Conductive-lubricating integrated coating and its preparation method and space moving parts
By establishing conductive pathways between spacecraft structures through an integrated conductive-lubricating coating, the problems of poor electrical conductivity and static electricity accumulation caused by traditional coatings are solved. This achieves an organic integration of static discharge and lubrication performance, simplifies the system structure, and improves reliability and safety.
Patent Information
- Application Number
- CN202611212034.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-11
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional solid lubricant coating materials are insulators, resulting in poor electrical conductivity between spacecraft structures, which cannot meet the requirements for electrostatic discharge and potential equalization. Furthermore, the addition of extra grounding wires and conductive bonding plates increases system complexity and motion resistance.
The conductive-lubricating integrated coating structure, consisting of a conductive layer, a conductive-lubricating transition layer, and a lubricating layer from the inside out, is adopted. The conductive network is formed by curing a polyimide resin system, which realizes the organic integration of charge conduction and lubrication performance, and avoids the need for additional grounding devices.
This technology enables the direct establishment of a stable conductive path on the contact surface of the friction pair, meeting the requirements for electrostatic discharge and friction wear control, simplifying the system structure, reducing weight, lowering the risk of electrostatic accumulation and discharge, and improving reliability and safety.
Smart Images

Figure CN123107534A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of solid lubricant coating technology, and in particular to a conductive-lubricating integrated coating, its preparation method, and a space motion component. Background Technology
[0002] As a key actuator for attitude control, energy acquisition, and payload pointing functions, the reliability of spacecraft motion mechanisms directly determines the success or failure of the entire mission. In a vacuum environment, to reduce friction and wear during motion and prevent vacuum cold welding effects, a solid lubricant coating is typically applied to the surface of the mechanism. However, traditional solid lubricant coating materials are generally insulators, resulting in extremely low surface conductivity. This makes it impossible to establish an effective charge conduction path during application, leading to uneven potential distribution between spacecraft structures and making it difficult to meet the stringent requirements for electrostatic discharge and potential equalization.
[0003] As spacecraft evolve towards higher integration, lighter weight, and longer lifespan, the demand for internal electrical connections within space mechanisms has increased significantly. Existing solutions often rely on adding dedicated grounding wires and conductive bonding pads to achieve electrical connections between structural units. This approach has revealed multiple drawbacks in practical applications: the additional cables not only significantly increase the complexity and overall weight of the system structure but are also prone to snagging during flexible movements, leading to increased motion resistance and affecting the dynamic accuracy of the mechanism; furthermore, the installation and maintenance of these cables significantly increases the difficulty of system integration and the workload of assembly. Summary of the Invention In view of this, the purpose of this application is to provide an integrated conductive-lubricating coating and its preparation method, which has excellent conductivity and lubrication properties, can simultaneously meet the requirements of static discharge and friction and wear control, effectively reduce the use of additional grounding wires and conductive lap pieces in space motion mechanisms, thereby simplifying the system structure, reducing weight, and improving reliability and safety; Another objective of this application is to provide a spatial motion component based on the aforementioned conductive-lubricating integrated coating, which enables the direct establishment of a stable conductive path on the contact surface of the friction pair, thereby achieving real-time discharge and uniform distribution of charge, fundamentally reducing the risk of static electricity accumulation and discharge, while possessing excellent and stable lubrication performance.
[0004] In order to solve the above-mentioned technical problems / achieve the above-mentioned objectives, or at least partially solve the above-mentioned technical problems / achieve the above-mentioned objectives, as a first aspect of this application, a conductive-lubricating integrated coating is provided, which includes a conductive layer, a conductive-lubricating transition layer and a lubricating layer from the inside to the outside. The conductive layer comprises 10-20 parts by weight of polyimide resin and 10-25 parts by weight of a first conductive agent; The conductive-lubricating transition layer comprises 10-20 parts by weight of polyimide resin, 10-21 parts by weight of a second conductive agent, 5-20 parts by weight of a first lubricant, and 1-5 parts by weight of a lubricating additive. The lubricating layer comprises 5-15 parts by weight of fluorinated polyimide resin, 5-20 parts by weight of a second lubricant, and 5-15 parts by weight of a third conductive agent.
[0005] Optionally, the first conductive agent, the second conductive agent, and the third conductive agent are each independently selected from one or more of silver, graphite, graphene, and conductive carbon black; the first lubricant and the second lubricant are each independently selected from molybdenum disulfide and / or polytetrafluoroethylene; and the lubricating additive is selected from antimony trioxide.
[0006] Further optionally, the first conductive agent includes silver, graphene, and conductive carbon black; the second conductive agent includes silver and graphite; and the third conductive agent includes graphite. Both the first and second lubricants include molybdenum disulfide and polytetrafluoroethylene.
[0007] Further optionally, the first conductive agent comprises 10-20 parts by weight of silver, 0.5-1.5 parts by weight of graphene, and 1-3 parts by weight of conductive carbon black; the second conductive agent comprises 8-16 parts by weight of silver and 2-5 parts by weight of graphite; and the third conductive agent comprises 6-12 parts by weight of graphite. The first lubricant comprises 5-10 parts by weight of molybdenum disulfide and 2-6 parts by weight of polytetrafluoroethylene; and the second lubricant comprises 4-8 parts by weight of molybdenum disulfide and 4-10 parts by weight of polytetrafluoroethylene.
[0008] Further optionally, the silver comprises flake silver powder with a particle size of 0.5~3μm; the graphene comprises few-layer graphene with 1~10 layers and a sheet size of 0.5~5μm; the graphite comprises flake graphite with a particle size of 0.5~3μm; and the conductive carbon black comprises high-structure conductive carbon black with a specific surface area of 200~1500m². 2 / g; the particle size of the molybdenum disulfide is 0.3~2μm; the particle size of the polytetrafluoroethylene is 1~3μm; the particle size of the antimony trioxide is 0.5~1.5μm.
[0009] Optionally, the thickness of the conductive layer is controlled at 4~8μm; the thickness of the conductive-lubricating transition layer is 2~5μm; the thickness of the lubricating layer is 3~7μm; and the total thickness of the integrated conductive-lubricating coating is 9~20μm.
