An acrylic aging-resistant hot melt pressure-sensitive adhesive and its preparation method
By introducing porous titanium dioxide and modifiers into acrylate hot melt pressure-sensitive adhesives, a semi-interpenetrating network structure is formed, which solves the problems of thermo-oxidative degradation and photodegradation, improves the aging resistance and mechanical properties of the adhesive, and extends its service life.
Patent Information
- Application Number
- CN202611496308.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-24
- Publication Date
- 2026-11-17
AI Technical Summary
Existing acrylic hot melt pressure-sensitive adhesives are prone to thermo-oxidative degradation and photodegradation in outdoor or high-temperature environments, resulting in decreased adhesive strength and reduced cohesion. Furthermore, the poor compatibility between inorganic fillers and organic polymer matrices affects the overall performance of the adhesive.
A semi-interpenetrating network structure is formed by chemical reaction of porous titanium dioxide and modifiers, which enhances the physical entanglement of the additives and acrylate prepolymer, forming a chemical-physical hybrid crosslinking network, thereby improving aging resistance and mechanical properties.
The prepared acrylic-based aging-resistant hot melt pressure-sensitive adhesive significantly extends service life and improves bonding strength and anti-aging properties while ensuring quality.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of adhesive technology, specifically to an acrylic-based aging-resistant hot melt pressure-sensitive adhesive and its preparation method. Background Technology
[0002] Hot melt pressure-sensitive adhesives are a type of adhesive that is applied in a molten state upon heating and then bonds upon application of slight pressure after cooling. Compared to traditional solvent-based pressure-sensitive adhesives, they offer advantages such as solvent-free operation, environmental friendliness, fast curing speed, and ease of automated production, making them widely used in packaging, labeling, medical, automotive, and electronics industries. Among these, acrylic hot melt pressure-sensitive adhesives have attracted considerable attention due to their excellent weather resistance, oxidation resistance, and optical transparency.
[0003] However, existing acrylic hot melt pressure-sensitive adhesives still face many challenges in practical applications. First, their high-temperature aging resistance and UV aging resistance need improvement. During long-term use outdoors or in high-temperature environments, the adhesive is prone to thermo-oxidative degradation and photodegradation, leading to decreased bond strength, reduced cohesion, and problems such as residual adhesive or embrittled adhesive layers, severely limiting its application in demanding fields such as automotive interiors, outdoor labels, and electronic components. Second, to improve aging resistance, existing technologies often add small-molecule antioxidants and UV absorbers, but these additives are prone to migration and precipitation during long-term use, resulting in a gradual weakening of their protective effect. Furthermore, to improve the mechanical properties and flame retardancy of the adhesive, inorganic fillers (such as magnesium hydroxide and ammonium polyphosphate) are often added, but inorganic fillers have poor compatibility with organic polymer matrices and are prone to aggregation, affecting the overall performance of the adhesive.
[0004] Therefore, the present invention provides an acrylic-based aging-resistant hot melt pressure-sensitive adhesive and its preparation method to solve the above-mentioned technical problems. Summary of the Invention
[0005] This invention provides an acrylic-based aging-resistant hot melt pressure-sensitive adhesive and its preparation method. The prepared pressure-sensitive adhesive not only has excellent aging resistance but also excellent mechanical properties. While ensuring the quality of the pressure-sensitive adhesive, it also effectively extends its service life to a certain extent.
[0006] To achieve the above objectives, the present invention provides the following technical solution: An acrylic-type aging-resistant hot melt pressure-sensitive adhesive, by weight, is composed of the following raw materials: 50-70 parts acrylate prepolymer, 3-8 parts lauryl methacrylate, 20-30 parts magnesium hydroxide, 10-20 parts ammonium polyphosphate, 3-6 parts reinforcing agent, 2-4 parts tin oxide, 1-2 parts antioxidant, 1-2 parts ultraviolet absorber, and 0.2-0.4% by weight of 1-hydroxycyclohexylphenyl ketone in the acrylate prepolymer.
