A weather-resistant UV coating for PP and its preparation method

By combining modified epoxy resin with aliphatic polyurethane acrylate and using a mercapto-olefin photopolymerization system, the problems of complex formulation and oxygen inhibition in UV coatings for PP substrates have been solved, resulting in UV coatings with high adhesion, low shrinkage, and excellent weather resistance, suitable for PP plastic flower pots, PP automotive parts, and PP packaging containers.

CN123107531APending Publication Date: 2026-11-17NANXIONG XINGLONG CHEM CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202611510879.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing UV coatings for PP substrates suffer from problems such as high formulation complexity, high cost, increased cost due to the use of inorganic nanofillers, the influence of oxygen inhibition on traditional UV curing systems, poor surface curing quality, and large shrinkage stress in single free radical polymerization networks.

Method used

By introducing the reaction product of dimercaprol and ethyl isocyanate acrylate to modify epoxy resin, acrylate double bonds and thiocarbamate bonds are introduced, and it is compounded with 2-6 functional aliphatic polyurethane acrylate to form a low internal stress crosslinking network. Combined with the mercapto-olefin photopolymerization system, oxygen inhibition is overcome, and adhesion and weather resistance are improved.

Benefits of technology

It achieves PP substrate adhesion grade 0, fast curing speed, low VOC emissions, and excellent weather resistance. The coating shows no obvious yellowing in QUV aging test, good water immersion resistance, high hardness and gloss, and meets environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to a weather-resistant UV coating for PP and its preparation method, belonging to the field of coating technology. The coating comprises a 2-6 functional aliphatic polyurethane acrylate, a difunctional modified epoxy acrylate, a reactive diluent, a photoinitiator and additives, and a solvent. The modified epoxy acrylate is prepared by reacting dimercaprol with ethyl isocyanate acrylate followed by ring-opening addition with epoxy resin, simultaneously introducing acrylate double bonds, thioether bonds, and thiocarbamate bonds into the molecule. This invention achieves a PP substrate adhesion rating of 0, no significant yellowing after 288 hours of QUV aging, no blistering after 96 hours of water resistance, a hardness ≥2H, and a gloss ≥95° through the combined rigidity and flexibility of the difunctional and hexafunctional polyurethane acrylates and the stress dissipation effect of the modified epoxy dynamic bonds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of coating technology and relates to a weather-resistant UV coating for PP and its preparation method. Background Technology

[0002] Polypropylene (PP) plastic is widely used in plastic flower pots, packaging containers, and other fields due to its excellent mechanical properties, chemical stability, and processability. UV-curable coatings, with their advantages of fast curing speed, low VOCs, and low energy consumption, have become an important development direction for PP plastic coating.

[0003] In the prior art, various UV coatings for PP substrates have been disclosed. For example, CN101602917B discloses a UV-curable coating that improves weather resistance by adding inorganic nanofillers such as nano zinc oxide or nano titanium dioxide, suitable for plastic substrates such as PP. CN105949966A discloses a UV coating specifically for PP substrates, which uses a compound of difunctional epoxy acrylate and trifunctional polyurethane acrylate, and adds an adhesion promoter to solve the adhesion problem of PP. CN104610856A discloses a vacuum electroplating UV coating for PP substrates, which achieves flame-free adhesion of PP by using a chlorinated polyolefin adhesion promoter in conjunction with a primer. CN117447912A discloses a PP mirror coating UV coating, which uses a compound of modified epoxy acrylate and difunctional aromatic polyurethane acrylate. Li Huilu et al. (Preparation of UV-curable coating for PP film) prepared a UV-curable coating for PP film using polyurethane acrylate and epoxy acrylate as prepolymers, achieving adhesion grade 0 and hardness 3H.