[0010] As a second aspect of this application, a method for preparing a conductive-lubricating integrated coating as described in this application is provided, comprising: Weigh out the conductive layer raw materials according to the proportions and mix them thoroughly with the solvent and dispersant to obtain the conductive layer slurry; Weigh out the conductive-lubricating transition layer raw materials according to the proportion and mix them thoroughly with solvent and defoamer to obtain conductive-lubricating transition layer slurry. Weigh out the lubricating layer raw materials according to the proportions and mix them thoroughly with the solvent and defoamer to obtain the lubricating layer slurry. A conductive layer, a conductive-lubricating transition layer, and a lubricating layer are sequentially sprayed from the inside out. During the spraying process, the next layer is sprayed after each layer is surface dry. After the lubricating layer is surface dry, it is heated and cured to obtain the integrated conductive-lubricating coating.
[0011] Optionally, the dispersant includes one or more of BYK-9076, BYK-190, and BYK-111; the solvent includes one or more of N-methylpyrrolidone, N,N-dimethylformamide, and dimethylacetamide; and the defoamer includes one or more of BYK-065, BYK-066N, and BYK-141.
[0012] As a third aspect of this application, a space motion component is provided, including a first metal substrate, the surface of which is provided with the conductive-lubricating integrated coating described in this application.
[0013] Optionally, it includes a first metal substrate and a second metal substrate. The surface of the first metal substrate is provided with the conductive-lubricating integrated coating described in this application. The second metal substrate is disposed opposite to the first metal substrate and forms a friction pair. When the first metal substrate and the second metal substrate move relative to each other and generate friction, at least a portion of the lubricating layer of the conductive-lubricating integrated coating is transferred to the surface of the second metal substrate to form a conductive-lubricating interface.
[0014] This application achieves the organic integration of conductivity and lubrication functions through a structural design that sequentially stacks a conductive layer, a conductive-lubricating transition layer, and a lubricating layer from the inside out. It can simultaneously establish an effective charge conduction path to meet the requirements of static discharge and provide stable friction and wear control. This avoids the reliance on additional grounding wires and conductive bonding plates in traditional solutions, and has excellent conductivity and lubrication performance. It significantly simplifies the system structure, reduces weight, lowers assembly difficulty and maintenance costs, and effectively eliminates the risk of discharge caused by static accumulation. Attached Figure Description
[0015] Figure 1 The diagram shown is a schematic representation of the integrated conductive-lubricating coating of this application. Figure 2 The image shown is a physical appearance of the conductive-lubricating integrated coating of this application; Figure 3 The image shown is an SEM image of the conductive-lubricating integrated coating of this application. Detailed Implementation
[0016] This application discloses an integrated conductive-lubricating coating and its preparation method, as well as a space motion component. Those skilled in the art can refer to the content of this document and appropriately modify the process parameters to achieve the desired result. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art and are considered to be included in this application. The products, processes, and applications described in this application have been described through preferred embodiments. Those skilled in the art can obviously modify or appropriately change and combine the preparation methods described herein without departing from the content, spirit, and scope of this application to realize and apply the technology of this application. Obviously, the described embodiments are only some, not all, of the embodiments of this application. All other embodiments obtained by those skilled in the art based on the embodiments in this application without creative effort are within the scope of protection of this application.
[0017] It should be noted that, in this document, relational terms such as "first" and "second," "step 1" and "step 2," and "(1)" and "(2)" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element. Moreover, the embodiments and features described in this application can be combined with each other without conflict.
[0018] Traditional space motion mechanism coatings typically use insulating materials for lubrication and cold welding prevention, resulting in poor electrical conductivity between structures and failing to meet the spacecraft's requirements for structural point balance and electrostatic discharge. Existing designs use dedicated grounding wires and conductive lap joints to ensure electrical connections, but this approach increases structural complexity, may lead to cable snagging during flexible movement, increases structural motion resistance, and significantly enhances system integration and assembly difficulties.
[0019] In response, the first aspect of this application proposes an integrated conductive-lubricating coating. This coating comprises, from the inside out, a conductive layer, a conductive-lubricating transition layer, and a lubricating layer, which are cured into an integrated functional coating. This integrated conductive-lubricating coating not only achieves an organic fusion of conductive and lubricating properties, but also, by using the same polyimide resin system to cure each layer into an organic whole, fundamentally eliminates clear physical interfaces, resulting in strong interlayer bonding and avoiding the risk of delamination. The functional components of each layer are cured within a unified three-dimensional network structure, enabling them to work synergistically and improving long-term reliability and durability. A structural schematic diagram is shown below. Figure 1 The conductive layer, composed of polyimide resin and a first conductive agent, provides the basic conductive path. The conductive-lubricating transition layer, composed of polyimide resin, a second conductive agent, a first lubricant, and a lubricating additive, combines conductive and lubricating functions. The lubricating layer, composed of fluorinated polyimide resin, a second lubricant, and a third conductive agent, provides friction-reducing and anti-wear properties while maintaining the conductivity of the friction interface. Thus, this coating meets the long-life lubrication requirements of space motion mechanisms without requiring additional external grounding devices. The conductive network within the coating enables electrical connections between structures, effectively simplifying system integration, reducing motion resistance, and fundamentally solving the aforementioned technical problems.
[0020] The conductive layer, serving as the bottom layer, comprises 10-20 parts by weight of polyimide resin and 10-25 parts by weight of a first conductive agent. The polyimide resin acts as a binder, providing mechanical support and adhesion to the coating. After curing, the coating exhibits high bonding strength to the metal substrate. Simultaneously, the polyimide resin also possesses lubricating properties, ensuring both filler adhesion and film formation. The first conductive agent is dispersed within the polyimide resin to form a conductive network. For example, the first conductive agent can be selected from conductive metal powders or carbon-based materials to ensure the conductive layer is conductive.
[0021] The conductive-lubricating transition layer, serving as an intermediate layer, comprises 10-20 parts by weight of polyimide resin, 10-21 parts by weight of a second conductive agent, 5-20 parts by weight of a first lubricant, and 1-5 parts by weight of a lubricating additive. This layer establishes a performance gradient between the conductive and lubricating layers. Using the same polyimide resin ensures consistency with the polyimide resin system of the underlayer and toplayer, guaranteeing uniform thermal deformation of each layer during curing and improving coating adhesion. The second conductive agent, together with the first conductive agent, maintains the conductive pathways within the coating. The first lubricant is introduced in this layer to initially provide lubrication and alleviate interlayer stress. For example, the first lubricant can be selected from solid lubricating particles with a low coefficient of friction. The lubricating additive is used to further optimize the tribological properties of the coating or improve the dispersion uniformity of the components. For example, the lubricating additive can be a compound with synergistic lubricating effects.
