A PUA adhesive for pressurized sealing reinforcement layer of gas leaks in GIS equipment

By modifying PUA adhesives to enhance the crosslinking density and interfacial bonding strength of GIS equipment adhesives, the problems of insufficient penetration and adhesion under high pressure are solved, achieving long-lasting sealing and sealing effects that can be achieved without power interruption during construction.

CN123107613APending Publication Date: 2026-11-17STATE GRID GANSU ELECTRIC POWER RESEARCH INSTITUTE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611555694.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The adhesives used for pressurized sealing reinforcement layers of gas leaks in existing GIS equipment are prone to penetration and have insufficient adhesion under high pressure, failing to meet long-term sealing requirements. Furthermore, they are prone to cracking under high-frequency vibration environments and cannot be adapted for live-line construction without power interruption.

Method used

The PUA adhesive modified with polyurethane acrylate is improved by introducing double bond-modified fumed silica and photoinitiator, thereby increasing the crosslinking density and interfacial bonding strength, enhancing its impermeability and weather resistance, and forming a highly adhesive elastic sealing layer.

Benefits of technology

It effectively resists SF6 gas penetration under pressure of 0.4~0.7MPa, extends the sealing life, is suitable for live-line construction without power interruption, and reduces power outage losses during operation and maintenance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107613A_ABST
    Figure CN123107613A_ABST
Patent Text Reader

Abstract

This invention relates to a PUA adhesive for reinforcing layers of pressurized gas leak sealing in GIS equipment. The adhesive is composed of the following components in chemical equivalents: 5-12 equivalents of PUA prepolymer, 1 equivalent of HDDA, 0.1-0.5 equivalents of double-bond modified fumed silica, and 0.05-0.6 equivalents of photoinitiator 819. This invention improves the curing rate and can be directly used for outer layer reinforcement protection after SF6 leak sealing in GIS equipment, significantly extending the outdoor service life of the sealing structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of pressurized gas leak sealing technology for GIS equipment, and more particularly to a PUA adhesive for a reinforcing layer of pressurized gas leak sealing for GIS equipment. Background Technology

[0002] The adhesive for the pressurized sealing reinforcement layer of gas leaks in GIS equipment is a special sealing material developed for live-line leak sealing scenarios without power interruption. It relies on a carbon nanotube modified resin system to achieve high-strength bonding with metal flanges and bolt substrates. After curing, it can withstand SF6 operating pressure of 0.3~1.0MPa, replacing the high-cost solution of replacing seals during traditional shutdown. In recent years, it has been gradually promoted in the operation and maintenance of power grids and self-owned power plants.

[0003] Currently, adhesives for pressurized sealing reinforcement layers of gas leaks in GIS equipment can be divided into three categories based on their functional characteristics: The first category is general-purpose epoxy-modified adhesives, suitable for conventional flange leakage scenarios. They cure at room temperature, are easy to operate, and are mostly used for ordinary sealing reinforcement under operating pressures below 0.5 MPa. The second category is superpolymer carbon composite adhesives, which rely on nano-carbon fillers to achieve high-strength adhesion and impermeability, and can withstand pressures above 1.0 MPa, making them suitable for high-temperature, high-load GIS equipment. The third category is modified adhesives specifically for damp surfaces, which can cure under conditions of condensation and small amounts of oil on the equipment surface, solving the problem of pressurized sealing in humid environments in outdoor substations. All three types of products are suitable for uninterrupted live-line operation requirements and can be flexibly selected according to the leak pressure and environmental conditions to meet different levels of long-term sealing needs.

