A low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling and its preparation method.

By preparing a compound of double-side-chain modified silicone oil with polyalphaolefin PAO-6 and branched saturated polyol ester in the same reaction system, the problem of balancing low viscosity and high flash point in liquid cooling media was solved, and the stability of dielectric cooling oil and the solubility of additives were improved.

CN123107634APending Publication Date: 2026-11-17JIANGSU AORUN ADVANCED MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611217060.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-12
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing liquid cooling media have shortcomings in balancing low viscosity and high flash point, and the long-term stability and additive solubility issues of alkyl-modified silicone oil physical mixing systems have not been effectively resolved.

Method used

A double-side-chain modified silicone oil was prepared by hydrosilylation reaction of 1-octene and 1-decene with polymethylhydrosiloxane in the same reaction system. The modified silicone oil was then compounded with polyalphaolefin PAO-6 and branched saturated polyol ester, and antioxidant mother liquor and passivation mother liquor were added to form a low-viscosity, high-flash-point dielectric cooling oil composition.

Benefits of technology

It achieves a balance of low viscosity, high flash point, low volatility, dielectric stability, and additive compatibility, improving appearance stability and dielectric properties during long-term storage and thermal cycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107634A_ABST
    Figure CN123107634A_ABST
Patent Text Reader

Abstract

This invention relates to the field of liquid cooling dielectric cooling materials, specifically disclosing a low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling and its preparation method. The composition comprises octyl-decyl co-modified methyl silicone oil (i.e., double-side-chain modified silicone oil), PAO-6, branched saturated polyol ester, antioxidant, metal passivator, polymethyl methacrylate, and polyether-modified polydimethylsiloxane. This invention introduces octyl and decyl side chains into the same reaction system and combines them with PAO-6, branched saturated polyol ester, and additive mother liquor, achieving a good overall balance between low viscosity, high flash point, low volatility, dielectric properties, additive dispersion stability, and material compatibility, making it suitable for immersion liquid cooling systems.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of liquid cooling dielectric cooling materials, specifically relating to a low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling and its preparation method. Background Technology

[0002] As the heat flux density of data centers, power electronic devices, energy storage devices, and high-power electronic modules continues to increase, traditional air cooling methods are gradually becoming limited in terms of heat dissipation efficiency, energy consumption, and noise control. Immersion liquid cooling, by directly immersing the heat-generating components in a dielectric coolant, allows the coolant to directly contact the chips, circuit boards, copper busbars, solder joints, connectors, and sealing materials, effectively reducing thermal resistance and improving localized hotspot issues.

[0003] Dielectric cooling oils used in immersion liquid cooling systems need to meet multiple performance requirements simultaneously. On one hand, the cooling oil needs to have low viscosity to reduce circulation pumping resistance and improve liquid flow heat transfer efficiency; on the other hand, it also needs to have a high flash point and low volatility to meet the safety and stability requirements of long-term high-temperature operation. Furthermore, since the cooling oil is in direct contact with electronic components, it should also have high breakdown voltage, high volume resistivity, low dielectric loss, low moisture content, low corrosivity, and good material compatibility.

[0004] Existing liquid cooling media mainly include fluorinated fluids, mineral oils, polyalphaolefins (PAOs), ester oils, silicone oils, and their compound systems. Fluorinated fluids have good electrical insulation and low viscosity, but suffer from high cost, environmental durability, and supply stability issues. Mineral oils are relatively inexpensive, but their complex composition and deficiencies in anti-aging properties, material compatibility, and batch stability are problematic. PAO base oils have low viscosity and good low-temperature performance, but when relying solely on PAOs, flash point, additive solubility, and long-term oxidation resistance still require further optimization. Ester base oils have good additive solubility, but their high polarity may lead to increased water absorption and dielectric loss when used alone in large quantities. Ordinary dimethyl silicone oil has good chemical stability, but there is still room for optimization in its comprehensive compatibility with hydrocarbon base oils, some additives, and sealing materials.

[0005] Long-chain alkyl-modified silicone oils, by introducing alkyl side chains onto the siloxane backbone, can improve the compatibility between silicone oil and hydrocarbon base oils and can be used as liquid cooling dielectrics. However, existing alkyl-modified silicone oil systems still have room for further optimization when used in immersion liquid cooling. For example, a single, shorter alkyl side chain is beneficial for reducing viscosity and improving low-temperature fluidity, but its flash point and high-temperature volatility are relatively insufficient; a single, longer alkyl side chain is beneficial for increasing flash point and reducing volatility, but its low-temperature transparency and low-temperature fluidity are easily affected.

