LCD diffusion film UV coating composition and diffusion film preparation process

By copolymerizing and fixing benzophenone-type photoinitiating units and tertiary amine synergistic units in the acrylate copolymer shell of the diffuser particles, combined with low-dose UV pre-curing and drying treatment, the displacement problem of the light diffuser particles during the wet film drying stage was solved, achieving a balance between the uniformity of the diffuser film and solvent removal.

CN123107532APending Publication Date: 2026-11-17CHENZHOU HAILI MICROELECTRONICS TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611514401.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

During the diffusion film coating process, the relative displacement of light-diffusing particles during the wet film drying stage is difficult to control, and the pre-curing of the wet film has a significant impact on the subsequent solvent escape.

Method used

The benzophenone-type photoinitiator and the tertiary amine synergistic unit are copolymerized and fixed in the acrylate copolymer shell of the diffused particles. Based on the limited prepolymerization in the bulk phase, an additional local free radical source is provided for the particle's adjacent region. The particle displacement is reduced by low-dose UV pre-curing and drying treatment.

Benefits of technology

It effectively reduces the relative displacement of light-diffusing particles during the wet film drying stage, taking into account both the uniformity of particle distribution and the effective removal of solvent, thereby improving the overall quality of the diffusion film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107532A_ABST
    Figure CN123107532A_ABST
Patent Text Reader

Abstract

This invention discloses a UV coating composition for LCD diffusion films and a diffusion film preparation process. The composition includes shell-fixed photoinitiating core-shell photodiffusing particles, aliphatic polyurethane acrylate, a reactive diluent, a bulk photoinitiator, additives, and an organic solvent. The core-shell particles comprise a polymethylsilsesquioxane core and an acrylate copolymer shell, wherein benzophenone-type photoinitiating units and tertiary amine synergistic units are copolymerized and fixed in the shell. The composition does not contain a free tertiary amine-type photoinitiating synergist. After coating, low-dose pre-curing is performed using 365nm UV light during the wet film stage, followed by drying and primary curing using 385–405nm UV light. This invention reduces the relative displacement of the diffusion particles during the wet film drying stage and is suitable for diffusion films used in LCD backlight modules.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of optical film coating technology, and particularly relates to an LCD diffusion film UV coating composition and diffusion film preparation process. Background Technology

[0002] LCD diffusion films typically consist of a transparent substrate and a resin coating containing light-diffusing particles on the surface of the substrate. The refractive index difference between the light-diffusing particles and the resin matrix causes light scattering, thereby improving light emission uniformity.

[0003] During the diffusion film coating process, after the solvent-based UV coating solution forms a wet film, before the solvent has completely evaporated, the light-diffusing particles may undergo relative displacement or local enrichment due to gravity, interfacial tension, and the flow of the wet film caused by solvent evaporation. Increasing the viscosity of the coating solution to inhibit particle movement may affect coating transfer and leveling; performing UV curing after the wet film has dried cannot reduce the displacement of particles that has already occurred during the wet film drying period.

[0004] Benzophenone-type photoinitiators can generate free radicals by abstracting hydrogen from hydrogen donors or by transferring electrons to electron donors, and tertiary amine co-initiators can improve their free radical generation efficiency. When benzophenone and tertiary amine co-initiators are added to the coating solution in free form, the tertiary amine co-initiator may diffuse or migrate in the wet film.

[0005] Therefore, there is still a need for further improvement in how to combine the fixed photoinitiator structure with low-dose pre-curing in the wet film stage to reduce the relative displacement of diffused particles in the drying stage without significantly increasing the viscosity of the coating liquid, while also taking into account subsequent solvent discharge. Summary of the Invention

[0006] The technical problem to be solved by the present invention is to reduce the relative displacement of light-diffusing particles during the wet film drying stage without significantly increasing the viscosity of the coating liquid, and to reduce the adverse effects of the overall pre-curing of the wet film on subsequent solvent escape.

[0007] The present invention further provides an additional source of local free radicals for the particle's neighborhood by immobilizing the benzophenone-type photoinitiator and the tertiary amine synergistic unit together in the acrylate copolymer shell of the diffused particles, based on the limited prepolymerization in the bulk phase.