[0004] However, the aforementioned existing technologies still have shortcomings: First, relying on inorganic nanofillers or adhesion promoters to solve adhesion and weather resistance problems increases the complexity and cost of the formulation; second, existing solutions mostly use physical blends of conventional epoxy acrylates and polyurethane acrylates, and the resin molecular structure itself lacks affinity design for PP substrates; third, traditional UV curing systems are affected by oxygen inhibition, the surface curing quality needs to be improved, and the single free radical polymerization network has high shrinkage stress, which is not conducive to PP adhesion. Therefore, developing a PP-specific UV coating that requires no complex pretreatment, has low shrinkage, and high weather resistance remains of significant practical importance. Summary of the Invention

[0005] The purpose of this invention is to provide a weather-resistant UV coating for PP and its preparation method. This invention modifies epoxy resin by introducing the reaction product of dimercaprol and ethyl isocyanate acrylate. It simultaneously introduces UV-curable acrylate double bonds and thiocarbamate bonds that dissipate shrinkage stress onto the epoxy backbone, and uses 2-6 functional aliphatic polyurethane acrylate to provide a rigid-flexible mechanical framework, constructing a crosslinked network with low internal stress and low curing shrinkage, thus achieving direct adhesion to PP substrates and long-term weather resistance.

[0006] The objective of this invention can be achieved through the following technical solutions: In a first aspect, the present invention provides a weather-resistant UV coating for PP, comprising the following components by weight: 40-60 parts of 2-6 functional aliphatic polyurethane acrylate; 10-20 parts of difunctional modified epoxy acrylate; 5-10 parts of reactive diluent; 1.8-4 parts of photoinitiator; 0.3-0.9 parts of leveling agent; 0.2-0.5 parts of wetting agent; 0.2-0.6 parts of defoamer; and 5-10 parts of solvent.

[0007] The 2-6 functional aliphatic polyurethane acrylate comprises difunctional aliphatic polyurethane acrylate and hexafunctional aliphatic polyurethane acrylate, with a weight ratio of 1-2:1. The difunctional aliphatic polyurethane acrylate has a flexible molecular chain, which can reduce the curing shrinkage stress and modulus of the coating, providing basic adhesion to the PP substrate. The hexafunctional aliphatic polyurethane acrylate contains multiple unsaturated double bonds, which can form a highly cross-linked three-dimensional network structure, significantly improving the hardness, water resistance, and weather resistance of the coating film. The combination of these two components forms a mechanical framework that combines rigidity and flexibility, ensuring both adhesion and the strength of the coating itself.

[0008] The preparation method of the difunctional modified epoxy acrylate includes: (a) Dimercaptopropanol and ethyl isocyanate acrylate are reacted at room temperature in the presence of a catalyst. A mercapto group of the dimercaptopropanol undergoes nucleophilic addition with the NCO group of the ethyl isocyanate acrylate to generate an intermediate, while a thiocarbamate bond is introduced. (b) The intermediate is subjected to a ring-opening addition reaction with bisphenol A type epoxy resin in the presence of a catalyst at 40-80°C. The thiol groups retained on the intermediate undergo a thiol-epoxy click ring-opening reaction with the epoxy groups to generate a modified epoxy acrylate containing acrylate double bonds, thioether bonds, thiocarbamate bonds and multiple hydroxyl groups.

[0009] Among them, the thioether bond imparts flexibility to the molecular chain segments and reduces internal stress during curing; the thiocarbamate bond has dynamic covalent bond characteristics, which can dissipate the curing shrinkage stress of the coating through dynamic exchange, thus significantly improving the adhesion between the coating and the substrate; the hydroxyl group can form hydrogen bonds at the interface between the coating and the PP substrate, enhancing interfacial adhesion.

[0010] The molar ratio of dimercaprol to ethyl isocyanate acrylate is preferably 1:1 to achieve single-sided end capping and retain one mercapto group for subsequent epoxy grafting; the catalyst in step (a) is preferably triethylamine or 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), and the amount of catalyst used is 0.1%-1% of the total mass of the reactants; the catalyst in step (b) is preferably tetrabutylammonium fluoride or triphenylphosphine, and the amount of catalyst used is 0.5%-2% of the total mass of the reactants.

[0011] Preferably, the reactive diluent comprises one or more of 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, and tripropylene glycol diacrylate, used to adjust the viscosity of the system and participate in UV curing crosslinking.