[0007] Furthermore, the acrylate prepolymer is prepared by the following method: 40-50 parts by weight of n-hexyl methacrylate, 6-10 parts by weight of n-butyl methacrylate, 6-10 parts by weight of acrylic acid and 1.5-3 parts by weight of N-(butoxymethyl)acrylamide are polymerized in the presence of 0.01-0.03 parts by weight of diphenyl-(2,4,6-trimethylbenzoyl)phosphorus oxide, 0.1-0.3 parts by weight of tert-dodecyl mercaptan and UV light. When the reaction temperature reaches 80-85°C, air is introduced to terminate the reaction, thereby obtaining the acrylate prepolymer.
[0008] Furthermore, the reinforcing agent is prepared by the following method: Step 1: Disperse 4,4-diaminobenzoylaniline uniformly in 20-30 times its mass of N,N-dimethylformamide. Under nitrogen protection, heat the resulting mixture to 50-60℃, then add dibutyltin dilaurate. After uniform dispersion, slowly add isophorone diisocyanate, stir until homogeneous, and continue the reaction for 2-3 hours. After the reaction is complete, evaporate the solvent from the reaction solution to obtain the modifier. The mass ratio of 4,4-diaminobenzoylaniline, dibutyltin dilaurate, and isophorone diisocyanate is 1:0.02-0.03:0.4-0.6. Step 2: Disperse carboxylated titanium dioxide uniformly in N,N-dimethylformamide at a dosage ratio of 10-30 g / L, then add a modifier with a mass of 2-3 times that of carboxylated titanium dioxide, mix well, and react at 50-70℃ for 4-6 h; after the reaction is complete, filter, wash and vacuum dry the reaction solution to obtain the reinforcing agent.
[0009] Furthermore, the preparation method of the carboxyl titanium dioxide is as follows: porous titanium dioxide is uniformly dispersed in deionized water at a dosage ratio of 10-20 g / L, and then sodium chloroacetate with a mass of 0.8-1.2 times that of porous titanium dioxide is added. The pH value of the resulting mixture is adjusted to 11.5-12.5, and the mixture is reacted at 100-120℃ for 3-5 hours. The reaction solution is then filtered, the filter cake is washed with water until neutral, and then vacuum dried to obtain the final product.
[0010] Furthermore, the porous titanium oxide is prepared by ultrasonically dispersing titanium isopropoxide, dodecyl dimethyl tertiary amine, and deionized water at a mass ratio of 1:0.3-0.5:20-40. Then, a hydrochloric acid aqueous solution with a mass of 0.2-0.4 times that of titanium isopropoxide and a concentration of 30-45wt% is added. After mixing and stirring evenly, the mixture is kept at 50-70℃ for 30-35 hours. After the reaction is complete, the filter cake in the reaction solution is filtered out and aged to obtain the final product.
[0011] Furthermore, the aging temperature is 110-130℃, and the aging time is 35-45h.
[0012] Furthermore, the antioxidant is any one of antioxidant 1010, antioxidant 168, antioxidant 1076, and antioxidant 1024.
[0013] Furthermore, the ultraviolet absorber is any one of 2-hydroxy-5-chlorobenzophenone, 2-hydroxy-4-alkoxybenzophenone, and 2-(2-hydroxy-3,5-di-tert-pentylphenyl)benzotriazole.
[0014] A method for preparing an acrylic-based aging-resistant hot melt pressure-sensitive adhesive includes the following steps: weighing each raw material according to the formula, then adding lauryl methacrylate to the acrylate prepolymer, stirring to dissolve, adding 1-hydroxycyclohexylphenyl ketone, continuing to stir to dissolve, then adding the remaining raw materials, mixing and stirring evenly, applying the resulting adhesive solution onto a polyester film, covering it with a release film to isolate oxygen, and curing it under UV light to obtain the acrylic-based aging-resistant hot melt pressure-sensitive adhesive.
[0015] Furthermore, the energy of the UV light during curing is 300-750 mJ / cm². 2 And the curing time is 6-8 minutes.