[0006] If different alkyl-modified silicone oils are physically mixed, different alkyl silicone oil components can be introduced into the macroscopic composition at the same time. However, there may still be differences in composition and compatibility between different alkyl silicone oil molecules. During long-term cold and heat cycling, high-temperature storage or cyclic operation, problems such as decreased appearance stability, local component shift or increased dielectric loss may occur.

[0007] Furthermore, submersible liquid cooling oils come into prolonged contact with copper, aluminum, tin solder, nickel-plated parts, sealing rubber, plastic housings, and electronic packaging materials during operation. To meet long-term operating requirements, antioxidants, metal passivators, viscosity-temperature regulators, and defoamers are typically added to the cooling oil. However, these additives have limited solubility in low-polarity alkyl silicone oils and polyalphaolefin systems, and direct addition can easily cause turbidity, excessively high local concentrations, precipitation, increased dielectric loss, and unstable foam control.

[0008] Therefore, there is an urgent need to provide a low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling and its preparation method that can take into account low viscosity, high flash point, low volatility, dielectric stability, additive compatibility and metal protection capabilities. Summary of the Invention

[0009] The purpose of this invention is to provide a low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling and its preparation method, in order to solve the problems of existing liquid cooling dielectric oils that are difficult to balance low viscosity and high flash point, insufficient long-term stability of physical mixing systems of different alkyl-modified silicone oils, and insufficient solubility and dispersion stability of trace additives in low-polarity base oil systems.

[0010] To achieve the above objectives, the present invention provides a method for preparing a low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling, comprising the following steps: Step (1) Under dry nitrogen protection, polymethylhydrosiloxane, 1-octene and 1-decene are subjected to hydrosilylation reaction in the same reaction system. After treatment with activated carbon, filtration and de-boiling point removal, double-side chain modified silicone oil is obtained. In the above process, 1-octene and 1-decene undergo hydrosilylation reactions with Si-H in polymethylhydrosiloxane through terminal carbon-carbon double bonds, respectively, introducing octyl and decyl groups onto the side groups of the siloxane backbone. The dual-side-chain modified silicone oil of this invention refers to octyl-decyl co-modified methyl silicone oil, which is prepared by 1-octene and 1-decene participating in a hydrosilylation reaction together in the same reaction system; the dual-side-chain designation distinguishes it from single octyl-modified silicone oil, single decyl-modified silicone oil, and mixtures of octyl-modified and decyl-modified silicone oils prepared separately and then physically mixed.

[0011] Step (2) Vacuum dehydrate the double-side-chain modified silicone oil, polyalphaolefin PAO-6 (PAO-6), and branched saturated polyol ester respectively; Step (3) Reserve a portion of PAO-6 from the total amount of PAO-6 to prepare antioxidant mother liquor, and reserve a portion of branched saturated polyol ester from the total amount of branched saturated polyol ester to prepare passivation mother liquor; after mixing the double-side-chain modified silicone oil, PAO-6 and branched saturated polyol ester, add the antioxidant mother liquor and passivation mother liquor. Step (4) Add polymethyl methacrylate and polyether-modified polydimethylsiloxane, and then degas and filter under vacuum to obtain the liquid cooling low viscosity high flash point dielectric cooling oil composition.

[0012] Preferably, in step (1), the ratio of the total molar amount of carbon-carbon double bonds in 1-octene and 1-decene to the molar amount of Si-H in polymethylhydrosiloxane is 1.08~1.15:1. The hydrosilylation reaction uses a Karstedt catalyst with a catalyst dosage of 5~20 ppm (calculated as platinum), a reaction temperature of 75~95℃, and a reaction time of 3~6h. The conditions for removing low-boiling points are: temperature 120~150℃, gauge pressure -0.098MPa~-0.095MPa, and time 2~5h.

[0013] Preferably, in step (1), the molar ratio of 1-octene to 1-decene is 30:70 to 70:30.

[0014] Preferably, the preparation method of the antioxidant mother liquor and the passivation mother liquor includes the following steps: Based on 100 parts by weight of the finished oil, 0.30~0.55 parts by weight of 4,4'-dioctyl diphenylamine and 0.18~0.40 parts by weight of isooctyl ester of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate are dissolved in the reserved PAO-6 to obtain an antioxidant mother liquor; Based on 100 parts by weight of the finished oil, 0.05 to 0.12 parts by weight of N,N-di(2-ethylhexyl)-1H-methylbenzotriazole-1-methylamine are dissolved in the reserved branched saturated polyol ester to obtain the passivation mother liquor. The reserved PAO-6 is included in the total amount of PAO-6 used, and the reserved branched saturated polyol ester is included in the total amount of branched saturated polyol ester used.