[0004] Traditional sealing adhesives generally suffer from insufficient adhesion and poor impermeability, making them unable to resist the continuous penetration of SF6 small molecules under operating pressures of 0.4~0.7MPa. They are also easily dispersed by airflow, making them unsuitable for live, pressurized installations. Replacing the sealing rings requires a complete shutdown and power outage, resulting in losses of millions of units of power or production. Currently, adhesives for reinforcing layers are mostly prepared using aerospace-grade resin composite nano-carbon materials. They exhibit high adhesion strength to commonly used GIS materials such as steel, aluminum, and ceramics, with a compressive strength exceeding 72 MPa after curing. They also possess anti-aging, vibration-resistant, and resistant-to-SF6 decomposition product corrosion properties. The reinforcing layer can be applied in confined spaces without open flame, achieving long-term sealing without equipment disassembly or power outages. However, the industry still faces three common problems: insufficient adhesion of aluminum flange surfaces, making them prone to detachment; incomplete sealing of micro-gap penetration; mismatch between on-site curing cycle and power grid operation ticket duration; and some common modified adhesives have shortcomings such as poor resistance to SF6 decomposition product corrosion and re-leakage after 3-6 months of long-term operation, making it difficult to meet the maintenance requirements of 3-5 years of long-term sealing.

[0005] The PUA adhesive used for the pressurized sealing reinforcement layer of gas leaks in GIS equipment is a special sealing material modified with polyurethane acrylate. It combines the high flexibility of polyurethane with the strong weather resistance of acrylate. After curing, the shear strength can reach more than 8MPa. It can form a highly adhesive elastic sealing layer on the surface of GIS metal flanges and is suitable for SF6 operating pressures of 0.4~0.7MPa. Taking the polyether-type PUA adhesive adapted for the pressurized sealing reinforcement layer of GIS equipment as an example, it uses polyether diol with Mn=2000 and toluene diisocyanate as core raw materials. After synthesizing the terminal isocyanate prepolymer in two steps, methacrylate-β-hydroxypropyl ester is added to complete the end-capping. The final product has a viscosity of about 6900 mPa·s, and the hardness of the cured adhesive layer is 57 HD and the shear strength can reach 8.19 MPa. It combines the high flexibility of polyurethane with the weather resistance of acrylate, and can tightly adhere to the surface of the metal flange of GIS equipment, buffering the vibration and micro-deformation generated by the operation of the equipment, effectively resisting the penetration of SF6 gas within 0.7 MPa. At the same time, it obtains a 25% LOI flame retardant index through phosphorus and nitrogen element modification, which meets the safety requirements of live and pressurized operation in substations. It can complete the reinforcement sealing of leaks without stopping the machine, which greatly reduces the power outage losses of power grid operation and maintenance.

[0006] Polyether-based PUA adhesives are used for pressurized sealing reinforcement layers of gas leaks in GIS equipment. Their advantages include excellent flexibility, buffering vibrations and flange micro-deformations during equipment operation, resistance to stress cracking, and maintenance of sealing performance even at low temperatures, making them suitable for complex outdoor substation conditions. However, their high ether bond ratio in the molecular chain makes them prone to chain breakage and degradation when in prolonged contact with highly corrosive media such as hydrogen fluoride and sulfur dioxide produced by SF6 decomposition within GIS equipment, leading to rapid attenuation of adhesive adhesion. Furthermore, the pure polyether system has a relatively low upper limit for crosslinking density, resulting in insufficient resistance to SF6 small molecules under high pressure conditions above 0.7 MPa, making it prone to micro-leakage after long-term operation. Additionally, the limited cohesive strength of polyether segments makes the adhesive layer susceptible to localized stress cracking under long-term high-frequency vibrations in GIS equipment, making it unsuitable for long-term sealing requirements exceeding 3 years when used alone as a reinforcement layer. Summary of the Invention

[0007] The technical problem to be solved by the present invention is to provide a PUA adhesive for pressurized sealing reinforcement layer of gas leakage in GIS equipment that improves curing efficiency and service life.

[0008] To solve the above problems, the present invention provides a PUA adhesive for a pressurized sealing reinforcement layer for gas leaks in GIS equipment, characterized in that the adhesive is composed of the following components in chemical equivalent parts: 5-12 equivalents of PUA prepolymer, 1 equivalent of HDDA, 0.1-0.5 equivalents of double-bond modified fumed silica, and 0.05-0.6 equivalents of photoinitiator 819.