[0008] This invention is achieved as follows: an LCD diffusion film UV coating composition, based on a total of 100 parts by weight of non-volatile components in the coating, comprises: 12-28 parts by weight (preferably 15-25 parts by weight) of shell-fixed photoinitiating core-shell photodiffusing particles A, 30-50 parts by weight (preferably 35-45 parts by weight) of aliphatic polyurethane acrylate B, 18-35 parts by weight (preferably 20-30 parts by weight) of monofunctional reactive diluent C, 6-18 parts by weight (preferably 8-15 parts by weight) of bifunctional reactive diluent D, 0.5-3 parts by weight (preferably 1-2.5 parts by weight) of bulk photoinitiator E, and 0.1-1.5 parts by weight (preferably 0.2-1 parts by weight) of additive F. The sum of the weight parts of the above non-volatile components is 100.

[0009] The composition further comprises, relative to 100 parts by weight of the non-volatile component of the coating, 90 to 180 parts by weight of an organic solvent, preferably 120 to 170 parts by weight. The organic solvent is selected from one or more of ethyl acetate, butanone, and propylene glycol methyl ether acetate.

[0010] The "bulk photoinitiator" mentioned in this article refers to a photoinitiator that is dissolved or dispersed in the resin phase of the coating liquid in a molecular state and is not covalently fixed in the shell of the core-shell light-diffusing particles.

[0011] The shell-fixed photoinitiated core-shell photodiffusing particle A comprises a polymethylsilsesquioxane core and an acrylate copolymer shell covering the outside of the core.

[0012] Preferably, the TEM average diameter of the core is 2.8–3.2 μm and the refractive index is 1.42–1.45; the TEM average thickness of the acrylate copolymer shell is 115–145 nm and the refractive index is 1.46–1.50.

[0013] The TEM average diameter and TEM average thickness mentioned in this article are the arithmetic mean of the core diameter and radial shell thickness measured by transmission electron microscopy of no less than 50 core-shell light-diffusing particles.

[0014] The acrylate copolymer shell is formed by copolymerization of methyl methacrylate, butyl acrylate, ethylene glycol dimethacrylate, benzophenone-type polymerizable monomers and tertiary amine-type polymerizable monomers.

[0015] The benzophenone-type polymerizable monomer is 4-methacryloyloxybenzophenone and / or 4-acryloyloxybenzophenone; the tertiary amine-type polymerizable monomer is dimethylaminoethyl methacrylate.

[0016] The benzophenone-type polymerizable monomer and the tertiary amine-type polymerizable monomer participate in shell copolymerization through their respective olefinic unsaturated groups.

[0017] Apart from the tertiary amine synergist units copolymerized and fixed in the shell, the composition does not contain any additional tertiary amine photoinitiator as an independent formulation component.

[0018] Based on the total amount of all polymerizable monomers forming the acrylate copolymer shell, methyl methacrylate is 55-75 wt%, butyl acrylate is 20-35 wt%, ethylene glycol dimethacrylate is 0.5-2 wt%, benzophenone-type polymerizable monomer is 2-6 wt%, tertiary amine-type polymerizable monomer is 2-6 wt%, and the sum of the mass percentages of all components is 100 wt%.

[0019] Preferably, the acrylate copolymer shell is formed by two-stage seed emulsion polymerization. In the first stage, the polymerizable monomers added account for 70-85 wt% of the total shell monomers, and in the second stage, the polymerizable monomers added account for 15-30 wt% of the total shell monomers. Both the benzophenone-type polymerizable monomer and the tertiary amine-type polymerizable monomer are added in the second stage.

[0020] The aliphatic polyurethane acrylate B has an average polymerizable functionality of 4–10 and a viscosity of 1000–8000 mPa·s at 25°C.

[0021] The monofunctional active diluent C is selected from one or more of isoborneol methacrylate, isoborneol acrylate, and acrylomorpholine.

[0022] The bifunctional active diluent D is selected from one or both of 1,6-hexanediol diacrylate and tripropylene glycol diacrylate.

[0023] The bulk photoinitiator E is selected from one or more of TPO-L, TPO, and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.

[0024] The additive F is selected from one or more of leveling agents, defoamers, and adhesion promoters.