[0022] The lubricating layer, as the surface layer, comprises 5-15 parts by weight of fluorinated polyimide resin (e.g., trifluoromethyl polyimide resin), 5-20 parts by weight of a second lubricant, and 5-15 parts by weight of a third conductive agent. The fluorinated polyimide resin, while maintaining the high-temperature resistance, wear resistance, and mechanical strength of polyimide, utilizes fluorinated groups to reduce surface energy, hygroscopicity, and interfacial adhesion tendency, thereby enhancing the stability of the lubrication transfer film. The second lubricant provides the primary lubrication at the friction interface. For example, the second lubricant can be a self-lubricating polymer or a layered solid lubricant. The third conductive agent is used to ensure that the friction interface maintains real-time charge dissipation during movement, preventing static electricity accumulation. For example, the third conductive agent can be a conductive carbon material or metal powder.
[0023] In certain embodiments of this application, it is further proposed that the first conductive agent, the second conductive agent, and the third conductive agent are each independently selected from one or more of silver, graphite, graphene, and conductive carbon black; the first lubricant and the second lubricant are each independently selected from molybdenum disulfide and / or polytetrafluoroethylene; and the lubricating additive is selected from antimony trioxide. By specifically selecting the conductive agent, lubricant, and lubricating additive, not only is the coating able to simultaneously perform the dual functions of conductivity and lubrication in space motion mechanisms, but also the overall physicochemical properties of the coating are optimized through the synergistic effect of different materials, enabling it to better adapt to the complex working conditions of the space environment. This lays a crucial material selection basis for achieving a long lifespan and high reliability of the coating.
[0024] In certain embodiments of this application, in order to further ensure the synergistic stability of the conductive network and the lubricating film between the layers, this application further proposes that the first conductive agent in the conductive layer includes silver, graphene and conductive carbon black, the second conductive agent in the conductive-lubricating transition layer includes silver and graphite, and the third conductive agent in the lubricating layer includes graphite; the first lubricant in the conductive-lubricating transition layer and the second lubricant in the lubricating layer both include molybdenum disulfide and polytetrafluoroethylene.
[0025] In the conductive layer, the combined use of silver, graphene, and conductive carbon black utilizes the geometric complementarity of conductive materials of different dimensions to form a dense and highly conductive network at the bottom layer, providing a stable basis for current transmission for the overall coating.
[0026] In the conductive-lubricating transition layer, the main functions are interlayer bonding, performance gradient transition, and lubrication. The resistance requirement is lower than that of the conductive layer, thus reducing the type and amount of the second conductive agent and preventing a decrease in the proportion of the lubricating component. The combination of silver and graphite not only ensures the continuity of interlayer electrical conduction but also effectively alleviates stress concentration between the conductive and lubricating layers through the interlayer shear properties of graphite, acting as a buffer and enhancing the overall structural stability of the coating. In the lubricating component, molybdenum disulfide reduces friction through interlayer slippage in its layered structure and possesses good load-bearing and wear-resistant capabilities. Polytetrafluoroethylene (PTFE) has low surface energy and easily forms a continuous transfer film during friction, reducing adhesive friction. Antimony trioxide primarily serves as a wear-resistant synergist and structural stabilizing component, forming a composite friction film with molybdenum disulfide, inhibiting crack propagation, and extending wear life. The three lubricating components synergistically achieve the effect of "low friction, high load-bearing capacity, and long life."
[0027] In the lubricating layer, graphite acts as a conductive agent, working in conjunction with a composite lubrication system of molybdenum disulfide and polytetrafluoroethylene (PTFE). This ensures that, even in direct contact at the friction interface, the necessary charge discharge pathway is maintained while providing excellent friction-reducing and anti-wear properties. By uniformly defining both the first and second lubricants as a composite of molybdenum disulfide and PTFE, the uniform distribution and consistent migration characteristics of the lubricating components within the coating are ensured, effectively avoiding the risk of interlayer delamination due to component differences.
[0028] In certain embodiments of this application, a scheme for finely proportioning the components of each layer in the conductive-lubricating integrated coating is further proposed. The first conductive agent comprises 10-20 parts by weight of silver, 0.5-1.5 parts by weight of graphene, and 1-3 parts by weight of conductive carbon black; for example, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20 parts by weight of silver, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, or 1.5 parts by weight of graphene, and 1, 1.5, 2, 2.5, or 3 parts by weight of conductive carbon black. The second conductive agent comprises 8 to 16 parts by weight of silver and 2 to 5 parts by weight of graphite; for example, 8, 9, 10, 11, 12, 13, 14, 15 or 16 parts by weight of silver and 2, 2.5, 3, 3.5, 4, 4.5 or 5 parts by weight of graphite. The third conductive agent comprises 6 to 12 parts by weight of graphite; for example, 6, 7, 8, 9, 10, 11 or 12 parts by weight of graphite; The first lubricant comprises 5 to 10 parts by weight of molybdenum disulfide and 2 to 6 parts by weight of polytetrafluoroethylene; for example, 5, 6, 7, 8, 9 or 10 parts by weight of molybdenum disulfide and 2, 3, 4, 5 or 6 parts by weight of polytetrafluoroethylene. The second lubricant comprises 4 to 8 parts by weight of molybdenum disulfide and 4 to 10 parts by weight of polytetrafluoroethylene; for example, 4, 5, 6, 7 or 8 parts by weight of molybdenum disulfide and 4, 5, 6, 7, 8, 9 or 10 parts by weight of polytetrafluoroethylene.
[0029] By differentiating the weight ratio of components in each layer, a gradient distribution of conductivity and lubrication properties is achieved. This allows the coating to effectively protect the conductive network structure under frictional loads through the synergistic effect of the components in each layer, avoiding drastic resistance fluctuations caused by wear, thereby ensuring the electrical connection reliability of space moving parts during long-term operation.