[0009] The PUA prepolymer is a hydroxyethyl acrylate modified trimer HDI prepolymer, synthesized as follows: In a three-necked flask equipped with a stirrer, reflux condenser, and thermometer, 4 equivalents of HDI trimer and 3 equivalents of ACMO are added respectively, stirred and mixed evenly, and heated to 40~60℃; then, a pre-dissolved 3 equivalents of hydroxyethyl acrylate mixed solution containing 0.01~0.05 equivalents of p-hydroxyanisole is added dropwise in batches; after the temperature stabilizes, the reaction temperature of the system is raised to 60~70℃ and reacted for 1 hour; after 1 hour, a 3% (w / w) ACMO solution of stannous octoate is added dropwise; the reaction is carried out at 60~70℃ for 1 hour, and then raised to 70~80℃ and reacted for 4 hours; the reaction is stopped, the temperature is lowered to 50℃, the product is poured out, sealed and stored.

[0010] The double-bond modified fumed silica was synthesized as follows: 1 equivalent of unmodified fumed silica was added to 30 equivalents of anhydrous ethanol; the resulting mixed solution was sonicated in an ultrasonic instrument for 0.5–1 h to uniformly disperse the silica in the ethanol solution, thus obtaining a fumed silica solution; then 5 equivalents of silane coupling agent were added to a three-necked flask containing 10 equivalents of deionized water, and magnetically stirred for 0.5–1 h to ensure complete hydrolysis of the silane coupling agent; the fumed silica solution was added to the three-necked flask, and after thorough mixing, it was placed in a constant-temperature magnetic stirrer and reacted at 40–80 °C for 6 h; the resulting reaction product was filtered, washed, and then vacuum dried at 80–100 °C for 3–6 h.

[0011] The preparation method of PUA adhesive for pressurized sealing reinforcement layer of gas leakage in GIS equipment as described above is characterized by: firstly, weighing according to the ratio; then mixing PUA prepolymer, HDDA, and double bond modified fumed silica at room temperature, stirring evenly and letting stand to eliminate bubbles, thus obtaining a mixed solution; under room temperature and light-protected conditions, adding photoinitiator 819 to the mixed solution, and quickly stirring and mixing evenly to form PUA adhesive for reinforcement layer.

[0012] Compared with the prior art, the present invention has the following advantages: 1. This invention improves the adhesive's resistance to highly corrosive media and the crosslinking density of the curing system by preparing a non-polyether type PUA prepolymer, thereby increasing its resistance to small molecules and extending the service life of the PUA sealing layer.

[0013] 2. This invention improves the curing rate of the reinforcing layer PUA adhesive by photo-initiated curing of PUA, while ensuring the interfacial bonding strength with the underlying PUA adhesive.

[0014] 3. This invention improves the crosslinking density and strength of the reinforced PUA adhesive by introducing a silica filler containing double bonds into the PUA adhesive, thereby enhancing the weather resistance of the adhesive coating.

[0015] 4. The adhesive of this invention has a similar structure to the matching primer and sealing adhesive, excellent interface compatibility, and no obvious phase separation. It can be directly used for the outer layer reinforcement protection after SF6 leakage sealing of GIS equipment, which greatly extends the outdoor service life of the sealing structure. Attached Figure Description

[0016] The specific embodiments of the present invention will be described in further detail below with reference to the accompanying drawings.

[0017] Figure 1 The PUA prepolymer in Example 1 of this invention 1 H-NMR spectrum.

[0018] Figure 2 The images show the FT-IR spectra of modified gaseous silicon (left) and double-bond modified gaseous silicon (right) in Example 1 of this invention.

[0019] Figure 3 This is the FT-IR image of the PUA curing coating in Embodiment 1 of the present invention.

[0020] Figure 4 This is the FT-IR image of the PUA curing coating in Embodiment 2 of the present invention.

[0021] Figure 5 This is the FT-IR image of the PUA curing coating in Embodiment 3 of the present invention. Detailed Implementation

[0022] A PUA adhesive for a pressurized sealing reinforcement layer for gas leaks in GIS equipment is provided. The adhesive is composed of the following components in chemical equivalent parts according to the requirements of GIS pressurized sealing scenarios: 5-12 equivalents of PUA prepolymer (PUA main component), 1 equivalent of HDDA (1,6-hexanediol diacrylate, active monomer), 0.1-0.5 equivalents of double bond modified fumed silica (inorganic filler), and 0.05-0.6 equivalents of photoinitiator 819 (photoinitiator).