[0015] Through the above technical solutions, 4,4'-dioctyldiphenylamine, an oil-soluble diarylamine antioxidant, can inhibit the growth of oxidation chains caused by peroxy free radicals at high temperatures; β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate isooctyl ester, a liquid hindered phenolic antioxidant, can capture initial free radicals through hindered phenolic hydroxyl groups. The combination of these two can form a synergistic antioxidant system of amine and phenol, while the liquid and branched structure helps to avoid low-temperature crystallization. The methylbenzotriazole ring in N,N-di(2-ethylhexyl)-1H-methylbenzotriazole-1-methylamine can undergo coordination adsorption with copper, tin solder, and copper alloy surfaces, forming a metal passivation protective layer; the N,N-di(2-ethylhexyl)aminomethyl structure improves the oil solubility of this benzotriazole derivative in low-polarity silicone oil and PAO base oil, making it more suitable for anhydrous dielectric cooling oil systems compared to ordinary benzotriazole.

[0016] Preferably, based on 100 parts by weight of the finished oil, the following components are used: 55-66 parts by weight of the double-side-chain modified silicone oil, 18-28 parts by weight of PAO-6, 8-16 parts by weight of the branched saturated polyol ester, 0.30-0.55 parts by weight of 4,4'-dioctyl diphenylamine, 0.18-0.40 parts by weight of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate isooctyl ester, 0.05-0.12 parts by weight of N,N-di(2-ethylhexyl)-1H-methylbenzotriazole-1-methylamine, 0.10-0.35 parts by weight of polymethacrylate, and 0.01-0.08 parts by weight of polyether-modified polydimethylsiloxane. The amounts of each component are selected within the above ranges, and the total amount of the finished oil is 100 parts by weight.

[0017] Preferably, in step (2), the vacuum dehydration conditions are: temperature 60~80℃, gauge pressure -0.095MPa~-0.080MPa, and time 1~3h.

[0018] Preferably, in step (3), the branched saturated polyol ester is selected from one or more of trimethylolpropane tri(ethylhexanoate), pentaerythritol tetra(2-ethylhexanoate), and neopentyl glycol di(ethylhexanoate).

[0019] Preferably, in step (4), the polymethacrylate is a methacrylate copolymer containing C8~C18 alkyl ester side groups, and its weight-average molecular weight is 30,000~200,000; the polyether-modified polydimethylsiloxane is a polydimethylsiloxane with methyl-terminated polyether side-linked branches, and its active ingredient content is not less than 90 wt%.

[0020] This invention also provides a low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling, comprising, based on 100 parts by weight, 55-66 parts by weight of double-side-chain modified silicone oil, 18-28 parts by weight of PAO-6, 8-16 parts by weight of branched saturated polyol ester, 0.30-0.55 parts by weight of 4,4'-dioctyl diphenylamine, 0.18-0.40 parts by weight of isooctyl β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 0.05-0.12 parts by weight of N,N-di(2-ethylhexyl)-1H-methylbenzotriazole-1-methylamine, 0.10-0.35 parts by weight of polymethacrylate, and 0.01-0.08 parts by weight of polyether-modified polydimethylsiloxane. The amounts of each component are selected within the above ranges, and the total composition is 100 parts by weight.

[0021] The dual-side-chain modified silicone oil is prepared by hydrosilylation reaction of polymethylhydrosiloxane, 1-octene, and 1-decene in the same reaction system. Since 1-octene and 1-decene simultaneously participate in the Si-H addition of polymethylhydrosiloxane in the same hydrosilylation reaction system, the resulting dual-side-chain modified silicone oil is distinct from mixed silicone oils prepared separately as octyl-modified silicone oil and decyl-modified silicone oil and then physically mixed. The dual-side-chain modified silicone oil, based on the feed ratio and reaction conversion results, contains, on average, methyloctylsiloxane and methyldecylsiloxane repeating units; this description does not require that each individual molecule have an identical repeating unit sequence, nor does it require the separation and determination of the repeating unit sequence of each individual molecule.

[0022] Preferably, after preparation, the residual Si-H content of the dual-side-chain modified silicone oil is not higher than 10 ppm, more preferably not higher than 1 ppm; the total residual 1-octene and 1-decene content is not higher than 0.5 wt%, more preferably not higher than 0.2 wt%; and the moisture content is not higher than 100 ppm, more preferably not higher than 50 ppm. The residual Si-H content, the total residual 1-octene and 1-decene content, and the moisture content are used as indicators for reaction conversion and product quality control, and are used to evaluate the preparation stability of the dual-side-chain modified silicone oil.