[0025] Secondly, the present invention provides a process for preparing an LCD diffusion film, comprising the following steps:

[0026] (1) Mix aliphatic polyurethane acrylate, reactive diluent, bulk photoinitiator and additives, add shell-fixed photoinitiating core-shell light-diffusing particles and disperse them evenly, then add organic solvent to obtain coating composition;

[0027] (2) The coating composition is coated onto the surface of an optical-grade PET substrate that has been corona-treated to form a wet film;

[0028] (3) Within 2 to 8 seconds after coating, the wet film is pre-cured with 365nm UV light in a nitrogen atmosphere with an oxygen content of not more than 1000ppm.

[0029] (4) Dry the pre-cured wet film at 50-85°C for 1.5-4 min;

[0030] (5) The dried coating is cured by UV light of 385-405nm.

[0031] The irradiation intensity in step (3) is 20–80 mW / cm². 2 The irradiation energy is 10–20 mJ / cm². 2 The preferred irradiance intensity is 40–60 mW / cm². 2 The irradiation energy is 12–18 mJ / cm². 2 .

[0032] The main curing light intensity in step (5) is 400–1200 mW / cm². 2 The primary curing energy is 600–1000 mJ / cm². 2 .

[0033] During low-dose irradiation at 365 nm, bulk photoinitiators can also participate in the photoinitiation reaction of the resin phase. This invention is not based on the premise that 365 nm irradiation only excites shell-fixed photoinitiating units.

[0034] The benzophenone-type photoinitiating unit and the tertiary amine synergistic unit fixed in the particle shell are used to provide additional local free radical sources for the particle neighborhood region on the basis of limited prepolymerization in the bulk phase, which is beneficial to improve the local initiation probability and prepolymerization degree in the particle neighborhood region.

[0035] The tertiary amine cooperating unit can serve as an electron donor and a hydrogen donor, thereby improving the efficiency of free radical generation by the benzophenone-type photoinitiator.

[0036] Thirdly, the present invention provides an LCD diffusion film comprising an optical-grade PET substrate and a UV-curable diffusion coating located on the surface of the substrate.

[0037] The UV-curable diffusion coating contains 15-25 wt% of shell-fixed photoinitiating core-shell photodiffusion particles, which comprise a polymethylsilsesquioxane core and an acrylate copolymer shell. The shell contains copolymerized and fixed benzophenone-type photoinitiating units and tertiary amine synergistic units.

[0038] Preferably, the

[0039] Compared with the prior art, the embodiments of this application have the following main advantages:

[0040] This invention copolymerizes and fixes benzophenone-type photoinitiating units and tertiary amine synergistic units in the acrylate copolymer shell of the same core-shell light-diffusing particle, reducing the migration risk caused by the separate addition of free tertiary amine synergist, and providing an additional source of local free radicals in the vicinity of the particle.

[0041] The present invention implements low-dose pre-curing in the wet film stage, which is beneficial to improve the prepolymerization degree of the particle adjacent area and reduce the degree of relative displacement of particles in the subsequent drying stage.

[0042] By limiting the pre-curing energy of the wet film and performing drying and main curing after pre-curing, it is possible to balance particle distribution uniformity and solvent removal. Attached Figure Description

[0043] Figure 1 This is a schematic diagram of the structure of a core-shell photodiffusing particle with a fixed shell.

[0044] Figure 2 This is a schematic diagram of the process sequence for wet film pre-curing, drying, and main curing. Detailed Implementation

[0045] Unless otherwise stated, all percentages are by mass; refractive index is the value at 25°C and 589 nm.

[0046] Preparation Example 1: Shell-immobilized photoinitiated core-shell photodiffusing particles A1

[0047] (1) Seed treatment

[0048] Take 100.0g of polymethylsilsesquioxane microspheres. The volume average particle size (nominal value of raw material) is 3.0μm, the measured laser particle size Dv is 3.12μm, and the refractive index is 1.43.

[0049] The microspheres were added to a mixture of 500g ethanol / water at a mass ratio of 1:1, and 2.0g γ-methacryloyloxypropyltrimethoxysilane was added. The pH was adjusted to 4.5-5.0 with acetic acid, and the mixture was stirred at 60°C for 3 hours.

[0050] The mixture was filtered, washed twice with ethanol, and dried under vacuum at 50°C to obtain seed microspheres with polymerizable double bonds on their surface.

[0051] (2) First stage shell aggregation

[0052] The above-mentioned seed microspheres, 500g of deionized water and 1.5g of polyoxyethylene alkyl ether were added to the reactor, and nitrogen gas was introduced to replace the air before the temperature was raised to 75°C.