[0023] The PUA prepolymer is a hydroxyethyl acrylate-modified trimer of HDI, synthesized as follows: In a three-necked flask equipped with a stirrer, reflux condenser, and thermometer, 4 equivalents of HDI trimer (hexamethylene diisocyanate trimer) and 3 equivalents of ACMO (4-acryloylmorpholine) were added separately, stirred until homogeneous, and heated to 40-60°C. Then, a pre-dissolved 3 equivalents of hydroxyethyl acrylate solution containing 0.01-0.05 equivalents of p-hydroxyanisole was added dropwise. After the temperature stabilized, the reaction temperature was raised to 60-70°C and reacted for 1 hour. After 1 hour, a 3% (w / w) ACMO solution of stannous octoate was added dropwise. The reaction was continued at 60-70°C for 1 hour, then raised to 70-80°C and reacted for 4 hours. The reaction was stopped, cooled to 50°C, and the product was poured out and sealed for storage. The obtained product is the PUA prepolymer, and its synthesis route is shown below: Double-bond modified fumed silica was synthesized as follows: One equivalent of unmodified fumed silica was added to 30 equivalents of anhydrous ethanol. The resulting mixture was sonicated for 0.5–1 h to ensure uniform dispersion of silica in the ethanol solution, yielding a fumed silica solution. Then, 5 equivalents of silane coupling agent were added to a three-necked flask containing 10 equivalents of deionized water and magnetically stirred for 0.5–1 h to ensure complete hydrolysis of the silane coupling agent. The fumed silica solution was added to the three-necked flask and thoroughly mixed. The mixture was then placed in a constant-temperature magnetic stirrer and reacted at 40–80 °C for 6 h. The resulting reaction product was filtered and washed three times with a washing solution of anhydrous ethanol and purified water at a 1:1 volume ratio (mL / mL). After washing, the sample was placed in a vacuum drying oven and vacuum dried at 80–100 °C for 3–6 h.

[0024] The process of modifying fumed silica with silane coupling agents involves the hydrolysis of the coupling agent's alkoxy groups to generate silanols, followed by dehydration with the silanols on the silica surface to form Si–O–Si covalent bonds. The general reaction equation is: Hydrolysis reaction: YR-Si(OR′)3+3H2O→YR-Si(OH)3+3R′OH Condensation grafting: YR-Si(OH)3+3≡Si-OH (表面) →YR-Si(-O- Si≡)3+3H2O A method for preparing a PUA adhesive for a pressurized sealing reinforcement layer of gas leaks in GIS equipment: First, weigh according to the ratio; then mix PUA prepolymer, HDDA, and double bond modified fumed silica at room temperature, stir evenly and let stand to eliminate bubbles to obtain a mixed solution; under room temperature and light-protected conditions, add photoinitiator 819 to the mixed solution, stir quickly and mix evenly (if bubbles are generated, let stand in the dark to eliminate them) to form a PUA adhesive for the reinforcing layer.

[0025] When using, apply the reinforcing layer with PUA adhesive according to the requirements of QGDW 12161-2021 "Technical Specification for Leakage Sealing of Gas Insulated Metal Enclosed Electrical Equipment" to the surface of the already dried primer resin; irradiate with ultraviolet light until surface dry; after surface dry, heat the PUA curing resin at 80~100℃ for 12~24 hours with heating equipment until the coating is completely cured, and then evaluate the performance of the cured coating.

[0026] PUA adhesive curing mode for the reinforcement layer: The photocuring of PUA (polyurethane acrylate) is essentially a free radical chain addition polymerization reaction that occurs when the terminal acrylate double bonds are activated by a photoinitiator. The general reaction formula is as follows: nPUA-(CH2=CH−COO−R)m→ [-CH2-CH(COO-R-PUA-R-COO)-]n (hν, photoinitiator) The free radical polymerization of PUA double bonds is accompanied by the copolymerization of active monomer HDDA, double bond-modified fumed silica, and solvent double bonds in PUA.