[0023] Preferably, the kinematic viscosity of the obtained low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling is 9.5–13.0 mm at 40°C. 2 / s, open flash point not lower than 224℃, evaporation loss at 150℃×24h not higher than 1.2wt%, breakdown voltage not lower than 55kV / 2.5mm, dielectric loss factor at 1kHz not higher than 0.0020, and moisture content not higher than 50ppm.

[0024] Preferably, based on 100 parts by weight of the total composition, the double-side-chain modified silicone oil comprises 58-62 parts by weight, PAO-6 comprises 22-25 parts by weight, the branched saturated polyol ester comprises 14-16 parts by weight, 4,4'-dioctyl diphenylamine comprises 0.38-0.46 parts by weight, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate isooctyl ester comprises 0.24-0.32 parts by weight, N,N-di(2-ethylhexyl)-1H-methylbenzotriazole-1-methylamine comprises 0.06-0.10 parts by weight, polymethacrylate comprises 0.20-0.32 parts by weight, and polyether-modified polydimethylsiloxane comprises 0.02-0.06 parts by weight.

[0025] Preferably, the polymethacrylate is a methacrylate copolymer containing C8~C18 alkyl ester side groups, and the polyether-modified polydimethylsiloxane is a polydimethylsiloxane with methyl-terminated polyether side-linked branches.

[0026] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are: 1. This invention employs a hydrosilylation reaction between 1-octene and 1-decene and polymethylhydrosiloxane in the same reaction system. The resulting dual-side-chain modified silicone oil, based on the feed ratio and reaction conversion results, contains an average of methyloctylsiloxane and methyldecylsiloxane units. The octyl side chain helps reduce the system's low-temperature viscosity and kinematic viscosity at 40°C, while the decyl side chain helps increase the flash point and reduce volatility. Co-modification with both avoids the problems of insufficient flash point of single short-chain alkyl silicone oils or low-temperature turbidity and increased viscosity of single long-chain alkyl silicone oils. Compared to a simple physical mixture of octyl-modified and decyl-modified silicone oils, this dual-side-chain modified silicone oil helps reduce the component differences between different alkyl silicone oil molecules, thereby improving the appearance stability and dielectric stability during long-term storage, high-temperature operation, and thermal cycling.

[0027] 2. This invention uses a dual-side-chain modified silicone oil as the main base oil, and combines it with PAO-6 and branched saturated polyol esters to form a ternary base oil system. The dual-side-chain modified silicone oil provides a base of low dielectric constant, high flash point, and low volatility; PAO-6 helps reduce system viscosity and improve low-temperature fluidity; and the branched saturated polyol ester helps improve the solubility and dispersion of antioxidants and metal passivators in low-polarity systems. The combination of these three components allows the composition to achieve a balance of low viscosity, high flash point, low-temperature transparency, dielectric stability, and additive compatibility.

[0028] 3. In this invention, 4,4'-dioctyl diphenylamine and β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate isooctyl ester are pre-prepared as an antioxidant mother liquor, and N,N-di(2-ethylhexyl)-1H-methylbenzotriazole-1-methylamine are pre-prepared as a passivation mother liquor, which are then added to a ternary base oil system. This method of adding the mother liquor helps improve the dispersion uniformity of trace additives in a low-polarity base oil system, reducing issues such as turbidity, precipitation, unstable foam control, or increased dielectric loss caused by excessively high local concentrations. Attached Figure Description

[0029] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0030] Figure 1 This is a schematic diagram of the preparation process of the low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling of the present invention; Figure 2 This is a comparison chart of the kinematic viscosity at 40°C of the low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling of the present invention. Figure 3 A comparison chart of flash points of the low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling of the present invention; Figure 4 A comparison diagram of evaporation loss of the low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling of the present invention; Figure 5 This is a comparison chart of dielectric loss factors of the low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling of the present invention. Figure 6 This is a comparison diagram of the material compatibility of the low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling of the present invention. Detailed Implementation

[0031] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0032] Unless otherwise specified, the following parts by weight are all based on 100 parts by weight of the total finished oil. The amount of each component is selected within the corresponding range to ensure that the total amount of the composition is 100 parts by weight.

[0033] The polymethylhydrosiloxane used in this invention is preferably a trimethylsiloxy-terminated methylhydrosiloxane-dimethylsiloxane copolymer with a kinematic viscosity of 10~80 mmHg at 25°C. 2 / s, Si-H hydrogen mass fraction 0.10~1.60wt%, moisture content not greater than 100ppm. The purity of 1-octene and 1-decene is preferably not less than 98.5%, and they are dehydrated by molecular sieve before use. PAO-6 has a kinematic viscosity of approximately 6mm at 100℃. 2 / s of polyalphaolefin base oil. The polymethacrylate is preferably a methacrylate copolymer containing C8-C18 alkyl ester side groups, with a weight-average molecular weight of 30,000-200,000; the polyether-modified polydimethylsiloxane is preferably a methyl-terminated polyether-branched polydimethylsiloxane, with an active ingredient content of not less than 90 wt%. The above limitations are used to improve the low-temperature flow stability and foam control stability of the composition.