[0012] Furthermore, the reactive diluent may also contain a thiol compound prepared by reacting 3-mercaptopropyltrimethoxysilane with o-nitrobenzyl halide. Under ultraviolet light irradiation, the o-nitrobenzyl group of this compound undergoes photolytic cleavage to release thiol groups. The released thiol groups then react with unsaturated double bonds in the system via a thiol-alkene click reaction, forming grafts. Studies have shown that the thiol-alkene photopolymerization system has advantages such as antioxidant polymerization inhibition, low volume shrinkage, and delayed gelation. It can effectively overcome the oxygen inhibition problem of traditional acrylate free radical polymerization, reduce curing shrinkage stress, improve double bond conversion rate, reduce gelation, and make the crosslinking network more uniform. In addition, the silane end (-Si(OCH3)3) of 3-mercaptopropyltrimethoxysilane, after hydrolysis, can form chemical bonds with polar sites on the surface of the PP substrate, enhancing adhesion.

[0013] Preferably, the photoinitiator is selected from one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexylphenyl ketone, and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and is used to generate free radicals to initiate polymerization under ultraviolet light irradiation.

[0014] Preferably, the leveling agent, wetting agent, and defoamer are conventional additives in the coatings industry, used to improve the leveling properties of the coating, the wettability of the substrate, and to eliminate air bubbles during the construction process, respectively.

[0015] Preferably, the solvent is butyl acetate or ethyl acetate, used to adjust the viscosity of the coating during application.

[0016] Secondly, the present invention provides a method for preparing a weather-resistant UV coating for PP, comprising the following steps: mixing a photoinitiator with a solvent and stirring until dissolved and free of particles; adding aliphatic polyurethane acrylate resin and modified epoxy acrylate resin and stirring evenly; adding an active diluent and stirring evenly; adding a leveling agent, a wetting agent and a defoamer and stirring evenly to obtain the weather-resistant UV coating for PP.

[0017] Thirdly, the present invention provides an application of a weather-resistant UV coating for PP.

[0018] The coating of this invention can be sprayed onto the surface of a PP substrate and cured by ultraviolet light to form a coating layer. The ultraviolet curing energy is 500-700 mJ / cm². 2 During the curing process, the photoinitiator absorbs ultraviolet light to generate free radicals, initiating the free radical polymerization of acrylate double bonds and the click reaction of thiol-olefins. The silane ends hydrolyze and bond with the substrate, forming a multi-stage curing system. PP plastic flower pots, PP automotive trim parts, or PP packaging containers can all be applications of this invention.

[0019] The UV curing mechanism of the coating of this invention is as follows: Under ultraviolet light irradiation, the photoinitiator absorbs light energy and decomposes to generate free radicals, which initiate a chemical reaction. First, the acrylate double bonds in the system undergo free radical chain polymerization to form a main crosslinking network. Second, the o-nitrobenzyl group in the thiol compound undergoes photolytic cleavage to release active thiol groups. The released thiol groups react with the unsaturated double bonds in the system to form a thiol-alkene click reaction, thus forming a graft.

[0020] The beneficial effects of this invention are as follows: (1) The present invention modifies epoxy resin by reacting dimercaprol with isocyanate ethyl acrylate, and simultaneously introduces acrylate double bonds, thioether bonds and thiocarbamate bonds into the epoxy skeleton. Combined with the rigid and flexible compound of difunctional and hexafunctional aliphatic polyurethane acrylate, it achieves 0-level adhesion to PP substrate, while having fast curing speed and low VOC emissions, which meets environmental protection requirements.

[0021] (2) This invention introduces a mercapto-olefin photopolymerization system into the reactive diluent, utilizing its advantages such as anti-oxidation polymerization, small volume shrinkage, and reduced system gelation to effectively overcome the oxygen inhibition problem of traditional acrylate free radical polymerization, reduce curing shrinkage stress, and make the crosslinking network more uniform. The coating obtained by this invention showed no obvious yellowing after 288 hours of QUV aging test, no blistering after 96 hours of water immersion, hardness ≥2H, gloss ≥95°, and excellent comprehensive performance. Detailed Implementation

[0022] To further illustrate the technical means and effects of the present invention in achieving the intended purpose, the following detailed description of the specific implementation methods, structures, features and effects of the present invention, in conjunction with preferred embodiments, is provided below.