[0027] Example 1 S1 Synthesis of PUA Prepolymer: In a 500 mL three-necked flask equipped with a stirrer, reflux condenser, and thermometer, 119.96 g of HDI trimer and 89.87 g of ACMO were added separately and stirred until homogeneous. The mixture was then heated to 50°C. Next, a pre-dissolved solution of 90.10 g of hydroxyethyl acrylate containing 0.62 g of p-hydroxyanisole was added dropwise. Once the temperature stabilized, the reaction temperature was raised to 65°C and the reaction was carried out for 1 hour. After 1 hour, 2 drops of a 3% (w / w) ACMO solution containing stannous octoate were added. The reaction was carried out at 70°C for 1 hour, then raised to 80°C and reacted for 4 hours. The reaction was stopped, the temperature was lowered to 50°C, the product was poured out, and sealed for storage. The obtained product is the PUA prepolymer.

[0028] The viscosity of the synthesized PUA prepolymer was tested using a rotating digital viscometer, and the result was 3383 mPa·s.

[0029] use 1 The structure of the PUA prepolymer was characterized by H-NMR, and the results are as follows: Figure 1As shown in the figure, the characteristic peaks of the solvent acrylomorpholine are: the peaks at ~6.55 ppm, 6.30 ppm, and 5.75 ppm belong to the CH double bond of acrylomorpholine; the peaks at ~4.30 ppm and 3.15 ppm belong to the CH adjacent to the O atom and the CH adjacent to the N atom of acrylomorpholine, respectively.

[0030] The characteristic peaks of the PUA prepolymer are as follows: the peaks at ~6.45 ppm, 6.20 ppm, and 5.87 ppm belong to the CH double bond of acrylate; the peaks at ~4.30 ppm, 3.80 ppm, 3.70 ppm, and 3.55 ppm belong to the CH adjacent to the O atom of hydroxyethyl acrylate (two characteristic peaks), the -CH adjacent to the N atom of urethane, and the CH adjacent to the N atom of trimer HDI, respectively; the peak at ~4.90 ppm belongs to NH of urethane; and the peak at ~2.0-0.5 ppm belongs to the saturated CH in trimer HDI.

[0031] 1 H-NMR spectral analysis indicates that the PUA prepolymer was successfully synthesized.

[0032] S2 synthesis of double-bond modified gaseous silicon: Weigh 8.00 g of unmodified fumed silica and add it to 240 mL of anhydrous ethanol. Sonicate the resulting mixture in an ultrasonicator for 30 min to ensure uniform dispersion of silica in the ethanol solution, thus obtaining a fumed silica solution. Then, add 40 mL of silane coupling agent to a three-necked flask containing 80 mL of deionized water and stir magnetically for 30 min to ensure complete hydrolysis of the silane coupling agent. Add the fumed silica solution to the three-necked flask, mix thoroughly, and then react at 60 °C for 6 h in a constant-temperature magnetic stirrer. Filter the resulting reaction product and wash it three times with a washing solution of anhydrous ethanol and purified water at a 1:1 volume ratio (mL / mL). After washing, place the sample in a vacuum drying oven and dry under vacuum at 80 °C for 3 h.

[0033] The structure of double-bonded modified gaseous silicon was characterized by FT-IR, and the results are as follows: Figure 2 As shown in the figure, the infrared absorption characteristic peak of unmodified gaseous silicon in the left figure is mainly attributed to the Si-O-Si stretching vibration absorption at ~1150 cm⁻¹. -1 The characteristic peak is located at [location missing]; while in the infrared absorption spectrum of double-bonded modified gaseous silicon (right figure), the peak at ~1150 cm⁻¹ is attributed to the Si-O-Si stretching vibration absorption. -1 The characteristic peak at ~1100 cm⁻¹ corresponds to the COC stretching vibration absorption in the KH570 component. -1 The characteristic peaks overlap at this point, increasing the absorption half-width at half-maximum; simultaneously at ~1650 cm⁻¹-1 The characteristic peak at ~1730 cm⁻¹ is attributed to the absorption of unsaturated =CH stretching and out-of-plane bending vibrations. -1 The characteristic peak of C=O vibrational absorption appears at ~2900 cm⁻¹. -1 A characteristic peak at ~3500 cm⁻¹ appears, attributed to the absorption of CH stretching vibration. -1 The presence of characteristic peaks at the location is attributed to the OH stretching vibration absorption (KH570 alcoholysis produces silanol structures). The appearance of these characteristic peaks indicates that KH570 successfully modified the double bonds of gaseous silicon.