[0034] The dual-side-chain modified silicone oil in this invention is prepared by simultaneously reacting 1-octene and 1-decene with the Si-H groups of polymethylhydrosiloxane in the same reaction system via hydrosilylation, rather than by physically mixing pre-prepared octyl-modified silicone oil and decyl-modified silicone oil. The average composition containing methyloctylsiloxane and methyldecylsiloxane repeating units refers to the average composition determined based on the molar ratio of 1-octene and 1-decene, Si-H conversion control, residual Si-H control, and residual olefin control; the repeating unit sequence of each individual molecule is not required to be specified.

[0035] During the production or experimentation process of this invention, quality control can be achieved through indicators such as feed metering, reaction exothermics and Si-H consumption, residual Si-H content, residual 1-octene and 1-decene content, moisture content, and appearance and viscosity after de-boiling point removal. The residual Si-H content is evaluated using conventional chemical analysis methods or rapid infrared detection methods suitable for detecting hydrogen content in organosilicon; the residual 1-octene and 1-decene content is evaluated using gas chromatography; and the moisture content is evaluated using the Karl Fischer method.

[0036] To ensure batch stability of the dual-side-chain modified silicone oils, after the preparation of A1 to A5, it is preferable to test the residual Si-H content, the total residual 1-octene and 1-decene content, and the moisture content, respectively. Preferably, the residual Si-H content of A1 to A5 is no higher than 10 ppm, the total residual 1-octene and 1-decene content is no higher than 0.5 wt%, and the moisture content is no higher than 100 ppm. This invention employs dry nitrogen protection and vacuum dehydration and low-boiling point removal operations to reduce the impact of moisture, residual low-boiling hydrocarbons, and residual Si-H on dielectric properties, volatility, and long-term stability.

[0037] For ease of explanation, taking a polymethylhydrosiloxane with a Si-H molar amount of 1.00 mol and a total molar ratio of carbon-carbon double bonds to Si-H molar amount of 1.10:1 in 1-octene and 1-decene as an example, dual-side-chain modified silicone oils with different side-chain ratios can be prepared as follows: A1: The molar ratio of 1-octene to 1-decene is 30:70, that is, 0.33 mol of 1-octene and 0.77 mol of 1-decene are added; A2: The molar ratio of 1-octene to 1-decene is 40:60, that is, 0.44 mol of 1-octene and 0.66 mol of 1-decene are added; A3: The molar ratio of 1-octene to 1-decene is 50:50, that is, 0.55 mol of 1-octene and 0.55 mol of 1-decene are added; A4: The molar ratio of 1-octene to 1-decene is 60:40, which means adding 0.66 mol of 1-octene and 0.44 mol of 1-decene; A5: The molar ratio of 1-octene to 1-decene is 70:30, which means adding 0.77 mol of 1-octene and 0.33 mol of 1-decene.

[0038] Table A: Quality Control Results of Dual-Side-Chain Modified Silicone Oil ; In the preparation processes of A1~A5 described above, the amount of Karstedt catalyst can be controlled at 10 ppm (based on platinum), the reaction temperature can be controlled at 85℃, and the reaction time can be controlled at 4 h. After the reaction, activated carbon is added for treatment, and after filtration, low-boiling substances are removed at 135℃ and a gauge pressure of -0.096 MPa for 3 h. In actual preparation, the amount of 1-octene and 1-decene added can be calculated proportionally based on the Si-H hydrogen mass fraction of polymethylhydrosiloxane.

[0039] During specific feeding, the molar amount of Si-H in polymethylhydrosiloxane can be calculated based on its Si-H hydrogen mass fraction, using the formula: Molar amount of Si-H = Mass of polymethylhydrosiloxane × Mass fraction of Si-H hydrogen / 1.008. The Si-H hydrogen mass fraction is calculated as a decimal; when the feeding mass is in grams, the calculated molar amount of Si-H is in mol. Based on the calculated molar amount of Si-H, the total molar amounts of 1-octene and 1-decene are determined according to a ratio of total molar amount of carbon-carbon double bonds to molar amount of Si-H of 1.08–1.15:1, and the amounts of 1-octene and 1-decene are allocated according to the set feeding molar ratio.