[0030] In certain embodiments of this application, the present application further proposes the above-mentioned conductive-lubricating integrated coating, wherein the polyimide resin is a thermosetting polyimide resin with an average molecular weight of 1×10⁻⁶. 4 ~5×10 4 The glass transition temperature after curing is not lower than 250℃; the silver includes flake silver powder with a particle size of 0.5~3μm; the graphene includes few-layer graphene with 1~10 layers and a sheet diameter of 0.5~5μm; the graphite includes flake graphite with a particle size of 0.5~3μm; the conductive carbon black includes high-structure conductive carbon black with a specific surface area of 200~1500m². 2 / g; the particle size of the molybdenum disulfide is 0.3~2μm; the particle size of the polytetrafluoroethylene is 1~3μm; the particle size of the antimony trioxide is 0.5~1.5μm.
[0031] In the coating composed of the aforementioned materials, the polyimide resin, after curing, possesses both extremely high bonding strength and excellent lubrication and friction-reducing properties, ensuring a low coefficient of friction and a long wear life. The flake-like silver powder exhibits excellent conductivity and primarily serves to form a low-resistance conductive framework. Few-layer graphene mainly connects the gaps between the silver powder particles, ensuring the coating's conductivity and providing some reinforcement. High-structure conductive carbon black, with its high specific surface area, fills tiny voids, supplementing conductivity and preventing power loss; additionally, conductive carbon black also provides some lubrication properties.
[0032] Precisely defining the particle size of molybdenum disulfide and polytetrafluoroethylene helps ensure their uniform dispersion in the coating, avoiding stress concentration or discontinuity in the lubricating film caused by excessively large particles, thereby forming a dense and durable lubrication transfer film on the friction pair surface. Defining the particle size of antimony trioxide aims to further ensure its uniform distribution in the conductive-lubricating transition layer, enabling it to fully exert its synergistic lubricating effect and thus extend the coating's service life.
[0033] In some embodiments of this application, a conductive-lubricating integrated coating is further proposed, wherein the thickness of the conductive layer is controlled at 4~8 μm; the thickness of the conductive-lubricating transition layer is 2~5 μm; the thickness of the lubricating layer is 3~7 μm; and the total thickness of the conductive-lubricating integrated coating is 9~20 μm. By optimizing and limiting the thickness of each layer and the total thickness of the coating, the coating ensures sufficient wear resistance life while avoiding risks such as decreased adhesion, excessive internal stress, or protection failure caused by excessive thickness or thinness. This provides reliable and durable charge discharge and lubrication protection for space motion components, significantly improving the reliability and service life of space motion mechanisms.
[0034] In a second aspect of this application, a method for preparing an integrated conductive-lubricating coating is also disclosed, comprising: Weigh out the conductive layer raw materials according to the proportions and mix them thoroughly with the solvent and dispersant to obtain the conductive layer slurry; Weigh out the conductive-lubricating transition layer raw materials according to the proportion and mix them thoroughly with solvent and defoamer to obtain conductive-lubricating transition layer slurry. Weigh out the lubricating layer raw materials according to the proportions and mix them thoroughly with the solvent and defoamer to obtain the lubricating layer slurry. A conductive layer, a conductive-lubricating transition layer, and a lubricating layer are sequentially sprayed from the inside out. During the spraying process, the next layer is sprayed after each layer is surface dry. After the lubricating layer is surface dry, it is heated and cured to obtain an integrated conductive-lubricating coating.
[0035] Among them, thorough mixing can be achieved by grinding methods such as ball milling to ensure that the materials are mixed evenly. For example, ZrO2 grinding balls with a particle size of 0.5mm can be added to a sand mill.
[0036] In certain embodiments of this application, this application further proposes that in the above preparation method, the dispersant includes one or more of BYK-9076, BYK-190, and BYK-111, the solvent includes one or more of N-methylpyrrolidone, N,N-dimethylformamide, and dimethylacetamide, and the defoamer includes one or more of BYK-065, BYK-066N, and BYK-141.
[0037] The solvent ensures that the polyimide resin is fully dissolved and forms a slurry with a suitable viscosity, providing a good leveling foundation for subsequent spraying processes. The dispersant effectively reduces the surface energy of the conductive and lubricating particles in the polyimide resin matrix, preventing particle agglomeration and ensuring a uniform distribution network of the conductive and lubricating phases within the coating. The defoamer effectively eliminates microbubbles generated during mixing and spraying, preventing residual pores after coating curing. The weight percentages of these components can be selected according to actual needs. These components decompose and volatilize during coating drying and curing, and are essentially not retained in the coating.
[0038] In some embodiments of this application, the composition of the conductive layer paste during preparation is as follows: Polyimide resin: 12-18 parts; Silver powder: 10-20 parts; Graphene: 0.5-1.5 parts; Conductive carbon black: 1-3 parts; Dispersant: 1-3 parts; Solvent: 55-70 parts; In some embodiments of this application, the composition of the slurry for the conductive-lubricating transition layer during preparation is as follows: Polyimide resin: 10-16 parts; Silver powder: 8-16 parts; Graphite: 2-5 parts; Molybdenum disulfide: 5-10 parts; Polytetrafluoroethylene: 2-6 parts; Antimony trioxide: 1-2.5 parts; Defoamer: 1-2 parts; Solvent: 50-70 parts; In some embodiments of this application, the composition of the lubricating layer slurry during preparation is as follows: Fluorinated polyimide resin: 8-12 parts; Molybdenum disulfide: 4-8 parts; Polytetrafluoroethylene: 4-10 parts; Graphite: 6-12 parts; Defoamer: 1-2 parts; Solvent: 50-70 parts.
[0039] In a third aspect, this application proposes a space motion component. This space motion component includes a first metal substrate, the surface of which is provided with the aforementioned conductive-lubricating integrated coating. According to the described functions and effects of the conductive-lubricating integrated coating, the space motion mechanism can achieve a synergistic effect of lubrication and electrical conduction, thereby effectively solving the risks of charge accumulation and electrostatic discharge caused by traditional coating insulation. Simultaneously, it avoids the problems of structural complexity, increased motion resistance, and high system integration difficulty caused by additional grounding cables, thus improving the reliability and integration of the space motion mechanism.