[0016] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention uses titanium isopropoxide and dodecyl dimethyl tertiary amine as raw materials to prepare porous titanium oxide through a chemical reaction. Then, the porous titanium oxide is uniformly dispersed in deionized water, and sodium chloroacetate is added to adjust the pH before a chemical reaction is carried out to prepare carboxylated titanium oxide. Furthermore, this invention uses 4,4-diaminobenzoylaniline and isophorone diisocyanate as raw materials, and the two react chemically under the action of dibutyltin dilaurate to prepare an anti-aging compound—a modifier—containing active reactive groups on its molecular chain. The carboxylated titanium oxide is uniformly dispersed in N,N-dimethylformamide, and then the modifier is added. Through a chemical reaction, the carboxylated titanium oxide reacts with the active reactive groups of the modifier. Ultimately, the modifier is anchored on the surface and porous structure of the carboxylated titanium oxide through a chemical reaction, forming a three-dimensional anti-aging "film" on the surface and inside the carboxylated oxidized state. Finally, under the synergistic effect of porous titanium oxide and the modifier, the anti-aging performance of the reinforcing agent is effectively improved. Meanwhile, the modifier itself has a long molecular chain, which can physically entangle with the acrylate prepolymer. In addition, the bonding of the modifier also effectively reduces the aggregation of porous titanium dioxide, while the porous carboxyl titanium dioxide acts as a multifunctional crosslinking point, jointly constructing a semi-interpenetrating network structure or a chemical-physical hybrid crosslinking network, effectively improving the mechanical properties of the pressure-sensitive adhesive.
[0017] 2. This invention uses hexyl methacrylate, butyl methacrylate, acrylic acid, diphenyl-(2,4,6-trimethylbenzoyl)phosphorus oxymethol, N-(butoxymethyl)acrylamide, and tert-dodecyl mercaptan as raw materials to prepare an acrylate prepolymer through a chemical reaction. As the main component of the pressure-sensitive adhesive, it provides basic viscoelasticity and initial tack. Specifically, hexyl methacrylate and butyl methacrylate provide flexible long-chain alkyl groups, giving the adhesive good wettability and initial tack; acrylic acid introduces polar carboxyl groups, enhancing adhesion to the substrate; N-(butoxymethyl)acrylamide contains reactive butoxymethyl and amide groups, which can participate in the crosslinking reaction during subsequent UV curing to form a three-dimensional network structure, effectively improving the cohesive strength and heat resistance of the pressure-sensitive adhesive.
[0018] In summary, the pressure-sensitive adhesive prepared by this invention not only has excellent aging resistance but also excellent mechanical properties. While ensuring the quality of the pressure-sensitive adhesive, it also effectively extends its service life to a certain extent. Detailed Implementation
[0019] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0020] Example 1 An acrylic-type aging-resistant hot melt pressure-sensitive adhesive is composed of the following raw materials by weight: 50 parts acrylate prepolymer, 3 parts lauryl methacrylate, 20 parts magnesium hydroxide, 10 parts ammonium polyphosphate, 3 parts reinforcing agent, 2 parts tin oxide, 1 part antioxidant 1010, 1 part 2-hydroxy-5-chlorobenzophenone, and 0.2% by weight of 1-hydroxycyclohexylphenyl ketone in the acrylate prepolymer.
[0021] The acrylate prepolymer was prepared by the following method: 40 parts by weight of n-hexyl methacrylate, 6 parts by weight of n-butyl methacrylate, 6 parts by weight of acrylic acid and 1.5 parts by weight of N-(butoxymethyl)acrylamide were subjected to polymerization reaction in 0.01 parts of diphenyl-(2,4,6-trimethylbenzoyl)phosphorus oxide, 0.1 parts by weight of tert-dodecyl mercaptan and UV light. When the reaction temperature reached 80°C, air was introduced to terminate the reaction, and the acrylate prepolymer was obtained.
[0022] The reinforcing agent is prepared by the following method: Step 1: Disperse 4,4-diaminobenzoylaniline uniformly in N,N-dimethylformamide at 20 times its mass. Under nitrogen protection, heat the resulting mixture to 50°C, then add dibutyltin dilaurate. After uniform dispersion, slowly add isophorone diisocyanate, stir until homogeneous, and continue the reaction for 3 hours. After the reaction is complete, evaporate the solvent from the reaction solution to obtain the modifier. The mass ratio of 4,4-diaminobenzoylaniline, dibutyltin dilaurate, and isophorone diisocyanate is 1:0.02:0.4. Step 2: Disperse carboxylated titanium dioxide evenly in N,N-dimethylformamide at a dosage ratio of 10 g / L, then add a modifier with a mass of twice that of carboxylated titanium dioxide, mix well, and react at 50°C for 6 hours; after the reaction is complete, filter, wash and vacuum dry the reaction solution to obtain the reinforcing agent.
