formula III are 2 to 30, and the degrees of polymerization M, N, and X are 2 to 40. The random copolymer containing phosphonic acid dihydroacridine has a number-average molecular weight Mn of 5000 Da to 11000 Da and a weight-average molecular weight Mw of 8000 Da to 16000 Da. The molar ratio of structural unit A to structural unit B is 1:20 to 20:1.

[0007] Preferably, the random copolymer containing phosphonic acid dihydroacridine comprises one of the following structural formulas: .

[0008] According to a second aspect of the present invention, a hole transport layer is provided, the hole transport layer comprising a hole transport base layer and an interface modification layer disposed on the hole transport base layer; the interface modification layer comprising the random copolymer containing dihydroacrylamide phosphonate.

[0009] According to a third aspect of the present invention, a perovskite solar cell is provided, the perovskite solar cell comprising the hole transport layer.

[0010] According to a fourth aspect of the present invention, a method for preparing a random copolymer containing dihydroacrylamide phosphonate is provided, comprising the following steps: Step 1: 2,7-dihalo-9,9-dialkyl-9,10-dihydroacridine is reacted with a dihaloalkane under basic conditions to undergo an N-alkylation reaction to obtain a haloalkylated dihydroacridine intermediate. Step 2: The haloalkylated dihydroacridine intermediate is reacted with triethyl phosphite in an Arbuzov reaction to obtain compound I; Step 3: Compound I and the comonomer are subjected to a Yamamoto coupling reaction to obtain a random copolymer containing dihydroacrylidine phosphonate; the comonomer is selected from compound II or compound III; Step four: The random copolymer containing phosphonate dihydroacridine is reacted with a halosilane and then subjected to alcoholysis to obtain the random copolymer containing phosphonate dihydroacridine. Wherein, compound I, after being coupled with Yamamoto, forms structural unit A in the random copolymer containing dihydroacridine phosphonate, and compound II or compound III, after being coupled with Yamamoto, forms structural unit B in the random copolymer containing dihydroacridine phosphonate.

[0011] Preferably, the structural formula of compound I is: or , The structural formula of compound II is: , The structural formula of compound III is: .

[0012] Preferably, R1, R1', R2, R2', R3, and R3' in the structures of compounds I, II, and III are each independently selected from Br.

[0013] In summary, compared with the prior art, the above-described technical solutions conceived by this invention can achieve the following beneficial effects: 1. This invention proposes a design strategy for random copolymers containing phosphonic acid dihydroacridine units as polymeric self-assembled interface modification materials, solving the fundamental defects of traditional small-molecule SAM materials at the molecular level, such as poor film uniformity, weak interfacial bonding, and easy diffusion and desorption. Existing small-molecule phosphonic acid carbazole-based SAM materials have limited bonding strength and are difficult to form a uniform coverage on rough, acidic PEDOT:PSS surfaces. This invention covalently links the phosphonic acid dihydroacridine units to the polymer backbone, achieving multi-point, high-strength bonding to the substrate surface through the synergistic anchoring effect of multiple phosphonic acid side groups on the molecular chain. At the same time, the inter-chain entanglement and cross-linking between polymer chains endow the interface modification layer with excellent erosion resistance and structural integrity, overcoming the inherent limitations of insufficient stability of small-molecule SAMs from the material's origin.

[0014] 2. This invention achieves synergistic optimization of material solubility, film-forming properties, energy level characteristics, and hole transport capability through a random copolymerization strategy of structural unit A and structural unit B. This overcomes the technical bottlenecks of poor solubility and inadequate wettability of existing polymeric phosphonic acid materials in perovskite precursor solutions. Structural unit A contains a dihydroacrylidine core, endowing the material with excellent hole transport capability and tunable energy level characteristics, ensuring efficient hole extraction and transport at the interface. Structural unit B introduces flexible alkoxybenzene or alkylthiophene side chains, effectively improving the polymer's solution processability and wettability in perovskite precursor solutions. The random distribution of the two structural units in the polymer backbone ensures uniform dispersion of functional groups, avoiding the phase separation problems that may exist in block copolymers. This allows the material to maintain excellent charge transport performance while also possessing excellent solubility and film-forming quality.