[0040] In some embodiments of this application, the bonding strength of the conductive-lubricating integrated coating reaches level 1 or above, the coefficient of friction of the coating is between 0.04 and 0.1 as tested by a ball-disc friction tester, the wear life is >150,000 revolutions, and the coating resistance is <20Ω as tested by a multimeter.
[0041] In some embodiments of this application, this application further proposes a spatial motion component, which includes a first metal substrate and a second metal substrate. The surface of the first metal substrate is provided with a conductive-lubricating integrated coating. The second metal substrate is disposed opposite to the first metal substrate and forms a friction pair. When the first metal substrate and the second metal substrate move relative to each other and generate friction, at least a portion of the lubricating layer of the conductive-lubricating integrated coating is transferred to the surface of the second metal substrate to form a conductive-lubricating interface.
[0042] The first and second metal substrates are the two main load-bearing bodies constituting the friction pair of the space-moving components. They are typically made of metal materials with good mechanical properties and adaptability to the space environment, such as, but not limited to, stainless steel, titanium alloys, aluminum alloys, or their composites. These substrates need to withstand certain loads and temperature changes in the space environment and serve as the base for coating adhesion. The first metal substrate can be a shaft, a gear, or a slider, while the second metal substrate can be a bearing housing, a gear, or a guide rail. The conductive-lubricating integrated coating is a pre-prepared functional coating applied to the surface of the first metal substrate, designed to provide both lubrication and conductivity. This coating achieves synergistic effects of conductivity and lubrication through its multi-layered structure. The coating can be uniformly applied to the surface of the first metal substrate using various methods such as spraying, brushing, dipping, or electrophoresis, ensuring good adhesion between the coating and the substrate to withstand subsequent friction and wear.
[0043] The friction pair refers to a combination of two components that come into contact with each other and move relative to each other. Here, the second metal substrate and the first metal substrate are designed with specific mechanical structures to enable them to come into contact and generate friction during operation. This relative arrangement can be sliding contact, rolling contact, or rotational contact; for example, the first metal substrate acts as a shaft and the second metal substrate acts as a bearing inner ring; or the first metal substrate acts as a slider and the second metal substrate acts as a guide rail. The relative motion refers to the mechanical displacement that occurs between the first and second metal substrates, such as linear reciprocating motion, rotational motion, or a combination of both. This motion is necessary for the spatial motion component to perform its function. When the two substrates move relative to each other, frictional forces are generated on their contact surfaces, which can lead to wear and energy loss.
[0044] The transfer refers to the phenomenon where, during friction, the outermost layer of lubricating material in the integrated conductive-lubricating coating detaches from the surface of the first metal substrate and adheres to the surface of the second metal substrate. This transfer is a crucial mechanism in the integrated coating design of this application, aiming to ensure that both surfaces of the friction pair acquire lubrication and conductivity. This transfer is achieved by selecting lubricating materials with appropriate adhesion and shear strength. For example, under frictional shear force, polytetrafluoroethylene and molybdenum disulfide in the lubricating layer can form a stable transfer film. Combined with the lamellar shear characteristics of graphite, this results in a coating with a low coefficient of friction and excellent wear resistance, significantly extending the service life of the space mechanism. This controlled material transfer mechanism ensures that both contact surfaces of the friction pair are covered with lubrication and conductivity, thereby continuously establishing and maintaining a continuous and stable conductive-lubricating interface during dynamic friction.
[0045] In the comparative experiments provided in this application, unless otherwise specified, all experimental conditions and materials are kept consistent to ensure comparability. Unless otherwise specified, all experimental materials and reagents used in the examples are commercially available.
[0046] The following provides a further description of the conductive-lubricating integrated coating, its preparation method, and a space motion component provided in this application.
[0047] Example 1: (1) Coating preparation: Preparation of conductive layer: Weigh out 15g of thermosetting polyimide resin, 18g of flake silver powder, 1.2g of few-layer graphene, 2g of high-structure conductive carbon black, 2g of BYK-9076 dispersant, and a mixed solvent consisting of 33g each of N-methylpyrrolidone and N,N-dimethylformamide. Add the above components sequentially to a sand mill, add 260g of ZrO2 grinding balls with a particle size of 0.5mm, and sand mill at 2500r / min for 3h. After removing the grinding balls, a uniform conductive layer undercoat is obtained.
[0048] Preparation of conductive-lubricating transition layer: Weigh out 14g of thermosetting polyimide resin, 14g of flake silver powder, 3g of flake graphite, 8g of molybdenum disulfide, 4g of polytetrafluoroethylene, 2g of antimony trioxide, 1.5g of BYK-066N defoamer, and a mixed solvent consisting of 30g each of N-methylpyrrolidone and N,N-dimethylformamide. Add the above components sequentially to a sand mill, add 270g of ZrO2 grinding balls with a particle size of 0.5mm, and sand mill at 2500r / min for 3h. After removing the grinding balls, a uniform conductive-lubricating transition layer coating is obtained.
[0049] Preparation of the lubricating layer: Weigh out 10g of thermosetting fluorinated polyimide resin, 6g of molybdenum disulfide, 8g of polytetrafluoroethylene, 10g of flake graphite, 1.5g of BYK-141 defoamer, and a mixed solvent consisting of 35g each of N-methylpyrrolidone and N,N-dimethylformamide. Add the above components sequentially to a sand mill, add 300g of ZrO2 grinding balls with a particle size of 0.5mm, and sand mill at 2500r / min for 3h. After removing the grinding balls, a uniform lubricating surface coating is obtained.
[0050] Coating spraying: Before spraying, the substrate surface can be sanded or sandblasted, etc. The spraying conditions are as follows: The nozzle diameter of the spray gun is 0.8–1.0 mm. Spraying pressure: 0.2 MPa to 0.4 MPa Spraying distance 20cm~30cm Number of spray coats: 3 coats of conductive layer, 2 coats of transition layer, and 2 coats of lubricating layer. Coating Curing: After the coating is surface dry, it is cured by baking: 80℃ for 1 hour, 120℃ for 1 hour, and 180℃ for 2 hours. After cooling to room temperature along the way, it is removed, completing the preparation of the conductive-lubricating integrated coating for space mechanisms; see the actual appearance picture. Figure 2 SEM image (see) Figure 3 .