[0053] 13.4 g of methyl methacrylate, 6.2 g of butyl acrylate, 0.4 g of ethylene glycol dimethacrylate, 0.30 g of polyoxyethylene alkyl ether, and 70 g of deionized water were pre-emulsified to obtain the first monomer pre-emulsion.

[0054] Separately, 0.12 g of potassium persulfate was dissolved in 10 g of deionized water to obtain an aqueous solution of the first initiator.

[0055] The first monomer preemulsion and the first initiator aqueous solution were added dropwise to the reactor separately and simultaneously over a period of 2 hours, with the pH of the system controlled at 6.5–7.0 during the addition. After the addition was completed, the mixture was kept at 75°C for 2 hours to obtain the first-stage core-shell particle dispersion.

[0056] (3) Second-stage functional shell aggregation

[0057] 0.55 g of 4-methacryloyloxybenzophenone and 0.06 g of ethylene glycol dimethacrylate were dissolved in 3.54 g of methyl methacrylate and 1.30 g of butyl methacrylate, and then 0.55 g of dimethylaminoethyl methacrylate was added to obtain the second-stage oil phase.

[0058] The second stage oil phase, 0.10 g of polyoxyethylene alkyl ether, and 25 g of deionized water were homogenized at 8000–12000 rpm for 5–10 min to obtain the second monomer preemulsion.

[0059] Separately, 0.04 g of potassium persulfate was dissolved in 10 g of deionized water to obtain an aqueous solution of the second initiator.

[0060] Before adding the droplets, the pH of the first-stage core-shell particle dispersion was adjusted to 8.5–9.0 using a 5% sodium hydroxide aqueous solution.

[0061] The second monomer preemulsion and the second initiator aqueous solution were added dropwise to the first-stage core-shell particle dispersion separately and simultaneously over a period of 1 hour, maintaining the pH of the system at 8.5–9.0 during the addition. After the addition was completed, the mixture was kept at 75°C for 2 hours.

[0062] The particles were filtered, washed three times with deionized water, then washed once with ethanol, and dried under vacuum at 50°C to constant weight to obtain shell-fixed photoinitiated core-shell photodiffusion particles A1.

[0063] The total amount of polymerizable monomers in the first stage is 20.0 g, the total amount of polymerizable monomers in the second stage is 6.0 g, and the total amount of shell monomers is 26.0 g. The monomers in the first stage and the second stage account for 76.9 wt% and 23.1 wt% of the total shell monomers, respectively.

[0064] The total amount of shell monomers is 2.1 wt% for both 4-methacryloyloxybenzophenone and dimethylaminoethyl methacrylate.

[0065] TEM was used to statistically analyze 50 particles. The average diameter of the A1 nucleus was 2.96 μm with a standard deviation of 0.08 μm; the average outer diameter of the core-shell particles was 3.22 μm with a standard deviation of 0.09 μm; and the average radial shell thickness was 128 nm with a standard deviation of 12 nm.

[0066] Based on the amount of feed, the amount of 4-methacryloyloxybenzophenone is equivalent to 0.016 mmol / g (based on the theoretical total mass of polymethylsilsesquioxane core and shell monomers), and the amount of dimethylaminoethyl methacrylate is equivalent to 0.028 mmol / g.

[0067] XPS analysis of A1 after Soxhlet extraction with ethyl acetate revealed a tertiary amine nitrogen signal. Solid-state nuclear magnetic resonance analysis detected a benzophenone structural signal, indicating that benzophenone-type photoinitiating units and tertiary amine cooperating units still exist in the extracted particles.

[0068] Preparation Example 2: Blank Core-Shell Particles A0

[0069] Similar to Preparation Example 1, except that in the second stage of functional shell polymerization, 1.10 g of methyl methacrylate was used instead of 0.55 g of 4-methacryloyloxybenzophenone and 0.55 g of dimethylaminoethyl methacrylate, while other conditions remained unchanged, to obtain A0.

[0070] The total amount of material added to the shell layer in the second stage of A0 is the same as that in A1, but no benzophenone-type polymerizable monomers or tertiary amine-type polymerizable monomers are added in the second stage.

[0071] Preparation Example 3: Single benzophenone shell particles A-BP

[0072] Similar to Preparation Example 1, except that in the second stage of functional shell polymerization, 0.55g of methyl methacrylate was used instead of 0.55g of dimethylaminoethyl methacrylate, while other conditions remained unchanged, to obtain A-BP.