[0015] 3. The interface modification strategy of this invention is highly compatible with the existing PEDOT:PSS hole transport base layer system. It achieves a comprehensive improvement in device performance without altering the main device structure or introducing complex processes, demonstrating promising prospects for industrial application. The polymeric phosphonate dihydroacrylidine interface modification layer proposed in this invention can be directly applied to the PEDOT:PSS surface via a simple and mild solution spin-coating method. Without changing the existing device fabrication process and conditions, it effectively passivates the PEDOT:PSS surface and optimizes energy levels, significantly improving the device's photoelectric conversion efficiency and operational stability. This technical solution features a simple process flow, readily available raw materials, and requires no expensive equipment investment. It is highly compatible with current mainstream perovskite solar cell fabrication processes, exhibiting excellent potential for large-scale application and feasibility for technology transfer. Attached Figure Description

[0016] Figure 1 Comparative photographs of the solubility properties of different materials; Figure 2 The 1H NMR spectrum of compound I obtained in step two of Example 1 of this invention; Figure 3 These are SEM images of the perovskite film surfaces obtained in Example 6 and Comparative Example 4 of the present invention. Figure 4 The X-ray diffraction (XRD) patterns of the perovskite thin films prepared in Example 6 and Comparative Example 4 of this invention are shown below. Figure 5 The images show the ultraviolet photoelectron spectroscopy (UPS) spectra of tin-lead perovskite and PEDOT:PSS, the cyclic voltammetry (CV) curves of the polymer self-assembled monolayer (Poly-SAM) prepared in Example 6 of this invention, and a schematic diagram of the energy level structure. Figure 6 The graphs show the TRPL (time-resolved fluorescence spectroscopy) decay curves of the perovskite thin films prepared in Example 6 and Comparative Example 4 of this invention. Figure 7 The JV test curves are shown for the tin-lead hybrid perovskite solar cells prepared in Example 6 and Comparative Example 4 of this invention. Detailed Implementation

[0017] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. Furthermore, the technical features involved in the various embodiments of this invention described below can be combined with each other as long as they do not conflict with each other.

[0018] The present invention provides a random copolymer containing dihydroacrylamide phosphonate, wherein the random copolymer containing dihydroacrylamide phosphonate contains structural unit A and structural unit B, wherein structural unit A has the structure shown in Formula I, and structural unit B has the structure shown in Formula II or Formula III; Equation I: or ; Formula II: ; Formula III: ;

[0019] The side chain lengths m, n, and x in the structures of Formula 1, Formula II, or Formula III are 2 to 30, and the degrees of polymerization M, N, and X are 2 to 40.

[0020] The random copolymer has a number-average molecular weight Mn of 5000 Da to 11000 Da and a weight-average molecular weight Mw of 8000 Da to 16000 Da. The molar ratio of structural unit A to structural unit B is 1:20 to 20:1.

[0021] The random copolymer containing phosphonic acid dihydroacridine includes one of the following structural formulas: .

[0022] The method for preparing the random copolymer containing dihydroacrylamide phosphonate includes the following steps: Step 1: 2,7-dihalo-9,9-dialkyl-9,10-dihydroacridine is reacted with a dihaloalkane under basic conditions to undergo an N-alkylation reaction to obtain a haloalkylated dihydroacridine intermediate. Step 2: The haloalkylated dihydroacridine intermediate is reacted with triethyl phosphite in an Arbuzov reaction to obtain compound I; Step 3: Compound I and the comonomer are subjected to a Yamamoto coupling reaction to obtain a random copolymer containing dihydroacrylidine phosphonate; the comonomer is selected from compound II or compound III; Step four: The random copolymer containing phosphonate dihydroacridine is reacted with a halosilane and then subjected to alcoholysis to obtain the random copolymer containing phosphonate dihydroacridine. Wherein, compound I, after being coupled with Yamamoto, forms structural unit A in the random copolymer containing dihydroacridine phosphonate, and compound II or compound III, after being coupled with Yamamoto, forms structural unit B in the random copolymer containing dihydroacridine phosphonate.

[0023] The structural formula of compound I is: or ; The structural formula of compound II is: , The structural formula of compound III is: .

[0024] In the structures of compounds I, II, and III, R1, R1', R2, R2', R3, and R3' are each independently selected from Br.

[0025] The present invention also provides a hole transport layer and a perovskite solar cell comprising the hole transport layer, wherein the hole transport layer comprises a hole transport base layer and an interface modification layer disposed on the hole transport base layer; the interface modification layer comprises the random copolymer containing dihydroacrylamide phosphonate. The hole transport base layer is a PEDOT:PSS layer.