[0051] Performance testing: The conductive layer thickness is 7μm, the conductive-lubricating transition layer thickness is 4μm, the lubricating layer thickness is 7μm, and the total coating thickness is 18μm. The coating vacuum friction coefficient is ~0.05, the wear life reaches 180,000 revolutions, and the resistance value measured by a multimeter is 13Ω.
[0052] Example 2: (1) Coating preparation: Preparation of conductive layer: Weigh out 13g of thermosetting polyimide resin, 12g of flake silver powder, 0.8g of few-layer graphene, 1.5g of high-structure conductive carbon black, 2g of BYK-190 dispersant, and a mixed solvent consisting of 25g each of N-methylpyrrolidone, N,N-dimethylformamide and dimethylacetamide. Add the above components sequentially to a sand mill, add 300g of ZrO2 grinding balls with a particle size of 0.5mm, and sand mill at 2000r / min for 4h. After removing the grinding balls, a uniform conductive layer undercoat is obtained.
[0053] Preparation of conductive-lubricating transition layer: Weigh out 12g of thermosetting polyimide resin, 10g of silver powder, 4g of graphite, 7g of molybdenum disulfide, 5g of polytetrafluoroethylene, 1.5g of antimony trioxide, 1g of BYK-065 defoamer, and a mixed solvent consisting of 25g each of N-methylpyrrolidone, N,N-dimethylformamide and dimethylacetamide. Add the above components sequentially to a sand mill, add 300g of ZrO2 grinding balls with a particle size of 0.5mm, and sand mill at 2000r / min for 4h. After removing the grinding balls, a uniform conductive-lubricating transition layer coating is obtained.
[0054] Preparation of the lubricating layer: Weigh out 9g of thermosetting fluorinated polyimide resin, 5g of molybdenum disulfide, 6g of polytetrafluoroethylene, 8g of flake graphite, 1g of BYK-065 defoamer, and a mixed solvent consisting of 22g each of N-methylpyrrolidone, N,N-dimethylformamide and dimethylacetamide. Add the above components sequentially to a sand mill, add 300g of ZrO2 grinding balls with a particle size of 0.5mm, and sand mill at 2000r / min for 4h. After removing the grinding balls, a uniform lubricating surface coating is obtained.
[0055] Coating spraying: Before spraying, the substrate surface can be sanded or sandblasted, etc. The spraying conditions are as follows: The nozzle diameter of the spray gun is 0.8–1.0 mm. Spraying pressure: 0.2 MPa to 0.4 MPa Spraying distance 20cm~30cm Number of spray coats: 2 coats of conductive layer, 1 coat of transition layer, and 3 coats of lubricating layer. Coating curing: After the coating is surface dry, it is baked and heated for curing: 80℃ for 1 hour, 120℃ for 1 hour, and 180℃ for 2 hours. After cooling to room temperature, it is taken out to complete the preparation of the conductive-lubricating integrated coating for space mechanisms.
[0056] Performance testing: The conductive layer thickness is 5μm, the conductive-lubricating transition layer thickness is 3μm, the lubricating layer thickness is 6μm, and the total coating thickness is 14μm. The coating vacuum friction coefficient is ~0.07, the wear life reaches 160,000 revolutions, and the resistance value measured by a multimeter is 17Ω.
[0057] Example 3: (1) Coating preparation: Preparation of conductive layer: Weigh out 16g of thermosetting polyimide resin, 10g of flake silver powder, 0.5g of few-layer graphene, 3g of high-structure conductive carbon black, 2g of BYK-111 dispersant, and a mixed solvent consisting of 34g each of N-methylpyrrolidone and dimethylacetamide. Add the above components sequentially to a sand mill, add 280g of ZrO2 grinding balls with a particle size of 0.5mm, and sand mill at 3000r / min for 2h. After removing the grinding balls, a uniform conductive layer undercoat is obtained.
[0058] Preparation of conductive-lubricating transition layer: Weigh out 10g of thermosetting polyimide resin, 8g of flake silver powder, 5g of flake graphite, 10g of molybdenum disulfide, 6g of polytetrafluoroethylene, 2.5g of antimony trioxide, 2g of BYK-141 defoamer, and a mixed solvent consisting of 30g each of N-methylpyrrolidone and N,N-dimethylformamide. Add the above components sequentially to a sand mill, add 280g of ZrO2 grinding balls with a particle size of 0.5mm, and sand mill at 3000r / min for 2h. After removing the grinding balls, a uniform conductive-lubricating transition layer coating is obtained.
[0059] Preparation of the lubricating layer: Weigh out 12g of thermosetting fluorinated polyimide resin, 8g of molybdenum disulfide, 10g of polytetrafluoroethylene, 12g of flake graphite, 2g of BYK-141 defoamer, and a mixed solvent consisting of 30g each of N-methylpyrrolidone and N,N-dimethylformamide. Add the above components sequentially to a sand mill, add 280g of ZrO2 grinding balls with a particle size of 0.5mm, and sand mill at 3000r / min for 2h. After removing the grinding balls, a uniform lubricating surface coating is obtained.
[0060] Coating spraying: Before spraying, the substrate surface can be sanded or sandblasted, etc. The spraying conditions are as follows: The nozzle diameter of the spray gun is 0.8–1.0 mm. Spraying pressure: 0.2 MPa to 0.4 MPa Spraying distance 20cm~30cm Number of spray coats: 3 coats of conductive layer, 2 coats of transition layer, and 3 coats of lubricating layer. Coating curing: After the coating is surface dry, it is baked and heated for curing: 80℃ for 1 hour, 120℃ for 1 hour, and 180℃ for 2 hours. After cooling to room temperature, it is taken out to complete the preparation of the conductive-lubricating integrated coating for space mechanisms.
[0061] Performance testing: The conductive layer thickness is 8μm, the conductive-lubricating transition layer thickness is 4μm, the lubricating layer thickness is 7μm, and the total coating thickness is 19μm. The coating vacuum friction coefficient is ~0.07, the wear resistance life reaches 190,000 revolutions, and the resistance value measured by a multimeter is 13Ω.