[0023] The preparation method of carboxylated titanium dioxide is as follows: porous titanium dioxide is uniformly dispersed in deionized water at a dosage ratio of 10 g / L, and then sodium chloroacetate with a mass of 0.8 times that of porous titanium dioxide is added. The pH value of the resulting mixture is adjusted to 11.5, and the mixture is reacted at 100℃ for 5 h. The reaction solution is then filtered, the filter cake is washed with water until neutral, and then vacuum dried to obtain the final product.
[0024] The preparation method of porous titanium dioxide is as follows: titanium isopropoxide, dodecyl dimethyl tertiary amine and deionized water are ultrasonically dispersed evenly at a mass ratio of 1:0.3:20. Then, hydrochloric acid aqueous solution with a mass of 0.2 times that of titanium isopropoxide and a concentration of 30wt% is added. After mixing and stirring evenly, the mixture is kept at 50℃ for 35h. After the reaction is complete, the filter cake in the reaction solution is filtered out and aged to obtain the product. The aging temperature is 110℃ and the aging time is 45h.
[0025] A method for preparing an acrylic-based aging-resistant hot-melt pressure-sensitive adhesive includes the following steps: weighing each raw material according to the formula, then adding lauryl methacrylate to the acrylate prepolymer, stirring to dissolve, adding 1-hydroxycyclohexylphenyl ketone, continuing to stir to dissolve, then adding the remaining raw materials, mixing and stirring evenly, applying the resulting adhesive solution onto a polyester film, covering it with a release film to isolate oxygen, and curing under UV light to obtain the acrylic-based aging-resistant hot-melt pressure-sensitive adhesive; wherein, the energy of the UV light during curing is 300 mJ / cm. 2 And the curing time is 8 minutes.
[0026] Example 2 An acrylic-type aging-resistant hot melt pressure-sensitive adhesive is composed of the following raw materials by weight: 60 parts acrylate prepolymer, 5 parts lauryl methacrylate, 25 parts magnesium hydroxide, 15 parts ammonium polyphosphate, 5 parts reinforcing agent, 3 parts tin oxide, 1.5 parts antioxidant 168, 1.5 parts 2-hydroxy-4-alkoxybenzophenone, and 0.3% by weight of 1-hydroxycyclohexylphenyl ketone in the acrylate prepolymer.
[0027] The acrylate prepolymer was prepared by the following method: 45 parts by weight of n-hexyl methacrylate, 8 parts by weight of n-butyl methacrylate, 8 parts by weight of acrylic acid and 1.5-3 parts by weight of N-(butoxymethyl)acrylamide were subjected to polymerization reaction in 0.02 parts by weight of diphenyl-(2,4,6-trimethylbenzoyl)phosphorus oxide, 0.2 parts by weight of tert-dodecyl mercaptan and UV light. When the reaction temperature reached 85°C, air was introduced to terminate the reaction, and the acrylate prepolymer was obtained.
[0028] The reinforcing agent is prepared by the following method: Step 1: Disperse 4,4-diaminobenzoylaniline uniformly in 25 times its mass of N,N-dimethylformamide. Under nitrogen protection, heat the resulting mixture to 55°C, then add dibutyltin dilaurate. After uniform dispersion, slowly add isophorone diisocyanate, stir until homogeneous, and continue the reaction for 3 hours. After the reaction is complete, evaporate the solvent from the reaction solution to obtain the modifier. The mass ratio of 4,4-diaminobenzoylaniline, dibutyltin dilaurate, and isophorone diisocyanate is 1:0.03:0.5. Step 2: Disperse carboxylated titanium dioxide evenly in N,N-dimethylformamide at a dosage ratio of 20 g / L, then add a modifier with a mass of 3 times that of carboxylated titanium dioxide, mix well, and react at 60°C for 5 h; after the reaction is complete, filter, wash and vacuum dry the reaction solution in sequence to obtain the reinforcing agent.
[0029] The preparation method of carboxylated titanium dioxide is as follows: porous titanium dioxide is uniformly dispersed in deionized water at a dosage ratio of 15 g / L, and then sodium chloroacetate of the same mass as the porous titanium dioxide is added. The pH value of the resulting mixture is adjusted to 12.0, and the reaction is carried out at 110℃ for 4 hours. The reaction solution is then filtered, the filter cake is washed with water until neutral, and then vacuum dried to obtain the final product.