[0040] During the hydrosilylation reaction, 1-octene and 1-decene can be added after pre-mixing or in batches within the same reaction system; however, the octyl-modified intermediate or the decyl-modified intermediate is not separated before the reaction is completed and the low-boiling point is removed. The resulting dual-side-chain modified silicone oil is a co-modified product formed in the same reaction system, rather than a simple physical mixture of separately prepared octyl-modified and decyl-modified silicone oils.

[0041] like Figure 1 As shown, the composition of the present invention is preferably prepared in the following order: preparation of double-side-chain modified silicone oil, dehydration of base oil, preparation of mother liquor, blending of base oil, addition of additives, vacuum degassing, and filtration.

[0042] Example 1: This example discloses a method for preparing a low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling, comprising the following steps: Based on 100 parts by weight of the finished oil, the following components are included: 55.00 parts by weight of A1, 28.00 parts by weight of PAO-6, 15.50 parts by weight of trimethylolpropane tri(ethylhexanoate), 0.55 parts by weight of 4,4'-dioctyl diphenylamine, 0.40 parts by weight of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate isooctyl ester, 0.12 parts by weight of N,N-di(2-ethylhexyl)-1H-methylbenzotriazole-1-methylamine, 0.35 parts by weight of polymethacrylate, and 0.08 parts by weight of polyether-modified polydimethylsiloxane.

[0043] Step (1) 100.00 parts by mass of polymethylhydrosiloxane, having a Si-H hydrogen mass fraction of 0.50 wt%, is added to a reactor purged with dry nitrogen. Based on this Si-H hydrogen mass fraction, the molar amount of Si-H in 100.00 parts by mass of polymethylhydrosiloxane is approximately 0.496 mol. 18.37 parts by mass of 1-octene and 53.56 parts by mass of 1-decene are added to the reactor, such that the ratio of the total molar amount of carbon-carbon double bonds in 1-octene and 1-decene to the molar amount of Si-H in polymethylhydrosiloxane is 1.10:1, and the molar ratio of 1-octene to 1-decene is 30:70. Subsequently, a Karstedt catalyst is added, which is a Karstedt catalyst solution with a platinum content of 2.0 wt%, in an amount of 0.086 parts by mass, so that the catalyst dosage, calculated as platinum, is approximately 10 ppm. The temperature was raised to 85℃, and the hydrosilylation reaction was carried out for 4 hours under dry nitrogen protection. The system temperature was kept stable during the reaction to avoid excessively rapid local temperature rise.

[0044] After the reaction was complete, 1.72 parts by mass of activated carbon were added, and the mixture was stirred at 80°C for 1 hour. The activated carbon and insoluble matter were removed by filtration. The filtrate was subjected to a 3-hour cooling process at 135°C and a gauge pressure of -0.096 MPa to remove low-boiling substances, yielding a double-side-chain modified silicone oil A1. The obtained A1 is a co-modified silicone oil in which octyl and decyl side chains were introduced in the same reaction system.

[0045] Step (2) A1, PAO-6 and trimethylolpropane tri(ethylhexanoic acid) ester were vacuum dehydrated for 2 h at 70 °C and gauge pressure of -0.095 MPa.

[0046] Reserve 3.00 parts by weight of PAO-6 from 28.00 parts by weight of PAO-6, add 0.55 parts by weight of 4,4'-dioctyl diphenylamine and 0.40 parts by weight of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate isooctyl ester at 50°C, and stir for 30 min to obtain antioxidant mother liquor.

[0047] Reserve 1.00 parts by weight of trimethylolpropane tri(ethylhexanoate) ester from 15.50 parts by weight of trimethylolpropane tri(ethylhexanoate) ester. Add 0.12 parts by weight of N,N-di(2-ethylhexyl)-1H-methylbenzotriazole-1-methylamine at 50°C and stir for 20 min to obtain the passivation mother liquor.

[0048] Of these, the reserved 3.00 parts by weight of PAO-6 are included in the total amount of 28.00 parts by weight of PAO-6, and the reserved 1.00 parts by weight of trimethylolpropane tri(ethylhexanoic acid) ester are included in the total amount of 15.50 parts by weight of trimethylolpropane tri(ethylhexanoic acid) ester.

[0049] Step (3) Add 55.00 parts by weight of A1, the remaining 25.00 parts by weight of PAO-6 and the remaining 14.50 parts by weight of trimethylolpropane tri(ethylhexanoate) ester to a mixing vessel and stir at 50°C for 60 min to obtain a base oil mixture. Add the antioxidant mother liquor and passivation mother liquor prepared in step (2) to the base oil mixture and continue stirring at 50°C for 90 min to ensure uniform dispersion of the antioxidant and metal passivator.