[0073] In the second stage of A-BP, benzophenone-type polymerizable monomers were added, but tertiary amine-type polymerizable monomers were not added.

[0074] Preparation Example 4: Single Tertiary Amine Shell Particles A-AM

[0075] Similar to Preparation Example 1, except that in the second stage of functional shell polymerization, 0.55g of methyl methacrylate was used instead of 0.55g of 4-methacryloyloxybenzophenone, while other conditions remained unchanged, to obtain A-AM.

[0076] In the second stage of A-AM, tertiary amine polymerizable monomers were added, but benzophenone polymerizable monomers were not added.

[0077] Example 1

[0078] Based on 100 parts by weight of the total non-volatile components of the coating, add 20 parts of A1, 40 parts of aliphatic polyurethane acrylate with an average polymerizable functionality of 6, 25 parts of isobornyl methacrylate, 12 parts of 1,6-hexanediol diacrylate, 2.5 parts of TPO-L and 0.5 parts of silicone leveling agent.

[0079] Aliphatic polyurethane acrylate, isobornyl methacrylate, 1,6-hexanediol diacrylate, TPO-L and leveling agent are mixed evenly at 30-35℃. After adding Al, the mixture is dispersed at 300-500 rpm for 30-45 min. Then, 90 parts of ethyl acetate and 60 parts of butanone are added to obtain a coating liquid with a solid content of 40 wt%.

[0080] Use after filtration through a 20–50 μm filter. The viscosity of the coating solution at 25°C is 260 mPa·s.

[0081] The coating liquid was applied to a corona-treated optical-grade PET substrate with a surface tension of 44 dyn / cm using a slot coating method, resulting in a wet film thickness of 45 μm.

[0082] Five seconds after coating, the wet film was pre-cured using a 365nm LED under a nitrogen atmosphere with an oxygen content not exceeding 1000ppm, with an irradiation intensity of 50mW / cm². 2 The irradiation energy is 15 mJ / cm. 2 .

[0083] The wet film was then dried sequentially through drying tunnels at 65°C and 80°C, with a total drying time of 3 minutes.

[0084] Curing was performed using a 395nm LED under a nitrogen atmosphere with an oxygen content not exceeding 1000ppm, with an irradiation intensity of 800mW / cm². 2 The irradiation energy is 800 mJ / cm. 2 .

[0085] The coating thickness after curing is 16μm.

[0086] Example 2

[0087] Based on 100 parts by weight of the total non-volatile components of the coating, add 24 parts of A1, 38 parts of aliphatic polyurethane acrylate with an average polymerizable functionality of 6, 24 parts of isobornyl methacrylate, 12 parts of tripropylene glycol diacrylate, 1.5 parts of TPO-L and 0.5 parts of silicone leveling agent.

[0088] Add 90 parts of ethyl acetate and 60 parts of butanone, and prepare the coating solution according to the method in Example 1. The viscosity of the coating solution at 25°C is 310 mPa·s.

[0089] The coating, drying, and primary curing were performed according to the method in Example 1, except that the wet film pre-curing light intensity was 60 mW / cm². 2 The irradiation energy is 18 mJ / cm. 2 .

[0090] The coating thickness after curing is 17μm.

[0091] Example 3

[0092] Based on 100 parts by weight of the total non-volatile components of the coating, add 16 parts of A1, 44 parts of aliphatic polyurethane acrylate with an average polymerizable functionality of 6, 25 parts of acrylamide morpholine, 13 parts of 1,6-hexanediol diacrylate, 1.5 parts of TPO-L and 0.5 parts of silicone leveling agent.

[0093] Add 90 parts of ethyl acetate and 60 parts of butanone, and prepare the coating solution according to the method in Example 1. The viscosity of the coating solution at 25°C is 220 mPa·s.

[0094] The coating, drying, and primary curing were performed according to the method in Example 1, except that the wet film pre-curing light intensity was 50 mW / cm² and the irradiation energy was 12 mJ / cm². 2 .

[0095] The coating thickness after curing is 15μm.

[0096] Comparative Example 1: Blank particle A0

[0097] Replace A1 in Example 1 with A0, and keep the other formulations and process conditions the same as in Example 1.

[0098] Comparative Example 2: Single benzophenone shell particles A-BP

[0099] Replace A1 in Example 1 with A-BP, and keep the other formulations and process conditions the same as in Example 1.