[0023] Example 1 A method for preparing a weather-resistant UV coating for PP includes the following steps: By weight, the following components are present: 30 parts of difunctional aliphatic polyurethane acrylate, 20 parts of hexafunctional aliphatic polyurethane acrylate, 15 parts of difunctional modified epoxy acrylate, 5 parts of 1,6-hexanediol diacrylate, 3 parts of trimethylolpropane triacrylate, 2.5 parts of 1-hydroxycyclohexylphenyl ketone, 0.5 parts of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 0.5 parts of BYK-358N, 0.3 parts of TEGO Wet KL 245, 0.3 parts of BYK-054, and 8 parts of butyl acetate.

[0024] Preparation method: Mix the photoinitiator with butyl acetate and stir until completely dissolved and free of particles; add difunctional aliphatic polyurethane acrylate, hexafunctional aliphatic polyurethane acrylate and difunctional modified epoxy acrylate, and stir at 800-1000 rpm for 30 minutes; add 1,6-hexanediol diacrylate and trimethylolpropane triacrylate, and continue stirring for 15 minutes; add BYK-358N, TEGO Wet KL 245 and BYK-054, and stir for 20 minutes to obtain a weather-resistant UV coating for PP.

[0025] Difunctional polyurethane acrylates have a viscosity of 4000-10000 cps / 25℃ and are colorless to slightly yellow viscous liquids, such as RU-2446. Hexafunctional polyurethane acrylates have a viscosity of 1000-3000 cps / 25℃ and are colorless to slightly yellow transparent viscous liquids, such as RU-6136B.

[0026] The preparation of difunctional modified epoxy acrylates includes: (a) In a reaction vessel, 54 parts of dimercaprol were added, and nitrogen gas was introduced for protection. 0.5 parts of triethylamine catalyst were added, and the mixture was stirred and heated to 25-30°C. 70 parts of ethyl isocyanate acrylate were slowly added dropwise, with the reaction temperature controlled to not exceed 30°C during the addition. After the addition was complete, the reaction was continued at room temperature for 2 hours. Samples were taken during the reaction for TLC monitoring. After the reaction was completed, a mercaptoacrylate intermediate was obtained.

[0027] Infrared display at 2268 cm -1 The characteristic absorption peak of the isocyanate group (-NCO) basically disappeared, while at 1528 cm⁻¹... -1 and 1692 cm -1 The appearance of new absorption peaks nearby corresponds to the NH bending vibration and C=O stretching vibration in the thiocarbamate bond, respectively, indicating that the mercapto group has reacted with the isocyanate ethyl acrylate.

[0028] (b) In a reaction vessel equipped with a thermometer, reflux condenser, and stirrer, add 100 parts of bisphenol A type epoxy resin (epoxy value 0.50-0.54 eq / 100g) and heat to 50-60℃ to melt it. Add 1.5 parts of a mercaptoacrylate intermediate and tetrabutylammonium fluoride, heat to 65-70℃, and maintain the temperature for 4 hours. During the reaction, take samples to measure the epoxy value. If the epoxy value no longer decreases significantly after 3-4 hours (0.05 eq / 100g), stop the reaction, cool down, and discharge the material to obtain difunctional modified epoxy acrylate.

[0029] Example 2 A method for preparing a weather-resistant UV coating for PP includes the following steps: By weight, the following components are present: 35 parts of difunctional aliphatic polyurethane acrylate, 20 parts of hexafunctional aliphatic polyurethane acrylate, 15 parts of difunctional modified epoxy acrylate, 6 parts of 1,6-hexanediol diacrylate, 4 parts of trimethylolpropane triacrylate, 4.0 parts of 1-hydroxycyclohexylphenyl ketone, 0.5 parts of BYK-358N, 0.3 parts of TEGO Wet KL 245, 0.3 parts of BYK-054, and 10 parts of ethyl acetate.

[0030] The preparation method is the same as in Example 1.

[0031] Example 3 A method for preparing a weather-resistant UV coating for PP includes the following steps: By weight, the following components are present: 25 parts of difunctional aliphatic polyurethane acrylate, 15 parts of hexafunctional aliphatic polyurethane acrylate, 10 parts of difunctional modified epoxy acrylate, 3 parts of 1,6-hexanediol diacrylate, 2 parts of trimethylolpropane triacrylate, 1.4 parts of 1-hydroxycyclohexylphenyl ketone, 0.4 parts of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 0.5 parts of BYK-358N, 0.3 parts of TEGO Wet KL 245, 0.3 parts of BYK-054, and 5 parts of butyl acetate.