[0030] The preparation method of porous titanium dioxide is as follows: titanium isopropoxide, dodecyl dimethyl tertiary amine and deionized water are ultrasonically dispersed evenly at a mass ratio of 1:0.4:30. Then, hydrochloric acid aqueous solution with a mass of 0.3 times that of titanium isopropoxide and a concentration of 40wt% is added. After mixing and stirring evenly, the mixture is kept at 60℃ for 35h. After the reaction is complete, the filter cake in the reaction solution is filtered out and aged to obtain the product. The aging temperature is 120℃ and the aging time is 40h.
[0031] A method for preparing an acrylic-based aging-resistant hot-melt pressure-sensitive adhesive includes the following steps: weighing each raw material according to the formula, then adding lauryl methacrylate to the acrylate prepolymer, stirring to dissolve, adding 1-hydroxycyclohexylphenyl ketone, continuing to stir to dissolve, then adding the remaining raw materials, mixing and stirring evenly, applying the resulting adhesive solution onto a polyester film, covering it with a release film to isolate oxygen, and curing under UV light to obtain the acrylic-based aging-resistant hot-melt pressure-sensitive adhesive; wherein, the energy of the UV light during curing is 550 mJ / cm. 2 And the curing time is 7 minutes.
[0032] Example 3 An acrylic-type aging-resistant hot melt pressure-sensitive adhesive is composed of the following raw materials by weight: 70 parts acrylate prepolymer, 8 parts lauryl methacrylate, 30 parts magnesium hydroxide, 20 parts ammonium polyphosphate, 6 parts reinforcing agent, 4 parts tin oxide, 2 parts antioxidant 1076, 2 parts 2-(2-hydroxy-3,5-di-tert-pentylphenyl)benzotriazole, and 0.4% by weight of 1-hydroxycyclohexylphenyl ketone in the acrylate prepolymer.
[0033] The acrylate prepolymer was prepared by the following method: 50 parts by weight of n-hexyl methacrylate, 10 parts by weight of n-butyl methacrylate, 10 parts by weight of acrylic acid and 3 parts by weight of N-(butoxymethyl)acrylamide were subjected to polymerization reaction in 0.03 parts of diphenyl-(2,4,6-trimethylbenzoyl)phosphorus oxide, 0.3 parts of tert-dodecyl mercaptan and UV light. When the reaction temperature reached 85°C, air was introduced to terminate the reaction, and the acrylate prepolymer was obtained.
[0034] The reinforcing agent is prepared by the following method: Step 1: Disperse 4,4-diaminobenzoylaniline uniformly in N,N-dimethylformamide at 30 times its mass. Under nitrogen protection, heat the resulting mixture to 60°C, then add dibutyltin dilaurate. After uniform dispersion, slowly add isophorone diisocyanate. Stir until homogeneous and continue the reaction for 2 hours. After the reaction is complete, evaporate the solvent from the reaction solution to obtain the modifier. The mass ratio of 4,4-diaminobenzoylaniline, dibutyltin dilaurate, and isophorone diisocyanate is 1:0.03:0.6. Step 2: Disperse carboxylated titanium dioxide evenly in N,N-dimethylformamide at a dosage ratio of 30 g / L, then add a modifier with a mass of 3 times that of carboxylated titanium dioxide, mix well, and react at 70°C for 4 hours; after the reaction is complete, filter, wash and vacuum dry the reaction solution in sequence to obtain the reinforcing agent.
[0035] The preparation method of carboxylated titanium dioxide is as follows: porous titanium dioxide is uniformly dispersed in deionized water at a dosage ratio of 20 g / L, and then sodium chloroacetate with a mass of 1.2 times that of porous titanium dioxide is added. The pH value of the resulting mixture is adjusted to 12.5, and the reaction is carried out at 120℃ for 3 hours. The reaction solution is then filtered, the filter cake is washed with water until neutral, and then vacuum dried to obtain the final product.