[0034] S3 PUA adhesive for preparing the reinforcing layer: Accurately weigh 4.03 g of PUA prepolymer, 0.41 g of HDDA, and 0.09 g of double-bond modified silica into a beaker at room temperature. Stir and mix thoroughly, then allow to stand to remove air bubbles. Add 0.18 g of photoinitiator 819 to the above solution at room temperature in the dark, and stir rapidly to mix thoroughly (if air bubbles are generated, allow to stand in the dark to remove them) to form the PUA adhesive for the reinforcing layer.

[0035] The viscosity of the prepared reinforcing layer PUA adhesive was tested using a rotating digital viscometer, and the result was 3435 mPa·s.

[0036] The reinforcing layer was applied to the already surface-dried primer resin surface using PUA adhesive according to the requirements of QGDW 12161-2021 "Technical Specification for Leakage Sealing of Gas-Insulated Metal-Enclosed Electrical Equipment". The reinforced layer was then irradiated with a UV lamp for 60 seconds to check if it was surface-dried (if not, irradiation continued until surface-dried). After surface drying, the PUA curing resin was heated to 80℃ and held for 12 hours until the coating was fully cured. The performance of the cured coating was then evaluated.

[0037] The structure of the reinforced PUA cured coating was characterized by FT-IR, and the results are as follows: Figure 3 As shown in the figure, the infrared characteristic peaks with high absorption in the cured coating are mainly divided into four regions: ~1100 cm⁻¹, which are attributed to the COC and Si-O-Si stretching vibration absorption. -1 The characteristic peak is located at ~1700 cm⁻¹, attributed to the C=O vibrational absorption. -1 The characteristic peak is located at ~2900 cm⁻¹, attributed to the absorption of saturated CH stretching vibration. -1 Characteristic peak at ~3500 cm⁻¹; attributed to the stretching vibration absorption of OH and NH. -1Characteristic peaks are observed. The COC and C=O structures originate from molecules such as ACMO, hydroxyethyl acrylate, HDDA, and PUA; the Si-O-Si structure originates from double-bond modified fumed silica; the saturated CH structure appears in all components (including ACMO, hydroxyethyl acrylate, HDDA, PUA, and KH570 modified fumed silica); the OH structure originates from double-bond modified fumed silica and hydroxyethyl acrylate; and the NH structure originates from the PUA component.

[0038] Due to the strong absorption properties of each functional group, the high content of functional groups in the cured coating, and the thickness of the coating, its infrared absorption intensity is close to 100%. That is, the corresponding infrared wavelength light cannot pass through this coating, which can protect the underlying adhesive.

[0039] Example 2 The synthesis of PUA prepolymer in S1 is the same as in Example 1.

[0040] S2 synthesis of double bond modified gaseous silicon is the same as in Example 1.

[0041] S3 PUA adhesive for preparing the reinforcing layer: Accurately weigh 2.21 g of PUA prepolymer, 0.40 g of HDDA, and 0.05 g of double-bond modified silica into a beaker at room temperature. Stir and mix thoroughly, then allow to stand to remove air bubbles. Add 0.02 g of photoinitiator 819 to the above solution at room temperature in the dark, and stir rapidly to mix thoroughly (if air bubbles are generated, allow to stand in the dark to remove them) to form the PUA adhesive for the reinforcing layer.

[0042] The viscosity of the prepared reinforcing layer PUA adhesive was tested using a rotating digital viscometer, and the result was 3272 mPa·s.