[0032] The preparation method is the same as in Example 1.

[0033] Example 4 A method for preparing a weather-resistant UV coating for PP includes the following steps: By weight, the following components are present: 35 parts of difunctional aliphatic polyurethane acrylate, 25 parts of hexafunctional aliphatic polyurethane acrylate, 20 parts of difunctional modified epoxy acrylate, 6 parts of 1,6-hexanediol diacrylate, 4 parts of trimethylolpropane triacrylate, 3.2 parts of 1-hydroxycyclohexylphenyl ketone, 0.8 parts of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 0.5 parts of BYK-358N, 0.3 parts of TEGO Wet KL 245, 0.3 parts of BYK-054, and 10 parts of butyl acetate.

[0034] The preparation method is the same as in Example 1.

[0035] Example 5 A method for preparing a weather-resistant UV coating for PP includes the following steps: By weight, the following components are present: 30 parts of difunctional aliphatic polyurethane acrylate, 20 parts of hexafunctional aliphatic polyurethane acrylate, 15 parts of difunctional modified epoxy acrylate, 4 parts of 1,6-hexanediol diacrylate, 2 parts of trimethylolpropane triacrylate, 0.8 parts of mercapto compound, 2.5 parts of 1-hydroxycyclohexylphenyl ketone, 0.5 parts of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 0.5 parts of BYK-358N, 0.3 parts of TEGO Wet KL 245, 0.3 parts of BYK-054, and 8 parts of butyl acetate.

[0036] The preparation method is the same as in Example 1.

[0037] The preparation of the thiol compound involved the following steps: In a reaction vessel, 20 parts of 3-mercaptopropyltrimethoxysilane and 22 parts of o-nitrobenzyl bromide were added and dissolved in 50 parts of anhydrous tetrahydrofuran under nitrogen protection. 18 parts of anhydrous potassium carbonate were then added, and the mixture was stirred at room temperature for 4 hours. The reaction was stopped after TLC monitoring showed that the starting material had essentially disappeared. The mixture was then filtered and rotary evaporated to obtain the thiol compound.

[0038] Comparative Example 1 It is basically the same as Example 1, except that: no difunctional modified epoxy acrylate is added, and an equal amount of difunctional aliphatic polyurethane acrylate is added to make up the difference.

[0039] Comparative Example 2 The method is basically the same as in Example 1, except that commercially available unmodified difunctional epoxy acrylate (Boxin B-100) is used in an equal amount to replace the self-made difunctional modified epoxy acrylate.

[0040] Comparative Example 3 It is basically the same as Example 1, except that: no hexafunctional aliphatic polyurethane acrylate is added, and an equal amount of difunctional aliphatic polyurethane acrylate is added instead.

[0041] Comparative Example 4 It is basically the same as Example 1, except that the mercapto compound in Example 5 is replaced with 3-mercaptopropyltrimethoxysilane.

[0042] Performance testing: The coatings prepared in Examples 1-5 and Comparative Examples 1-3 were sprayed onto the surface of a PP substrate with a coating thickness of 20-30 μm and a spraying strength of 500-700 mJ / cm. 2 UV curing was performed under specific energy conditions, and performance testing was conducted using the following methods: Adhesion test: conducted in accordance with GB / T 9286-2021, with a rating standard of 0 to 5 (0 being the best).

[0043] Weather resistance test: QUV aging test was conducted in accordance with GB / T 1865-2009, and the yellowing of the coating was observed after 288 hours.

[0044] Water resistance test: Immerse the coated sample in water at room temperature (25±2℃) for 96 hours, observe whether the coating blisters or peels off, and test the adhesion after boiling in water.

[0045] Hardness test: The pencil hardness test was conducted in accordance with GB / T 6739-2022.

[0046] Gloss test: The gloss of the coating was measured using a 60° gloss meter in accordance with GB / T 9754-2025.

[0047] High and low temperature cycling test: Place the coated sample in alternating cycles of -40℃ and 80℃ (2 hours each, for a total of 4 cycles) and observe whether the paint film cracks or wrinkles.