[0100] Comparative Example 3: Single Tertiary Amine Shell Particles A-AM

[0101] Replace A1 in Example 1 with A-AM, and keep the other formulations and process conditions the same as in Example 1.

[0102] Comparative Example 4: Elimination of wet film pre-curing

[0103] Using the formulation of Example 1, the coating was dried directly, and then only 395nm primary curing was performed.

[0104] Comparative Example 5: Pre-curing energy too high

[0105] Using the formulation of Example 1, the wet film pre-curing was performed at 365nm and 50mW / cm.2 60mJ / cm 2 Other conditions are the same as in Example 1.

[0106] Comparative Example 6: Pre-curing after drying

[0107] Using the formulation of Example 1, after coating, the material was first dried in ovens at 65°C and 80°C for 3 minutes, and then subjected to a 365nm, 50mW / cm2 drying process. 2 15mJ / cm 2 Irradiation was performed, followed by 395nm, 800mW / cm 2 800mJ / cm 2 Perform primary curing.

[0108] Detection methods

[0109] Particle structure

[0110] The volume average particle size of the core-shell particles was determined using a laser particle size analyzer. At least 50 particles were observed using TEM, and the nucleus diameter, outer diameter of the core-shell particles, and radial shell thickness were statistically analyzed. The arithmetic mean and standard deviation were reported.

[0111] Functional structure confirmed

[0112] The dried particles were subjected to Soxhlet extraction with ethyl acetate until 4-methacryloyloxybenzophenone and dimethylaminoethyl methacrylate were not detected by HPLC in two consecutive extracts.

[0113] XPS was used to detect the nitrogen-containing structure of the extracted particles, and solid-state NMR or pyrolysis gas chromatography-mass spectrometry was used to detect the benzophenone structure of the extracted particles. These detections were used to assist in confirming the retention of the functional structure in the extracted particles and were not used as quantitative methods for the covalent fixation of functional units.

[0114] Shell refractive index

[0115] A monomer mixture with the same composition was prepared according to the mass ratio of all shell monomers in the first and second stages. After being polymerized into a transparent film, the refractive index was measured using an Abbe refractometer at 25°C and 589 nm, which was used as the characterization value of the shell refractive index.

[0116] wet film prepolymerization degree

[0117] A bulk prepolymer control wet film was prepared by replacing A1 in the test formulation with an equal mass of A0, while keeping other resin phases, solvent composition, wet film thickness, atmosphere, light source distance and irradiation conditions the same.

[0118] The bulk prepolymerized control wet film was tested using real-time FTIR at 1635 cm⁻¹. -1 The nearby acrylate double bond peak and 1720 cm⁻¹-1 The double bond conversion rate is calculated from the area ratio of the carbonyl peak. This conversion rate is used to evaluate the limited prepolymerization degree of the wet film bulk phase under pre-curing conditions.

[0119] Particle thickness distribution

[0120] After the cured film was subjected to liquid nitrogen embrittlement, cross-sectional SEM observation was performed. The coating thickness direction was divided into three regions: the substrate side, the middle part, and the air side. At least 10 fields of view were observed in each region.

[0121] The particle area fraction in each region was statistically analyzed using the same magnification, grayscale threshold, and image segmentation parameters. The particle thickness distribution was evaluated by the ratio of the particle area fraction on the substrate side to the particle area fraction on the air side. Three different cross-sectional locations were selected for each sample, and the arithmetic mean of the measurement results at the three locations was reported.

[0122] Residual solvent

[0123] Residual ethyl acetate and butanone were determined by headspace gas chromatography after drying and before primary curing. The residual solvent content was calculated based on the dry coating mass, with a method limit of quantitation of 5 ppm.

[0124] Optical performance

[0125] Total light transmittance was determined according to JIS K7361, and haze was determined according to JIS K7136. Three independent samples were taken for each sample, and the mean and standard deviation were reported.

[0126] Test Results

[0127] Table 1 Particle structure parameters

[0128] Note: The amount of BPMA and DMAEMA fed is calculated by dividing the number of moles of functional monomers by the theoretical total mass of polymethylsilsesquioxane core and shell monomers.

[0129] Table 2 Validation of wet film pre-curing process window

[0130] Note: For bulk prepolymerized control wet films, A0 of equal mass is used to replace A1 in the corresponding formulation.