[0026] It should be noted that the random copolymerization strategy of structural unit A and structural unit B in this invention is designed to address the inherent defects of phosphonic acid dihydroacrylidine homopolymers, namely insufficient solubility and lack of solution processing feasibility. If the phosphonic acid dihydroacrylidine monomer is directly homopolymerized, the resulting homopolymer backbone has a highly conjugated rigid structure with strong π-π stacking interactions between the backbones. At the same time, the phosphonic acid groups on the side chains can form a dense network of intermolecular hydrogen bonds. Under this dual association, the homopolymer has extremely low solubility in polar solvents commonly used in perovskite devices, such as DMSO and DMF, making it impossible to prepare a clear solution that meets the requirements of spin coating and thus lacking device fabrication feasibility. This invention introduces alkoxybenzene structural units (structural unit B) into the polymer backbone for random copolymerization. By disrupting the conjugated regularity of the backbone to weaken π-π stacking, and by using flexible alkoxy side chains to enhance the affinity of the polymer chain for polar solvents and partially shield the hydrogen bonding between phosphonic acid groups, the material achieves good solubility and solution processability while retaining the core optoelectronic functions of dihydroacrylidine units such as hole transport, interface passivation, and energy level matching. This meets the spin-coating requirements for interface modification of perovskite devices.

[0027] Based on the above design concept, this invention systematically investigated the solubility of the obtained copolymer after its preparation and before its application in perovskite solar cells, such as... Figure 1 As shown.

[0028] like Figure 1 As shown in (a), the solubility of conventionally used polymeric hole transport materials (poly-4PACz on the left and Poly-2PACz on the right) was tested. When added to DMSO, a commonly used polar solvent for device fabrication, at a concentration of 2 mg / mL, it was found to be difficult to dissolve completely, making it impossible to prepare a clear solution suitable for spin-coating. Subsequently, the solubility of the phosphonic acid dihydroacridine random copolymer obtained in Example 1 of this invention was tested at a concentration of 3 mg / mL. Figure 1 As shown in (b), the copolymer can be completely dissolved in DMSO to form a clear and transparent solution, meeting the requirements for spin coating (its solubility concentration is higher than that of poly-4PACz, yet it still dissolves completely). Based on this, the effect of the copolymerization ratio of structural units A and B on the solubility performance was further investigated, as shown in (b). Figure 1As shown in (c), when the A / B ratio exceeds the 1:20~20:1 range specified in this invention (e.g., if the A ratio is too low, A:B=1:30), the resulting copolymer is difficult to form a stable solution in DMSO due to excessive alkoxybenzene units and overly flexible molecular chains. The above results indicate that the phosphonic acid dihydroacrylidine random copolymer described in this invention has excellent solubility in DMSO, and the copolymerization ratio of structural units A and B must be maintained within an appropriate range to balance solution processability and film quality. Subsequently, the random copolymer that passed the solubility screening was applied to the preparation of the interface modification layer for perovskite solar cells, and the photoelectric performance of the device was systematically tested.

[0029] In this invention, DMF represents N,N-dimethylformamide, DMSO represents dimethyl sulfoxide, and Poly-SAM represents a polymer self-assembled monolayer interface modification layer formed by a random copolymer containing dihydroacrylamide phosphonate. The degrees of polymerization M, N, and X are calculated based on the measured number-average molecular weight and the theoretical molecular weight of the corresponding repeating unit. The following detailed description is provided in conjunction with specific embodiments.

[0030] Example 1 Step 1: Synthesis of 2,7-dibromo-9,9-dimethyl-10-(4-bromobutyl)-9,10-dihydroacridine Under nitrogen protection, potassium carbonate (2.0 eq) and tetrabutylammonium bromide (0.2 eq) were added to 20 mL of 1,4-dibromobutane as a base, along with 2,7-dibromo-9,9-dimethyl-10-(4-bromobutyl)-9,10-dihydroacridine. The mixture was then stirred at 60 °C for 12 hours. After the reaction was complete, the mixture was cooled to room temperature, concentrated under reduced pressure, filtered, and purified by column chromatography to obtain 2,7-dibromo-9,9-dimethyl-10-(4-bromobutyl)-9,10-dihydroacridine. The structural formula of 2,7-dibromo-9,9-dimethyl-10-(4-bromobutyl)-9,10-dihydroacridine is shown below:

[0031] Step 2: Synthesis of diethyl phosphonate (4-(2,7-dibromo-9,9-dimethyl-9,10-dihydroacrylin-10-yl)butyl)phosphonate Based on the product from step one (1.0 eq), it was dissolved in 10 mL of triethyl phosphite and reacted with stirring at 140 °C for 12 hours. After the reaction, triethyl phosphite was removed by vacuum distillation, and the product was purified by column chromatography to obtain diethyl (4-(2,7-dibromo-9,9-dimethyl-9,10-dihydroacrylin-10-yl)butyl)phosphonate. The structural formula of the diethyl (4-(2,7-dibromo-9,9-dimethyl-9,10-dihydroacrylin-10-yl)butyl)phosphonate is as follows:

[0032] 1H NMR spectrum of diethyl phosphonate (4-(2,7-dibromo-9,9-dimethyl-9,10-dihydroacryl-10-yl)butyl)phosphonate ( 1 Characterized by ¹H NMR, the test conditions were DMSO-d6, 400 MHz. The spectral data are as follows: δ 7.50 (d, 2H, Ar-H), 7.36–7.34 (m, 2H, Ar-H), 7.07 (d, 2H, Ar-H), 4.02–3.92 (m, 6H, overlap of OCH24H and N-CH22H in P(O)(OCH2CH3)2), 1.83–1.74 (m, 4H, two intermediate CH2 atoms in the chain), 1.65–1.59 (m, 2H, P-CH2), 1.45 (s, 6H, 9,9-(CH3)2), 1.23 (t, 6H, CH3 in P(O)(OCH2CH3)2), with an integral total of 30H, corresponding to the molecular formula C. 23 H 30 The theoretical number of hydrogen atoms in Br2NO3P is consistent with that of Br2NO3P. 1 The H NMR spectrum is shown in [reference]. Figure 2 .

[0033] Step 3: Yamamoto Coupling Ni(Cod)₂ (1.1 eq), bipyridine (1.1 eq), and 1,5-cyclooctadiene (1.1 eq) were dissolved in 100 mL DMF and activated by stirring at 80 °C for 30 minutes. Separately, the product from step two and 1,4-dibromo-2,5-dipropoxybenzene were dissolved in 100 mL DMF and slowly added dropwise to the above activated reaction solution. The reaction was continued at 80 °C with stirring for 24 hours. The molar ratio of the product from step two to 1,4-dibromo-2,5-dipropoxybenzene was 2:1. After the reaction was completed, the mixture was cooled to room temperature, and dilute hydrochloric acid was slowly added dropwise with stirring until the system turned transparent yellow. The precipitate was collected by filtration to obtain a yellow random copolymer powder containing phosphonate dihydroacridine. The structural formula of the random copolymer containing phosphonate dihydroacridine is as follows:

[0034] Step 4: Phosphate hydrolysis Based on the product from step three (1.0 eq), the solution was dissolved in 200 mL of dichloromethane, and 20 mL of trimethylbromosilane (4.0 eq, 0.1 g / mL dichloromethane solution) was added dropwise. The mixture was stirred at room temperature for 24 hours. After the reaction was complete, excess methanol was added dropwise to quench the remaining trimethylbromosilane. The mixture was concentrated by vacuum distillation, precipitated in diethyl ether, filtered, washed with diethyl ether, and dried to obtain a random copolymer containing dihydroacridine phosphonate. The structural formula of the random copolymer containing dihydroacridine phosphonate is as follows:

[0035] The obtained random copolymer was determined to have a number-average molecular weight (Mn) of approximately 7500, a weight-average molecular weight (Mw) of approximately 11000, a degree of polymerization of M of 16, and a degree of polymerization of N of 8.

[0036] In this embodiment, the side chain length of structural unit A is m=4 (introduced by 1,4-dibromobutane in step one), and structural unit B is the structure shown in formula (II), with an alkoxy side chain length of n=3 (introduced by the propoxy group of the comonomer 1,4-dibromo-2,5-dipropoxybenzene).

[0037] Example 2 The difference between this embodiment and Example 1 is as follows: in step one, structural unit A is replaced by 1,2-dibromoethane instead of 1,2-dibromobutane (m=2); in step three, 1,4-dibromo-2,5-diethoxybenzene is replaced by 1,4-dibromo-2,5-dipropoxybenzene (n=2), and the molar ratio of A / B is 1:1; the coupling reaction temperature in step three is 20 °C, and the reaction time is 6 hours. The remaining steps and conditions are the same as in Example 1. The obtained random copolymer containing dihydroacrylamide phosphonate has a Mn of approximately 6100, a Mw of approximately 9200, a degree of polymerization M of 13, and a N of 13.