[0036] The preparation method of porous titanium dioxide is as follows: titanium isopropoxide, dodecyl dimethyl tertiary amine and deionized water are ultrasonically dispersed evenly at a mass ratio of 1:0.5:40. Then, hydrochloric acid aqueous solution with a mass of 0.4 times that of titanium isopropoxide and a concentration of 45wt% is added. After mixing and stirring evenly, the mixture is kept at 70℃ for 30h. After the reaction is complete, the filter cake in the reaction solution is filtered out and aged to obtain the product. The aging temperature is 130℃ and the aging time is 35h.
[0037] A method for preparing an acrylic-based aging-resistant hot-melt pressure-sensitive adhesive includes the following steps: weighing each raw material according to the formula, then adding lauryl methacrylate to the acrylate prepolymer, stirring to dissolve, adding 1-hydroxycyclohexylphenyl ketone, continuing to stir to dissolve, then adding the remaining raw materials, mixing and stirring evenly, applying the resulting adhesive solution onto a polyester film, covering it with a release film to isolate oxygen, and curing under UV light to obtain the acrylic-based aging-resistant hot-melt pressure-sensitive adhesive; wherein, the energy of the UV light during curing is 750 mJ / cm. 2 And the curing time is 6 minutes.
[0038] Comparative Example 1: The difference between this comparative example and Example 1 is that an equal amount of porous titanium dioxide is used instead of the reinforcing agent in this comparative example.
[0039] Comparative Example 2: The difference between this comparative example and Example 1 is that in this comparative example, an equal amount of titanium dioxide with a particle size similar to that of porous titanium dioxide (average particle size of 160 nm) is used to replace the reinforcing agent.
[0040] Performance testing: The relevant properties of the hot melt pressure-sensitive adhesive samples prepared in Examples 1-3 and Comparative Examples 1-2 were tested as follows, and the test data are recorded in the table below: 1. Peel strength and peel strength after aging: The PET samples prepared in each example and comparative example were pasted onto steel plates, and the peel strength was tested according to GB / T 2792-2014; the pasted samples prepared according to the above method were placed at 70℃ for 3 days, and the peel strength of the steel plate was tested according to GB / T 2792. 2. High-temperature tackiness: Each sample was tested according to GB / T 4851-2014 standard; 3. Alkaline washing effect on PET bottles: Prepare a 5wt% NaOH aqueous solution and heat it to 80℃. Attach the PET sample to the PET bottle body. Cut the bottle body with the PET sample attached into square pieces of 1cm×1cm, put them into the alkaline solution and stir. Observe whether it falls off within 10 minutes and record the time of fall-off.
[0041] 4. Alkaline water washing effect on glass bottles: Prepare a 5wt% NaOH aqueous solution and heat it to 80℃. Attach the PET sample to the glass bottle and immerse it in the alkaline water. Observe whether it falls off within 5 minutes and record the time of detachment.
[0042] By comparing and analyzing the relevant data in the table, it can be seen that the acrylic-based aging-resistant hot-melt pressure-sensitive adhesive prepared by this invention not only has excellent aging resistance but also excellent mechanical properties. While ensuring the quality of the pressure-sensitive adhesive, it also effectively extends its service life to a certain extent. This indicates that the acrylic-based aging-resistant hot-melt pressure-sensitive adhesive and its preparation method provided by this invention have a broader market prospect and are more suitable for widespread application.
[0043] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0044] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.
Claims
1. An acrylic-based aging-resistant hot melt pressure-sensitive adhesive, characterized in that, Composed of the following raw materials by weight: 50-70 parts acrylate prepolymer, 3-8 parts lauryl methacrylate, 20-30 parts magnesium hydroxide, 10-20 parts ammonium polyphosphate, 3-6 parts reinforcing agent, 2-4 parts tin oxide, 1-2 parts antioxidant, 1-2 parts ultraviolet absorber, and 0.2-0.4% by weight of 1-hydroxycyclohexylphenyl ketone.
2. The acrylic aging-resistant hot melt pressure-sensitive adhesive according to claim 1, characterized in that, The acrylate prepolymer is prepared by the following method: 40-50 parts by weight of n-hexyl methacrylate, 6-10 parts by weight of n-butyl methacrylate, 6-10 parts by weight of acrylic acid and 1.5-3 parts by weight of N-(butoxymethyl)acrylamide are polymerized in the presence of 0.01-0.03 parts by weight of diphenyl-(2,4,6-trimethylbenzoyl)phosphorus oxide, 0.1-0.3 parts by weight of tert-dodecyl mercaptan and UV light. When the reaction temperature reaches 80-85°C, air is introduced to terminate the reaction, thus obtaining the acrylate prepolymer.