[0048]

[0049] In Example 5, the surface was completely cured, non-sticky, and had a uniform gloss, while the surfaces of the other examples were slightly sticky. This indicates that the thiol groups released by photolysis improved the surface drying performance of the coating through an antioxidant polymerization inhibition mechanism. The protection of the thiol groups by the o-nitrobenzyl group effectively solved the storage stability problem, preventing the formulation from gelling after 6 months of storage at room temperature, while Comparative Example 4 showed gelation after 20 days.

[0050] This invention modifies epoxy resin by reacting dimercaprol with ethyl isocyanate acrylate, introducing acrylate double bonds, thioether bonds, and thiocarbamate dynamic bonds into the epoxy backbone. Combined with difunctional and hexafunctional aliphatic polyurethane acrylates, it achieves comprehensive performance of PP substrate adhesion grade 0, hardness 2H, no obvious yellowing after 288 hours of QUV aging, and no blistering after 96 hours of water resistance. At the same time, it has low VOC emissions and fast curing speed, meeting environmental protection requirements.

[0051] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. A weather-resistant UV coating for PP, characterized in that, The following components are included by weight: 40-60 parts of 2-6 functional aliphatic polyurethane acrylate; 10-20 parts of difunctional modified epoxy acrylate; 5-10 parts reactive diluent; Photoinitiator 1.8-4 parts; Leveling agent 0.3-0.9 parts; 0.2-0.5 parts of wetting agent; Defoamer 0.2-0.6 parts; 5-10 parts solvent; The preparation method of the difunctional modified epoxy acrylate includes: (a) Dimercaptopropanol was reacted with ethyl isocyanate acrylate at room temperature in the presence of a catalyst to obtain a mercapto-containing acrylate intermediate; (b) The intermediate is subjected to ring-opening addition with bisphenol A type epoxy resin to obtain the modified epoxy acrylate.

2. The weather-resistant UV coating for PP according to claim 1, characterized in that, The 2-6 functional aliphatic polyurethane acrylates include difunctional aliphatic polyurethane acrylates and hexafunctional aliphatic polyurethane acrylates.

3. The weather-resistant UV coating for PP according to claim 1, characterized in that, The reactive diluent comprises one or more of 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, and tripropylene glycol diacrylate.

4. The weather-resistant UV coating for PP according to claim 1, characterized in that, The molar ratio of dimercaprol to ethyl isocyanate acrylate is 1:

1.

5. The weather-resistant UV coating for PP according to claim 1, characterized in that, The catalyst described in step (a) is triethylamine or 1,8-diazabicyclo[5.4.0]undec-7-ene.

6. The weather-resistant UV coating for PP according to claim 1, characterized in that, The catalyst mentioned in step (b) is tetrabutylammonium fluoride or triphenylphosphine.

7. The weather-resistant UV coating for PP according to claim 1, characterized in that, The photoinitiator is selected from one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexylphenyl ketone, and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide.

8. The weather-resistant UV coating for PP according to claim 3, characterized in that, The reactive diluent also contains a thiol compound, which is prepared by reacting 3-mercaptopropyltrimethoxysilane with o-nitrobenzyl halide.

9. A method for preparing a weather-resistant UV coating for PP as described in any one of claims 1-8, characterized in that, Includes the following steps: The photoinitiator and solvent are mixed and stirred until dissolved and free of particles; aliphatic polyurethane acrylate resin and modified epoxy acrylate resin are added and stirred evenly; reactive diluent is added and stirred evenly; leveling agent, wetting agent and defoamer are added and stirred evenly to obtain the weather-resistant UV coating for PP.

10. An application of the weather-resistant UV coating for PP as described in any one of claims 1-8, characterized in that, The coating is sprayed onto the surface of a PP substrate and cured under ultraviolet light to form a coating layer. The energy of the ultraviolet curing is 500-700 mJ / cm². 2 .

Citation Information

Patent Citations

  • A UV-curable coating

    CN101602917B

  • Vacuum plating UV coating of PP base material as well as preparation method and use of vacuum plating UV coating

    CN104610856A

  • Special UV paint for PP (polypropylene) substrates

    CN105949966A

  • PP mirror coating UV paint and preparation method and construction method thereof

    CN117447912A