[0038] Example 3 The difference between this embodiment and Example 1 is as follows: in step one, structural unit A is replaced by 1,10-dibromodecane instead of 1,4-dibromobutane (m=10); in step three, 1,4-dibromo-2,5-didecoxybenzene is replaced by 1,4-dibromo-2,5-dipropoxybenzene (n=10), and the molar ratio of A / B is 1:10; the coupling reaction temperature in step three is 40 °C, and the reaction time is 12 hours. The remaining steps and conditions are the same as in Example 1. The obtained random copolymer containing dihydroacrylamide phosphonate has a Mn of approximately 9200, a Mw of approximately 13500, a degree of polymerization M of 2, and a N of 20.

[0039] Example 4 The difference between this embodiment and Example 1 is as follows: In step one, structural unit A is replaced by 1,20-dibromoeicosane instead of 1,4-dibromobutane (m=20); in step three, 2,5-dibromo-3-eicosylthiophene is replaced by 1,4-dibromo-2,5-dipropoxybenzene, with an alkyl side chain length x=20, and the molar ratio of A / B is 1:20; the coupling reaction temperature in step three is 60 ℃, and the reaction time is 24 hours. The remaining steps and conditions are the same as in Example 1. The obtained random copolymer containing dihydroacrylamide phosphonate has a Mn of approximately 10500, a Mw of approximately 15800, a degree of polymerization M of 2, and a X of 40.

[0040] Example 5 The difference between this embodiment and Example 1 is as follows: In step one, structural unit A is replaced by 1,30-dibromotriane instead of 1,4-dibromobutane (m=30); in step three, 2,5-dibromo-3-trianethiophene is replaced by 1,4-dibromo-2,5-dipropoxybenzene, with an alkyl side chain length x=30, and the molar ratio of A / B is 20:1; the coupling reaction temperature in step three is 100 °C, and the reaction time is 48 hours. The remaining steps and conditions are the same as in Example 1. The obtained random copolymer containing dihydroacrylamide phosphonate has a Mn of approximately 5700, a Mw of approximately 8600, a degree of polymerization M of 40, and a X of 2.

[0041] Example 6 This embodiment provides a perovskite solar cell, and the specific fabrication steps are as follows: (1) A PEDOT:PSS solution (diluted at a ratio of PEDOT:PSS:IPA = 1:3) was spin-coated onto ITO conductive glass at 3000 rpm for 30 s, followed by annealing at 100 ℃ for 10 min to obtain a PEDOT:PSS hole transport layer. The PEDOT is poly(3,4-ethylenedioxythiophene), PSS is polystyrene sulfonate, and IPA is isopropanol.

[0042] (2) The phosphonic acid dihydroacrylidine random copolymer prepared in Example 1 was dissolved in dimethyl sulfoxide to prepare a Poly-SAM solution of 1.1 mg / mL. The Poly-SAM solution was spin-coated on PEDOT:PSS at 3000 rpm for 30 s, followed by annealing at 100°C for 10 min. Then, isopropanol was spin-coated at 4000 rpm for 30 s and annealed at 100°C for 5 min to form a Poly-SAM interface modification layer on the PEDOT:PSS hole transport layer, thus obtaining a hole transport layer modified with Poly-SAM.

[0043] (3) The Al2O3 solution was then spin-coated onto the hole transport layer modified by Poly-SAM at 6000 rpm for 22 s and annealed at 100 °C for 5 min to form an Al2O3 crystal template layer.

[0044] (4) Subsequently, 1.9 M MA was spin-coated onto the Al2O3 crystal template layer. 0.3 FA 0.6 Cs 0.1 (Pb 0.5 Sn 0.5The I3 perovskite light-absorbing layer was prepared using a two-step spin-coating process, followed by annealing at 100 °C for 10 min. After the film cooled to room temperature, an ethylenediamine dihydroiodide solution was coated onto the perovskite film, and annealed at 100 °C for 5 min. Subsequently, (6,6)-phenyl-C 61 methyl butyrate solution was spin-coated onto a perovskite film at 3000 rpm for 30 s, followed by annealing at 70 °C for 10 min. Finally, 20 nm C20 nm films were sequentially deposited under high vacuum. 60 The tin-lead hybrid perovskite solar cell was fabricated using an 8 nm BCP and a 120 nm Ag electrode.

[0045] Example 7 This embodiment provides a perovskite solar cell, which differs from Example 6 in that the phosphonic acid dihydroacrylidine random copolymer in step 2 is the one prepared in Example 2.