3. The acrylic aging-resistant hot melt pressure-sensitive adhesive according to claim 1, characterized in that, The reinforcing agent is prepared by the following method: Step 1: Disperse 4,4-diaminobenzoylaniline uniformly in 20-30 times its mass of N,N-dimethylformamide. Under nitrogen protection, heat the resulting mixture to 50-60℃, then add dibutyltin dilaurate. After uniform dispersion, slowly add isophorone diisocyanate, stir until homogeneous, and continue the reaction for 2-3 hours. After the reaction is complete, evaporate the solvent from the reaction solution to obtain the modifier. The mass ratio of 4,4-diaminobenzoylaniline, dibutyltin dilaurate, and isophorone diisocyanate is 1:0.02-0.03:0.4-0.
6. Step 2: Disperse carboxylated titanium dioxide uniformly in N,N-dimethylformamide at a dosage ratio of 10-30 g / L, then add a modifier with a mass of 2-3 times that of carboxylated titanium dioxide, mix well, and react at 50-70℃ for 4-6 h; after the reaction is complete, filter, wash and vacuum dry the reaction solution to obtain the reinforcing agent.
4. The acrylic-based aging-resistant hot melt pressure-sensitive adhesive according to claim 3, characterized in that, The method for preparing the carboxyl titanium dioxide is as follows: porous titanium dioxide is uniformly dispersed in deionized water at a dosage ratio of 10-20 g / L, and then sodium chloroacetate with a mass of 0.8-1.2 times that of porous titanium dioxide is added. The pH value of the resulting mixture is adjusted to 11.5-12.5, and the mixture is reacted at 100-120℃ for 3-5 hours. The reaction solution is then filtered, the filter cake is washed with water until neutral, and then vacuum dried to obtain the final product.
5. The acrylic aging-resistant hot melt pressure-sensitive adhesive according to claim 4, characterized in that, The porous titanium oxide is prepared by ultrasonically dispersing titanium isopropoxide, dodecyl dimethyl tertiary amine, and deionized water at a mass ratio of 1:0.3-0.5:20-40. Then, hydrochloric acid aqueous solution with a mass of 0.2-0.4 times that of titanium isopropoxide and a concentration of 30-45wt% is added. After mixing and stirring evenly, the mixture is kept at 50-70℃ for 30-35 hours. After the reaction is complete, the filter cake in the reaction solution is filtered out and aged to obtain the final product.
6. The acrylic aging-resistant hot melt pressure-sensitive adhesive according to claim 5, characterized in that, The aging temperature is 110-130℃, and the aging time is 35-45h.
7. The acrylic aging-resistant hot melt pressure-sensitive adhesive according to claim 1, characterized in that: The antioxidant is any one of antioxidant 1010, antioxidant 168, antioxidant 1076, and antioxidant 1024.
8. The acrylic aging-resistant hot melt pressure-sensitive adhesive according to claim 1, characterized in that: The ultraviolet absorber is any one of 2-hydroxy-5-chlorobenzophenone, 2-hydroxy-4-alkoxybenzophenone, and 2-(2-hydroxy-3,5-di-tert-pentylphenyl)benzotriazole.
9. A method for preparing an acrylic-based aging-resistant hot-melt pressure-sensitive adhesive according to any one of claims 1-8, characterized in that, The process includes the following steps: Weigh each raw material according to the formula, then add lauryl methacrylate to the acrylate prepolymer, stir to dissolve, add 1-hydroxycyclohexylphenyl ketone, continue stirring to dissolve, then add the remaining raw materials, mix and stir evenly, apply the resulting adhesive to a polyester film, cover with a release film to isolate oxygen, and cure under UV light to obtain an acrylic aging-resistant hot melt pressure-sensitive adhesive.
10. An acrylic-based aging-resistant hot melt pressure-sensitive adhesive according to claim 9, characterized in that: The energy of the UV light during curing is 300-750 mJ / cm. 2 And the curing time is 6-8 minutes.