[0050] Step (4) Add 0.35 parts by weight of polymethacrylate to the mixture obtained in step (3) and stir for 45 min; after cooling to 40°C, add 0.08 parts by weight of polyether-modified polydimethylsiloxane and continue stirring for 30 min. Then degas under vacuum for 60 min at 60°C and gauge pressure of -0.095 MPa, and filter through 5 μm and 1 μm filter elements in sequence to obtain a low viscosity, high flash point dielectric cooling oil composition for liquid cooling.

[0051] Example 2: This example discloses a method for preparing a low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling.

[0052] Based on 100 parts by weight of the finished oil, the following components are included: 58.00 parts by weight of A2, 25.00 parts by weight of PAO-6, 15.72 parts by weight of trimethylolpropane tri(ethylhexanoate), 0.46 parts by weight of 4,4'-dioctyl diphenylamine, 0.32 parts by weight of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate isooctyl ester, 0.10 parts by weight of N,N-di(2-ethylhexyl)-1H-methylbenzotriazole-1-methylamine, 0.32 parts by weight of polymethyl methacrylate, and 0.08 parts by weight of polyether-modified polydimethylsiloxane.

[0053] A2 was prepared using the same method as A1 in Example 1, except that: based on 100.00 parts by mass of polymethylhydrosiloxane, 24.49 parts by mass of 1-octene and 45.91 parts by mass of 1-decene were added, so that the ratio of the total molar amount of carbon-carbon double bonds in 1-octene and 1-decene to the molar amount of Si-H was 1.10:1, and the molar ratio of 1-octene to 1-decene was 40:60; the remaining catalyst dosage, reaction temperature, reaction time, activated carbon treatment, filtration, and de-boiling conditions were the same as in Example 1. The resulting A2 is a co-modified silicone oil in which octyl and decyl side chains are introduced in the same reaction system.

[0054] A2, PAO-6, and trimethylolpropane tri(ethylhexanoate) ester were vacuum dehydrated for 2 h at 70 °C and a gauge pressure of -0.095 MPa. 2.50 parts by weight of PAO-6 were reserved from 25.00 parts by weight of PAO-6 to dissolve 0.46 parts by weight of 4,4'-dioctyl diphenylamine and 0.32 parts by weight of isooctyl β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate to prepare an antioxidant mother liquor. 1.00 parts by weight of trimethylolpropane tri(ethylhexanoate) ester were reserved from 15.72 parts by weight of trimethylolpropane tri(ethylhexanoate) ester to dissolve 0.10 parts by weight of N,N-di(2-ethylhexyl)-1H-methylbenzotriazole-1-methylamine to prepare a passivation mother liquor. All reserved components were included in the total amount of the corresponding components used.

[0055] 58.00 parts by weight of A2, the remaining 22.50 parts by weight of PAO-6, and the remaining 14.72 parts by weight of trimethylolpropane tri(ethylhexanoate) ester were added to a mixing vessel and stirred at 50°C for 60 min. Antioxidant mother liquor and passivation mother liquor were added and stirring was continued for 90 min. Then, 0.32 parts by weight of polymethacrylate were added and stirred for 45 min. After cooling to 40°C, 0.08 parts by weight of polyether-modified polydimethylsiloxane were added and stirred for 30 min. Subsequently, vacuum degassing was carried out at 60°C and a gauge pressure of -0.095 MPa for 60 min. The mixture was then filtered through 5 μm and 1 μm filter elements to obtain a low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling.

[0056] Example 3: This example discloses a method for preparing a low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling.

[0057] Based on 100 parts by weight of the finished oil, take 60.00 parts by weight of A3, 23.50 parts by weight of PAO-6, 15.40 parts by weight of trimethylolpropane tri(ethylhexanoate), 0.42 parts by weight of 4,4'-dioctyl diphenylamine, 0.28 parts by weight of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate isooctyl ester, 0.08 parts by weight of N,N-di(2-ethylhexyl)-1H-methylbenzotriazole-1-methylamine, 0.28 parts by weight of polymethacrylate and 0.04 parts by weight of polyether-modified polydimethylsiloxane.

[0058] A3 was prepared using the same method as A1 in Example 1, except that: based on 100.00 parts by mass of polymethylhydrosiloxane, 30.62 parts by mass of 1-octene and 38.27 parts by mass of 1-decene were added, so that the total molar amount of carbon-carbon double bonds in 1-octene and 1-decene was 1.10:1, and the molar ratio of 1-octene to 1-decene was 50:50; the remaining catalyst dosage, reaction temperature, reaction time, activated carbon treatment, filtration, and de-boiling conditions were the same as in Example 1. The resulting A3 is a co-modified silicone oil in which octyl and decyl side chains are introduced in the same reaction system.