[0046] Example 8 This embodiment provides a perovskite solar cell, which differs from Example 6 in that the phosphonic acid dihydroacrylidine random copolymer in step 2 is the one prepared in Example 3.

[0047] Example 9 This embodiment provides a perovskite solar cell, which differs from Example 6 in that the phosphonic acid dihydroacrylidine random copolymer in step 2 is the one prepared in Example 4.

[0048] Example 10 This embodiment provides a perovskite solar cell, which differs from Embodiment 6 in that the phosphonic acid dihydroacrylidine random copolymer in step 2 is the one prepared in Embodiment 5.

[0049] Comparative Example 1 This comparative example provides a perovskite solar cell, differing from Example 6 in that a small-molecule dihydroacridine phosphonate compound ((4-(2,7-dibromo-9,9-dimethyl-9,10-dihydroacridine-10-yl)butyl)phosphonic acid) is used instead of the dihydroacridine phosphonate random copolymer in Example 1 as the interface modification material. Specifically, a 1.1 mg / mL dimethyl sulfoxide solution of dihydroacridine phosphonate is spin-coated at 3000 rpm for 30 s on a PEDOT:PSS hole transport layer, followed by annealing at 100 °C for 10 min; then isopropanol is spin-coated at 4000 rpm for 30 s and annealed at 100 °C for 5 min. The remaining steps and conditions are the same as in Example 6. The number-average molecular weight (Mn) and weight-average molecular weight (Mw) of this dihydroacridine phosphonate compound are approximately 520.

[0050] Comparative Example 2 This comparative example provides a perovskite solar cell, which differs from Example 6 in that the molar ratio of A / B in step three of the preparation of the phosphonic acid dihydroacrylidine random copolymer is 1:30 (i.e., the molar ratio of the product from step two to 1,4-dibromo-2,5-dipropoxybenzene is 1:30). The number-average molecular weight (Mn) of the obtained copolymer was determined to be approximately 12,100, and the weight-average molecular weight (Mw) was approximately 18,900.

[0051] Comparative Example 3 This comparative example provides a perovskite solar cell, which differs from Example 6 in that the molar ratio of A / B in step three of the preparation process of the phosphonic acid dihydroacridine random copolymer is 30:1 (i.e., the molar ratio of the product from step two to 1,4-dibromo-2,5-dipropoxybenzene is 30:1). The number-average molecular weight (Mn) of the obtained copolymer was determined to be approximately 4900, and the weight-average molecular weight (Mw) was approximately 7200.

[0052] Comparative Example 4 This comparative example provides a perovskite solar cell, which differs from Example 6 in that the preparation step of the Poly-SAM interface modification layer is omitted, that is, Al2O3 solution is directly spin-coated on the PEDOT:PSS hole transport layer, and the remaining steps and conditions are the same as in Example 6.

[0053] Perovskite solar cell performance testing JV curve tests were performed on the perovskite solar cells prepared in Examples 6 to 10 and Comparative Examples 1 to 4. The photoelectric performance parameters, including open-circuit voltage, were recorded under AM 1.5G standard illumination conditions for both forward and reverse scanning. V OC ), short-circuit current density ( J SC ), fill factor ( FF The results of the photoelectric conversion efficiency (PCE) are shown in Table 1.

[0054] Table 1 JV Performance Parameters of Various Perovskite Solar Cells

[0055] As shown in Table 1, Examples 6-10, which used the phosphonic acid dihydroacrylidine random copolymer of the present invention as the interface modification layer, exhibited significantly higher photoelectric conversion efficiencies than Comparative Example 1, which used a small-molecule interface modification material, and Comparative Example 4, which did not have an interface modification layer. This indicates that the polymeric SAM strategy of the present invention is generally superior to the small-molecule SAM scheme. Furthermore, the copolymerization ratio of structural unit A to structural unit B needs to be maintained within an appropriate range. An imbalance in the ratio will lead to copolymer dysfunction, resulting in a significant decrease in the interface modification effect. There is a suitable window for the side chain length; both excessively long and excessively short side chains are detrimental to obtaining optimal performance. In addition, the coupling reaction conditions, by affecting the molecular weight of the polymerization product, also affect the film quality of the interface modification layer, ultimately manifesting as differences in device performance.

[0056] To further explore the underlying reasons for the excellent photoelectric performance obtained in Example 6, the perovskite thin film modified with the Poly-SAM interface prepared in Example 6 of this invention and the thin film prepared in Comparative Example 4 without interface modification were compared and tested in terms of film morphology, crystallinity, energy level arrangement, carrier dynamics and device stability.