[0062] Comparative Example 1: Compared to Example 1, the lubricating layer is missing, but the total coating thickness remains the same; (1) Coating preparation: Preparation of conductive layer: Weigh out 15g of thermosetting polyimide resin, 18g of flake silver powder, 1.2g of few-layer graphene, 2g of high-structure conductive carbon black, 2g of BYK-9076 dispersant, and a mixed solvent consisting of 33g each of N-methylpyrrolidone and N,N-dimethylformamide. Add the above components sequentially to a sand mill, add 260g of ZrO2 grinding balls with a particle size of 0.5mm, and sand mill at 2500r / min for 3h. After removing the grinding balls, a uniform conductive layer undercoat is obtained.
[0063] Preparation of conductive-lubricating transition layer: Weigh out 14g of thermosetting polyimide resin, 14g of flake silver powder, 3g of flake graphite, 8g of molybdenum disulfide, 4g of polytetrafluoroethylene, 2g of antimony trioxide, 1.5g of BYK-066N defoamer, and a mixed solvent consisting of 30g each of N-methylpyrrolidone and N,N-dimethylformamide. Add the above components sequentially to a sand mill, add 270g of ZrO2 grinding balls with a particle size of 0.5mm, and sand mill at 2500r / min for 3h. After removing the grinding balls, a uniform conductive-lubricating transition layer coating is obtained.
[0064] Coating spraying: Before spraying, the substrate surface can be sanded or sandblasted, etc. The spraying conditions are as follows: The nozzle diameter of the spray gun is 0.8–1.0 mm. Spraying pressure: 0.2 MPa to 0.4 MPa Spraying distance 20cm~30cm Number of spray coatings: 4 coats of conductive layer and 4 coats of transition layer Coating curing: After the coating is surface dry, it is baked and heated for curing: 80℃ for 1 hour, 120℃ for 1 hour, and 180℃ for 2 hours. After cooling to room temperature, it is taken out to complete the preparation of the conductive-lubricating integrated coating for space mechanisms.
[0065] Performance testing: The conductive layer thickness was 10 μm, the conductive-lubricating transition layer thickness was 8 μm, and the total coating thickness was 18 μm. Testing was conducted using a vacuum ball-disc friction tester. The coating's vacuum friction coefficient was ~0.15, its wear life reached 50,000 revolutions, and the resistance value measured with a multimeter was 5 Ω. Compared with the performance test results of Example 1, the lack of a lubricating layer significantly reduced its wear resistance, manifested as an increase in the friction coefficient and a decrease in wear life.
[0066] Comparative Example 2: Compared to Example 1, the conductive-lubricating transition layer is missing, but the total coating thickness remains the same; (1) Coating preparation: Preparation of conductive layer: Weigh out 15g of thermosetting polyimide resin, 18g of flake silver powder, 1.2g of few-layer graphene, 2g of high-structure conductive carbon black, 2g of BYK-9076 dispersant, and a mixed solvent consisting of 33g each of N-methylpyrrolidone and N,N-dimethylformamide. Add the above components sequentially to a sand mill, add 260g of ZrO2 grinding balls with a particle size of 0.5mm, and sand mill at 2500r / min for 3h. After removing the grinding balls, a uniform conductive layer undercoat is obtained.
[0067] Preparation of the lubricating layer: Weigh out 10g of thermosetting fluorinated polyimide resin, 6g of molybdenum disulfide, 8g of polytetrafluoroethylene, 10g of flake graphite, 1.5g of BYK-141 defoamer, and a mixed solvent consisting of 35g each of N-methylpyrrolidone and N,N-dimethylformamide. Add the above components sequentially to a sand mill, add 300g of ZrO2 grinding balls with a particle size of 0.5mm, and sand mill at 2500r / min for 3h. After removing the grinding balls, a uniform lubricating surface coating is obtained.
[0068] Coating spraying: Before spraying, the substrate surface can be sanded or sandblasted, etc. The spraying conditions are as follows: The nozzle diameter of the spray gun is 0.8–1.0 mm. Spraying pressure: 0.2 MPa to 0.4 MPa Spraying distance 20cm~30cm Number of spray coats: 4 coats of conductive layer, 3 coats of lubricating layer Coating curing: After the coating is surface dry, it is baked and heated for curing: 80℃ for 1 hour, 120℃ for 1 hour, and 180℃ for 2 hours. After cooling to room temperature, it is taken out to complete the preparation of the conductive-lubricating integrated coating for space mechanisms.
[0069] Performance testing: The conductive layer thickness is 11 μm, the lubricating layer thickness is 7 μm, and the total coating thickness is 18 μm. Testing was conducted using a vacuum ball-disc friction tester. The coating's vacuum friction coefficient was ~0.07, and its wear life reached 70,000 revolutions. The resistance value measured with a multimeter was 4 Ω. Compared with the performance test results of Example 1, although the friction coefficient did not change significantly after the absence of the conductive-lubricating transition layer, its wear life decreased significantly to 70,000 revolutions. This may be related to the lack of transition layer material, which indirectly indicates that the three sub-layers in the coating of this application have a synergistic effect in improving lubrication performance.
[0070] Comparative Example 3: Compared to Example 1, it lacks a conductive layer, but the total coating thickness remains the same; (1) Coating preparation: Preparation of conductive-lubricating transition layer: Weigh out 14g of thermosetting polyimide resin, 14g of flake silver powder, 3g of flake graphite, 8g of molybdenum disulfide, 4g of polytetrafluoroethylene, 2g of antimony trioxide, 1.5g of BYK-066N defoamer, and a mixed solvent consisting of 30g each of N-methylpyrrolidone and N,N-dimethylformamide. Add the above components sequentially to a sand mill, add 270g of ZrO2 grinding balls with a particle size of 0.5mm, and sand mill at 2500r / min for 3h. After removing the grinding balls, a uniform conductive-lubricating transition layer coating is obtained.
[0071] Preparation of the lubricating layer: Weigh out 10g of thermosetting fluorinated polyimide resin, 6g of molybdenum disulfide, 8g of polytetrafluoroethylene, 10g of flake graphite, 1.5g of BYK-141 defoamer, and a mixed solvent consisting of 35g each of N-methylpyrrolidone and N,N-dimethylformamide. Add the above components sequentially to a sand mill, add 300g of ZrO2 grinding balls with a particle size of 0.5mm, and sand mill at 2500r / min for 3h. After removing the grinding balls, a uniform lubricating surface coating is obtained.