[0043] The reinforcing layer was applied to the already surface-dried primer resin surface using PUA adhesive according to the requirements of QGDW 12161-2021 "Technical Specification for Leakage Sealing of Gas-Insulated Metal-Enclosed Electrical Equipment". The reinforced layer was then irradiated with UV light for 3 minutes to check if it was surface-dried (if not, irradiation continued until surface-dried). After surface drying, the PUA curing resin was heated to 80 ℃ and held for 12 hours until the coating was fully cured. The performance of the cured coating was then evaluated.

[0044] The structure of the reinforced PUA cured coating was characterized by FT-IR, and the results are as follows: Figure 4 As shown in the figure, the infrared characteristic peaks with high absorption in the cured coating are mainly divided into four regions: ~1100 cm⁻¹, which are attributed to the COC and Si-O-Si stretching vibration absorption. -1 The characteristic peak is located at ~1700 cm⁻¹, attributed to the C=O vibrational absorption. -1The characteristic peak is located at ~2900 cm⁻¹, attributed to the absorption of saturated CH stretching vibration. -1 Characteristic peak at ~3500 cm⁻¹; attributed to the stretching vibration absorption of OH and NH. -1 Characteristic peaks are observed. The COC and C=O structures originate from molecules such as ACMO, hydroxyethyl acrylate, HDDA, and PUA; the Si-O-Si structure originates from double-bond modified fumed silica; the saturated CH structure appears in all components (including ACMO, hydroxyethyl acrylate, HDDA, PUA, and KH570 modified fumed silica); the OH structure originates from double-bond modified fumed silica and hydroxyethyl acrylate; and the NH structure originates from the PUA component.

[0045] Due to the strong absorption properties of each functional group, the high content of these functional groups in the cured coating, and the thickness of the coating, the intensity of each functional group in the characteristic infrared absorption peak region is close to 100%, but the absorption half-peak width is relatively low. Figure 3 It is relatively narrow, and can be clearly distinguished at ~3500 cm. -1 Location, ~2900 cm -1 The characteristic absorption peak distribution is at ~1100 cm⁻¹. -1 The absorption peak at that point is almost identical to the absorption peak at ~1700 cm⁻¹ of the C=O vibration. -1 The characteristic peaks clustered together indicate the strong stretching vibration absorption characteristics of COC and Si-O-Si.

[0046] Example 3 The synthesis of PUA prepolymer in S1 is the same as in Example 1.

[0047] S2 synthesis of double bond modified gaseous silicon is the same as in Example 1.

[0048] S3 PUA adhesive for preparing the reinforcing layer: Accurately weigh 4.38 g of PUA prepolymer, 0.39 g of HDDA, and 0.19 g of double-bond modified silica into a beaker at room temperature. Stir and mix thoroughly, then allow to stand to remove air bubbles. Add 0.20 g of photoinitiator 819 to the above solution at room temperature in the dark, and stir rapidly to mix thoroughly (if air bubbles are generated, allow to stand in the dark to remove them) to form the PUA adhesive for the reinforcing layer.

[0049] The viscosity of the prepared reinforcing layer PUA adhesive was tested using a rotating digital viscometer, and the result was 3639 mPa·s.

[0050] The reinforcing layer was applied to the already surface-dried primer resin surface using PUA adhesive according to the requirements of QGDW 12161-2021 "Technical Specification for Leakage Sealing of Gas-Insulated Metal-Enclosed Electrical Equipment". The reinforced layer was then irradiated with a UV lamp for 20 seconds to check if it was surface-dried (if not, irradiation continued until surface-dried). After surface drying, the PUA curing resin was heated to 80℃ for 12 hours until the coating was fully cured, and then the performance of the cured coating was evaluated.