[0057] Figure 3 The images show the SEM morphology of the perovskite films prepared in Example 6 and Comparative Example 4. It is clearly observed that the perovskite film in Comparative Example 4 has an uneven grain size distribution and obvious pores and gap defects at the grain boundaries; while the perovskite film in Example 6 has a significantly larger and more uniform grain size, with dense and continuous grain arrangement, and a smooth film surface without obvious pinholes or defects. This indicates that the present invention, by introducing a random copolymer interface modification layer containing phosphonic acid dihydroacrylidine onto the PEDOT:PSS surface, can effectively control the wettability and crystal growth process of the perovskite precursor solution, induce the formation of a high-quality, fully covered, dense perovskite film, significantly reduce film defect sites, and provide a solid structural foundation for reducing carrier recombination and improving device performance.

[0058] Figure 4 The X-ray diffraction (XRD) patterns of the perovskite thin films prepared in Example 6 and Comparative Example 4 are shown. It can be seen that both samples exhibit characteristic diffraction peaks of the tin-lead perovskite phase. However, compared to Comparative Example 4, the relative intensity of the corresponding characteristic diffraction peaks in Example 6 is significantly enhanced, and the full width at half maximum (FWHM) is noticeably narrower. According to the Scherrer equation, the increased diffraction peak intensity and narrower FWHM directly correspond to a significant increase in perovskite grain size and improved crystallinity. This indicates that the present invention can significantly improve the crystallinity of perovskite thin films and effectively reduce the defect state density at grain boundaries. This not only suppresses nonradiative recombination but also reduces the transport resistance of charge carriers at grain boundaries, thereby greatly improving the carrier transport efficiency within the device.

[0059] Figure 5The images show the ultraviolet photoelectron spectroscopy (UPS) spectra of perovskite and PEDOT:PSS, the cyclic voltammetry (CV) curves of the polymer self-assembled monolayer (Poly-SAM) containing the phosphonic acid dihydroacridine random copolymer prepared in Example 6 of this invention, and a schematic diagram of its energy level structure. Figure 5 (a) is the UPS spectrum of tin-lead perovskite, including the secondary electron cutoff edge (binding energy 16.67 eV, corresponding to work function W in the right figure). f (4.55 eV) and the valence band edge region (the top of the valence band in the left figure is 0.74 eV away from the Fermi level); Figure 5 (b) is the UPS spectrum of PEDOT:PSS, including the secondary electron cutoff edge (binding energy 16.38 eV, corresponding to work function W). f (4.84 eV) and the valence band edge region (the top of the valence band in the left figure is 0.27 eV away from the Fermi level); Figure 5 (c) is the cyclic voltammetry (CV) curve of Poly-SAM, showing that it has a significant oxidation peak; Figure 5 (d) is a schematic diagram of the energy level structures of tin-lead perovskite, PEDOT:PSS, and Poly-SAM. Figure 5 From (a), we know that the valence band top (VBM) level of tin-lead perovskite is calculated to be -5.29 eV; Figure 5 From (b), we know that the calculated valence band top (VBM) level of PEDOT:PSS is -5.11 eV. From Figure 5 The CV curve (c) was used to calculate the HOMO level of Poly-SAM as -5.18 eV based on the oxidation peak potential and a ferrocene reference. These test results were finally compiled and plotted as follows: Figure 5 The diagram shows the energy level structure (d). It can be seen that the energy level difference between pure PEDOT:PSS and perovskite is 0.18 eV. However, after introducing Poly-SAM, its -5.18 eV energy level is precisely interposed between PEDOT:PSS (-5.11 eV) and perovskite (-5.29 eV), constructing a perfect "stepped" energy level gradient (energy differences of only 0.11 eV and 0.07 eV). This indicates that the present invention can utilize this smooth gradient transition to not only significantly reduce the potential barrier for hole injection from the perovskite layer to the transport layer, promoting efficient hole extraction, but also act as an electron blocking layer, effectively blocking electron reverse leakage and suppressing nonradiative recombination at the interface. This dynamic optimization achieved through precise energy level control is precisely the device open-circuit voltage (V... OC The fundamental reason for the significant improvement.