[0131] Table 3. Test results of the diffusion film

[0132] Note: Transmittance and haze are the average ± standard deviation of three independent samples; particle area ratio is the arithmetic mean of the results measured at three different cross-sectional locations.

[0133] Results Analysis

[0134] The particle area ratio of the substrate side to the air side in Examples 1 to 3 is 1.05 to 1.08, which is closer to 1, indicating that the particle thickness direction is more uniformly distributed.

[0135] Comparative Example 1 uses A0 instead of A1, with a particle area ratio of 1.72. A0 does not have an additional local free radical source provided by the shell-fixed photoinitiating unit, and its wet film prepolymerization is mainly initiated by the bulk photoinitiator.

[0136] Comparative Example 2 used A-BP with only benzophenone-type polymerizable monomers added, and its particle area ratio was 2.10; Comparative Example 3 used A-AM with only tertiary amine-type polymerizable monomers added, and its particle area ratio was 1.68. Neither A-BP nor A-AM exhibited the particle proximity region additional initiation effect present in A1.

[0137] The particle area ratio of A1 is significantly closer to 1 than that of A0, A-BP, and A-AM. This result supports the role of the benzophenone-type photoinitiating unit and the tertiary amine cooperating unit in the shell in improving the particle distribution.

[0138] Comparative Example 4, which eliminated wet film pre-curing, had a particle area ratio of 2.35, indicating that eliminating wet film pre-curing increased the degree of vertical migration of particles during the drying process.

[0139] Comparative Example 6, after drying, underwent 365 nm irradiation, and its particle area ratio was 1.95, still significantly higher than that of Example 1. This result supports the role of low-dose pre-curing during the wet film stage in reducing vertical particle migration.

[0140] Comparative Example 5 increased the wet film pre-curing energy to 60 mJ / cm², achieving a particle area ratio of 1.25, but with a residual solvent content of 268 ppm. The double bond conversion rate of the corresponding bulk prepolymerized control wet film was 16.8%. These results indicate that while excessively high pre-curing energy can reduce the relative displacement of particles, it is detrimental to subsequent solvent removal.

[0141] The above results indicate that by immobilizing benzophenone-type photoinitiating units and tertiary amine synergistic units in the shell and employing controlled low-dose UV irradiation before drying, the relative displacement of light-diffusing particles during the wet film drying stage can be reduced while maintaining subsequent solvent removal conditions.

[0142] Polymethylsilsesquioxane microspheres, methyl methacrylate, butyl acrylate, ethylene glycol dimethacrylate, 4-methacryloyloxybenzophenone, dimethylaminoethyl methacrylate, aliphatic polyurethane acrylate, TPO-L, PET, and the organic solvents mentioned above are all commercially available.

[0143] Seed emulsion polymerization, microgravure or slot coating, nitrogen protection, LED irradiation, and oven drying can all be completed using existing equipment, making it industrially applicable.

[0144] It should be noted that, for the sake of simplicity, the foregoing embodiments are all described as a series of actions. However, those skilled in the art should understand that the present invention is not limited to the described order of actions, as some steps may be performed in other orders or simultaneously according to the present invention. Furthermore, those skilled in the art should also understand that the embodiments described in the specification are preferred embodiments, and the actions and modules involved are not necessarily essential to the present invention.

Claims

1. An LCD diffuser film UV coating composition characterized in that, Based on a total of 100 parts by weight of non-volatile components in the coating, it includes 15-25 parts by weight of shell-fixed photoinitiating core-shell photodiffusing particles, 35-45 parts by weight of aliphatic polyurethane acrylate, 20-30 parts by weight of monofunctional reactive diluent, 8-15 parts by weight of bifunctional reactive diluent, 1-2.5 parts by weight of bulk photoinitiator, and 0.2-1 parts by weight of additives. The coating also includes 120 to 170 parts by weight of organic solvent, relative to 100 parts by weight of the non-volatile components. The shell-fixed photoinitiated core-shell photodiffusing particle comprises a polymethylsilsesquioxane core and an acrylate copolymer shell covering the outside of the core. The average TEM diameter of the core is 2.8–3.2 μm, and the average TEM thickness of the shell is 115–145 nm. The acrylate copolymer shell is formed by copolymerization of methyl methacrylate, butyl acrylate, ethylene glycol dimethacrylate, benzophenone-type polymerizable monomers and tertiary amine-type polymerizable monomers; The benzophenone-type polymerizable monomer is 4-methacryloyloxybenzophenone and / or 4-acryloyloxybenzophenone, and the tertiary amine-type polymerizable monomer is dimethylaminoethyl methacrylate. Apart from the tertiary amine synergist units copolymerized and immobilized in the shell, the composition does not contain a free tertiary amine photoinitiator synergist.