[0051] The structure of the reinforced PUA cured coating was characterized by FT-IR, and the results are as follows: Figure 5 As shown in the figure, the infrared characteristic peaks with high absorption in the cured coating are mainly divided into four regions: ~1100 cm⁻¹, which are attributed to the COC and Si-O-Si stretching vibration absorption. -1 The characteristic peak is located at ~1700 cm⁻¹, attributed to the C=O vibrational absorption. -1 The characteristic peak is located at ~2900 cm⁻¹, attributed to the absorption of saturated CH stretching vibration. -1 Characteristic peak at ~3500 cm⁻¹; attributed to the stretching vibration absorption of OH and NH. -1 Characteristic peaks are observed. The COC and C=O structures originate from molecules such as ACMO, hydroxyethyl acrylate, HDDA, and PUA; the Si-O-Si structure originates from double-bond modified fumed silica; the saturated CH structure appears in all components (including ACMO, hydroxyethyl acrylate, HDDA, PUA, and KH570 modified fumed silica); the OH structure originates from double-bond modified fumed silica and hydroxyethyl acrylate; and the NH structure originates from the PUA component.

[0052] and Figure 3 Similarly, due to the strong absorption properties of each functional group, the high content of these groups in the cured coating, and the thickness of the coating, the infrared absorption intensity is close to 100%. This means that the corresponding infrared wavelengths cannot penetrate this coating, thus protecting the underlying adhesive. The high addition amount of modified fumed silica significantly contributes to the infrared absorption intensity, indicating that it can protect the underlying adhesive.

Claims

1. A PUA adhesive for GIS equipment gas leakage pressure plugging reinforcement layer, characterized in that: The adhesive is composed of the following components in chemical equivalent parts: 5-12 equivalents of PUA prepolymer, 1 equivalent of HDDA, 0.1-0.5 equivalents of double bond modified fumed silica, and 0.05-0.6 equivalents of photoinitiator 819.

2. The PUA adhesive for GIS equipment gas leakage zone pressure plugging reinforcement layer according to claim 1, characterized in that: The PUA prepolymer is a hydroxyethyl acrylate modified trimer HDI prepolymer, synthesized as follows: In a three-necked flask equipped with a stirrer, reflux condenser, and thermometer, 4 equivalents of HDI trimer and 3 equivalents of ACMO are added respectively, stirred and mixed evenly, and heated to 40~60℃; then, a pre-dissolved 3 equivalents of hydroxyethyl acrylate mixed solution containing 0.01~0.05 equivalents of p-hydroxyanisole is added dropwise in batches; after the temperature stabilizes, the reaction temperature of the system is raised to 60~70℃ and reacted for 1 hour; after 1 hour, a 3% (w / w) ACMO solution of stannous octoate is added dropwise; the reaction is carried out at 60~70℃ for 1 hour, and then raised to 70~80℃ and reacted for 4 hours; the reaction is stopped, the temperature is lowered to 50℃, the product is poured out, sealed and stored.

3. The PUA adhesive for GIS equipment gas leakage zone pressure plugging reinforcement layer according to claim 1, characterized in that: The double-bond modified fumed silica was synthesized as follows: 1 equivalent of unmodified fumed silica was added to 30 equivalents of anhydrous ethanol; the resulting mixed solution was sonicated in an ultrasonic instrument for 0.5–1 h to uniformly disperse the silica in the ethanol solution, thus obtaining a fumed silica solution; then 5 equivalents of silane coupling agent were added to a three-necked flask containing 10 equivalents of deionized water, and magnetically stirred for 0.5–1 h to ensure complete hydrolysis of the silane coupling agent; the fumed silica solution was added to the three-necked flask, and after thorough mixing, it was placed in a constant-temperature magnetic stirrer and reacted at 40–80 °C for 6 h; the resulting reaction product was filtered, washed, and then vacuum dried at 80–100 °C for 3–6 h.

4. The method for preparing the PUA adhesive for the GIS equipment gas leakage zone pressure plugging reinforcement layer according to any one of claims 1-3, characterized in that: First, weigh the components according to the specified ratio; then, mix the PUA prepolymer, HDDA, and double-bond modified silica at room temperature, stir until homogeneous, and let stand to remove air bubbles to obtain a mixed solution; under room temperature and light-protected conditions, add photoinitiator 819 to the mixed solution, and quickly stir until homogeneous to form a PUA adhesive for the reinforcing layer.