[0060] Figure 6The figures show the TRPL (time-resolved fluorescence spectroscopy) decay curves of the perovskite films prepared in Example 6 and Comparative Example 4. Double exponential fitting reveals that the carrier lifetime of the perovskite film in Comparative Example 4 is 261.28 ns, while the carrier lifetime of the perovskite film in Example 6 is significantly shortened to 205.72 ns, exhibiting a strong fluorescence quenching effect. This indicates that the introduction of the Poly-SAM modification layer significantly accelerates the extraction and separation rate of holes at the interface, effectively reducing the bulk recombination loss of carriers before extraction. This demonstrates that the modification layer successfully constructs a smoother hole transport channel, greatly improving the interface carrier extraction efficiency.

[0061] Figure 7 The table shows the JV test curves of the tin-lead hybrid perovskite solar cells prepared in Example 6 and Comparative Example 4. Analysis of the data in Table 1 shows that, compared to the control device with a pure PEDOT:PSS hole transport substrate, the target device (Example 6) modified with the Poly-SAM interface has a significantly higher open-circuit voltage (V1). OC ), short-circuit current density (J SC Both the fill factor (FF) and the energy level (SAM) were simultaneously improved. This indicates that the present invention, through Poly-SAM interface modification, achieved comprehensive optimization of microstructure, crystal quality, energy level matching, and carrier dynamics, ultimately synergistically contributing to a comprehensive breakthrough in the photovoltaic performance of the device.

[0062] Those skilled in the art will readily understand that the above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A random copolymer containing dihydroacridine phosphonate, characterized in that, The random copolymer containing dihydroacrylamide phosphonate contains structural unit A and structural unit B, which are randomly distributed in the copolymer backbone. Structural unit A has the structure shown in Formula I, and structural unit B has the structure shown in Formula II or Formula III. Equation I: or ; Formula II: ; Formula III: ; The side chain lengths m, n, and x in the structures of Formula I, Formula II, or Formula III are 2 to 30, and the degrees of polymerization M, N, and X are 2 to 40. The random copolymer containing dihydroacrylamide phosphonate has a number-average molecular weight (Mn) of 5000 Da to 11000 Da and a weight-average molecular weight (Mw) of 8000 Da to 16000 Da; The molar ratio of structural unit A to structural unit B is 1:20 to 20:

1.

2. The random copolymer containing dihydroacrylamide phosphonate according to claim 1, characterized in that, The random copolymer containing phosphonic acid dihydroacridine includes one of the following structural formulas: 。 3. A hole transport layer, characterized in that, The hole transport layer comprises a hole transport base layer and an interface modification layer disposed on the hole transport base layer; the interface modification layer comprises a random copolymer containing phosphonic acid dihydroacridine as described in claim 1 or 2.

4. A perovskite solar cell, characterized in that, The perovskite solar cell includes the hole transport layer as described in claim 3.

5. A method for preparing a random copolymer containing dihydroacrylamide phosphonate according to claim 1 or 2, characterized in that, Includes the following steps: Step 1: 2,7-dihalo-9,9-dialkyl-9,10-dihydroacridine is reacted with a dihaloalkane under basic conditions to undergo an N-alkylation reaction to obtain a haloalkylated dihydroacridine intermediate. Step 2: The haloalkylated dihydroacridine intermediate is reacted with triethyl phosphite in an Arbuzov reaction to obtain compound I; Step 3: Compound I and the comonomer are subjected to a Yamamoto coupling reaction to obtain a random copolymer containing dihydroacrylidine phosphonate; the comonomer is selected from compound II or compound III; Step four: The random copolymer containing phosphonate dihydroacridine is reacted with a halosilane and then subjected to alcoholysis to obtain the random copolymer containing phosphonate dihydroacridine. Wherein, compound I, after being coupled with Yamamoto, forms structural unit A in the random copolymer containing dihydroacridine phosphonate, and compound II or compound III, after being coupled with Yamamoto, forms structural unit B in the random copolymer containing dihydroacridine phosphonate.

6. The method for preparing a random copolymer containing dihydroacrylamide phosphonate according to claim 5, characterized in that, The structural formula of compound I is: or , The structural formula of compound II is: , The structural formula of compound III is: .

7. The method for preparing a random copolymer containing dihydroacrylamide phosphonate according to claim 6, characterized in that, In the structures of compounds I, II, and III, R1, R1', R2, R2', R3, and R3' are each independently selected from Br.

Citation Information

Patent Citations

  • Perovskite solar cell based on composite hole transport layer and preparation method thereof

    CN111509128A

  • Perovskite solar cell and preparation method thereof

    CN118870943A

  • Carbazole phosphate material as well as preparation method and application thereof

    CN119504858A