2. The LCD diffuser film UV coating composition of claim 1, wherein, Based on the total amount of all polymerizable monomers forming the acrylate copolymer shell, methyl methacrylate is 55-75 wt%, butyl acrylate is 20-35 wt%, ethylene glycol dimethacrylate is 0.5-2 wt%, benzophenone-type polymerizable monomer is 2-6 wt%, tertiary amine-type polymerizable monomer is 2-6 wt%, and the sum of the mass percentages of all components is 100 wt%.

3. The LCD diffuser film UV coating composition of claim 1, wherein, The acrylate copolymer shell is formed by two-stage seed emulsion polymerization. In the first stage, the polymerizable monomers added account for 70-85 wt% of the total shell monomers, and in the second stage, the polymerizable monomers added account for 15-30 wt% of the total shell monomers. Both the benzophenone-type polymerizable monomer and the tertiary amine-type polymerizable monomer are added in the second stage.

4. The LCD diffuser film UV coating composition of claim 1, wherein, The aliphatic polyurethane acrylate has an average polymerizable functionality of 4 to 10 and a viscosity of 1000 to 8000 mPa·s at 25°C. The monofunctional active diluent is one or more of isoborneol methacrylate, isoborneol acrylate, and acrylmorpholine; The bifunctional active diluent is 1,6-hexanediol diacrylate and / or tripropylene glycol diacrylate.

5. The LCD diffuser film UV coating composition of claim 1, wherein, The bulk photoinitiator is one or more of TPO-L, TPO, and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide; the additive is one or more of leveling agent, defoamer, and adhesion promoter; and the organic solvent is one or more of ethyl acetate, butanone, and propylene glycol methyl ether acetate.

6. A process for preparing an LCD diffusion film, characterized by, Includes the following steps: (1) The LCD diffusion film UV coating composition according to any one of claims 1 to 5 is coated on the surface of an optical grade PET substrate that has been corona treated to form a 30-55 μm wet film; (2) within 2-8 seconds after coating, irradiating the wet film with 365 nm UV light in a nitrogen atmosphere with an oxygen content of not higher than 1000 ppm, the irradiation light intensity being 20-80 mW / cm 2 , and the irradiation energy being 10-20 mJ / cm 2 ; (3) Dry the wet film treated in step (2) at 50-85°C for 1.5-4 min; (4) The coating after drying is subjected to main curing with 385-405 nm UV light, the main curing light intensity is 400-1200 mW / cm 2 , and the main curing energy is 600-1000 mJ / cm 2 .

7. The LCD diffusion film manufacturing process of claim 6, wherein, The irradiation light intensity of step (2) is 40-60 mW / cm 2 , the irradiation energy is 12-18 mJ / cm 2 ; the drying temperature of step (3) is 60-80℃, and the drying time is 2-3.5 min.

8. The LCD diffusion film manufacturing process of claim 6, wherein, The surface tension of the PET substrate after corona treatment is not less than 42 dyn / cm. The coating is done by microgravure coating or slot coating. The main curing in step (4) is carried out in a nitrogen atmosphere with an oxygen content of not more than 1000 ppm.

9. The LCD diffusion film manufacturing process of claim 6, wherein, The wet film thickness is 35–45 μm, and the coating thickness after curing is 14–18 μm.

10. An LCD diffusion film comprising an optical grade PET substrate and a UV cured diffusion coating on the surface of the substrate, characterized in that, The UV-curable diffusion coating contains shell-fixed photoinitiated core-shell photodiffusion particles accounting for 15-25 wt% of the dry mass of the UV-curable diffusion coating; The shell-fixed photoinitiating core-shell light-diffusing particles include a polymethylsilsesquioxane core with an average TEM diameter of 2.8–3.2 μm and an acrylate copolymer shell with an average TEM thickness of 115–145 nm. The acrylate copolymer shell contains benzophenone-type photoinitiating units and tertiary amine co-units.