[0072] Coating spraying: Before spraying, the substrate surface can be sanded or sandblasted, etc. The spraying conditions are as follows: The nozzle diameter of the spray gun is 0.8–1.0 mm. Spraying pressure: 0.2 MPa to 0.4 MPa Spraying distance 20cm~30cm Number of spray coats: 4 coats for the transition layer, 4 coats for the lubricating layer Coating curing: After the coating is surface dry, it is baked and heated for curing: 80℃ for 1 hour, 120℃ for 1 hour, and 180℃ for 2 hours. After cooling to room temperature, it is taken out to complete the preparation of the conductive-lubricating integrated coating for space mechanisms.
[0073] Performance testing: The conductive-lubricating transition layer thickness is 9 μm, the lubricating layer thickness is 9 μm, and the total coating thickness is 18 μm. Testing was conducted using a vacuum ball-disc friction tester. The coating's vacuum friction coefficient was ~0.05, its wear life reached 120,000 revolutions, and the resistance value measured with a multimeter was 132 Ω. Compared with the performance test results of Example 1, the conductivity significantly decreased after the absence of the conductive layer, manifested as a significant increase in resistance; simultaneously, the wear resistance also decreased to some extent, with the wear life decreasing to 120,000 revolutions. This may be related to the lack of conductive layer material, which indirectly indicates that the three sub-layers in the coating of this application synergistically enhance lubrication and conductivity.
[0074] The above description is merely a specific embodiment of this application, enabling those skilled in the art to understand or implement this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed herein.
Claims
1. An electrically conductive-lubricating integrated coating, characterized by, From the inside out, it consists of a conductive layer, a conductive-lubricating transition layer, and a lubricating layer. The conductive layer comprises 10-20 parts by weight of polyimide resin and 10-25 parts by weight of a first conductive agent; The conductive-lubricating transition layer comprises 10-20 parts by weight of polyimide resin, 10-21 parts by weight of a second conductive agent, 5-20 parts by weight of a first lubricant, and 1-5 parts by weight of a lubricating additive. The lubricating layer comprises 5-15 parts by weight of fluorinated polyimide resin, 5-20 parts by weight of a second lubricant, and 5-15 parts by weight of a third conductive agent.
2. The electrically-conductive, lubricious integrated coating of claim 1, wherein, The first conductive agent, the second conductive agent, and the third conductive agent are each independently selected from one or more of silver, graphite, graphene, and conductive carbon black; the first lubricant and the second lubricant are each independently selected from molybdenum disulfide and / or polytetrafluoroethylene; and the lubricating additive is selected from antimony trioxide.
3. The electrically-conductive, lubricious integrated coating of claim 1 or 2, wherein, The first conductive agent includes silver, graphene, and conductive carbon black; the second conductive agent includes silver and graphite; and the third conductive agent includes graphite. Both the first and second lubricants include molybdenum disulfide and polytetrafluoroethylene.
4. The electrically-conductive, lubricious integrated coating of claim 3, wherein, The first conductive agent comprises 10-20 parts by weight of silver, 0.5-1.5 parts by weight of graphene, and 1-3 parts by weight of conductive carbon black; the second conductive agent comprises 8-16 parts by weight of silver and 2-5 parts by weight of graphite; and the third conductive agent comprises 6-12 parts by weight of graphite. The first lubricant comprises 5-10 parts by weight of molybdenum disulfide and 2-6 parts by weight of polytetrafluoroethylene; and the second lubricant comprises 4-8 parts by weight of molybdenum disulfide and 4-10 parts by weight of polytetrafluoroethylene.
5. The electrically-conductive, lubricious integrated coating of claim 4, wherein, The silver includes flaky silver powder with a particle size of 0.5-3 μm; the graphene includes few-layer graphene with a layer number of 1-10 layers and a flake size of 0.5-5 μm; the graphite includes flaky graphite with a particle size of 0.5-3 μm; the conductive carbon black includes high-structure conductive carbon black with a specific surface area of 200-1500 m 2 / g; the molybdenum disulfide has a particle size of 0.3-2 μm; the polytetrafluoroethylene has a particle size of 1-3 μm; and the antimony trioxide has a particle size of 0.5-1.5 μm.
6. The electrically-conductive, lubricious integrated coating of claim 1, wherein, The thickness of the conductive layer is controlled at 4~8μm; the thickness of the conductive-lubricating transition layer is 2~5μm; the thickness of the lubricating layer is 3~7μm; and the total thickness of the integrated conductive-lubricating coating is 9~20μm.
7. A method for producing the electrically conductive-lubricative integrated coating according to any one of claims 1 to 6, characterized by, include: Weigh out the conductive layer raw materials according to the proportions and mix them thoroughly with the solvent and dispersant to obtain the conductive layer slurry; Weigh out the conductive-lubricating transition layer raw materials according to the proportion and mix them thoroughly with solvent and defoamer to obtain conductive-lubricating transition layer slurry. Weigh out the lubricating layer raw materials according to the proportion and mix them thoroughly with solvent and defoamer to obtain the lubricating layer slurry; A conductive layer, a conductive-lubricating transition layer, and a lubricating layer are sequentially sprayed from the inside out. During the spraying process, the next layer is sprayed after each layer is surface dry. After the lubricating layer is surface dry, it is heated and cured to obtain the integrated conductive-lubricating coating.
8. The preparation method according to claim 7, characterized in that, The dispersant includes one or more of BYK-9076, BYK-190, and BYK-111; the solvent includes one or more of N-methylpyrrolidone, N,N-dimethylformamide, and dimethylacetamide; and the defoamer includes one or more of BYK-065, BYK-066N, and BYK-141.
9. A spatial motion component, characterized by It includes a first metal substrate, the surface of which is provided with the conductive-lubricating integrated coating as described in any one of claims 1-6.
10. The spatial motion component of claim 9, wherein, The invention includes a first metal substrate and a second metal substrate. The surface of the first metal substrate is provided with a conductive-lubricating integrated coating as described in any one of claims 1-6. The second metal substrate is disposed opposite to the first metal substrate and forms a friction pair. When the first metal substrate and the second metal substrate move relative to each other and generate friction, at least a portion of the lubricating layer of the conductive-lubricating integrated coating is transferred to the surface of the second metal substrate to form a conductive-lubricating interface.