[0059] A3, PAO-6, and trimethylolpropane tri(ethylhexanoate) ester were vacuum dehydrated for 2 hours at 70°C and a gauge pressure of -0.095 MPa. 2.50 parts by weight of PAO-6 were reserved from 23.50 parts by weight of PAO-6 for preparing the antioxidant mother liquor; 1.00 part by weight of trimethylolpropane tri(ethylhexanoate) ester was reserved from 15.40 parts by weight of trimethylolpropane tri(ethylhexanoate) ester for preparing the passivation mother liquor. The preparation methods of the antioxidant and passivation mother liquors were the same as in Example 1, except that the amounts of antioxidant and metal passivating agent added were the same as those in the corresponding formulation of this example.

[0060] 60.00 parts by weight of A3, the remaining 21.00 parts by weight of PAO-6, and the remaining 14.40 parts by weight of trimethylolpropane tri(ethylhexanoate) ester were added to a mixing vessel and stirred at 50°C for 60 min. Antioxidant mother liquor and passivation mother liquor were added and stirring was continued for 90 min. Then, 0.28 parts by weight of polymethacrylate were added and stirred for 45 min. After cooling to 40°C, 0.04 parts by weight of polyether-modified polydimethylsiloxane were added and stirred for 30 min. Subsequently, vacuum degassing was carried out at 60°C and a gauge pressure of -0.095 MPa for 60 min. The mixture was then filtered through 5 μm and 1 μm filter elements to obtain a low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling.

[0061] Example 4: This example discloses a method for preparing a low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling.

[0062] Based on 100 parts by weight of the finished oil, the following components are included: 62.00 parts by weight of A4, 22.00 parts by weight of PAO-6, 14.80 parts by weight of pentaerythritol tetra(2-ethylhexanoic acid) ester, 0.46 parts by weight of 4,4'-dioctyl diphenylamine, 0.32 parts by weight of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate isooctyl ester, 0.10 parts by weight of N,N-di(2-ethylhexyl)-1H-methylbenzotriazole-1-methylamine, 0.26 parts by weight of polymethacrylate, and 0.06 parts by weight of polyether-modified polydimethylsiloxane.

[0063] A4 was prepared using the same method as A1 in Example 1, except that: based on 100.00 parts by mass of polymethylhydrosiloxane, 36.74 parts by mass of 1-octene and 30.62 parts by mass of 1-decene were added, so that the ratio of the total molar amount of carbon-carbon double bonds in 1-octene and 1-decene to the molar amount of Si-H was 1.10:1, and the molar ratio of 1-octene to 1-decene was 60:40; the remaining catalyst dosage, reaction temperature, reaction time, activated carbon treatment, filtration, and de-boiling conditions were the same as in Example 1. The resulting A4 is a co-modified silicone oil in which octyl and decyl side chains are introduced in the same reaction system.

[0064] A4, PAO-6, and pentaerythritol tetra(2-ethylhexanoate) ester were vacuum dehydrated for 2 hours at 70°C and a gauge pressure of -0.095 MPa. 2.50 parts by weight of PAO-6 were reserved from 22.00 parts by weight of PAO-6 for preparing the antioxidant mother liquor; 1.00 part by weight of pentaerythritol tetra(2-ethylhexanoate) ester was reserved from 14.80 parts by weight of pentaerythritol tetra(2-ethylhexanoate) ester for preparing the passivation mother liquor. The preparation methods of the antioxidant and passivation mother liquors were the same as in Example 1, except that the amounts of antioxidant and metal passivating agent added were the same as those in the corresponding formulation of this example.

[0065] 62.00 parts by weight of A4, the remaining 19.50 parts by weight of PAO-6, and the remaining 13.80 parts by weight of pentaerythritol tetra(2-ethylhexanoic acid) ester were added to a mixing vessel and stirred at 50°C for 60 min. Antioxidant mother liquor and passivation mother liquor were added and stirring was continued for 90 min. Then, 0.26 parts by weight of polymethacrylate were added and stirred for 45 min. After cooling to 40°C, 0.06 parts by weight of polyether-modified polydimethylsiloxane were added and stirred for 30 min. Subsequently, vacuum degassing was carried out at 60°C and a gauge pressure of -0.095 MPa for 60 min. The mixture was then filtered through 5 μm and 1 μm filter elements to obtain a low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling.

[0066] Example 5: This example discloses a method for preparing a low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling.

[0067] Based on 100 parts by weight of the finished oil, the following components are included: 66.00 parts by weight of A5, 18.00 parts by weight of PAO-6, 14.50 parts by weight of neopentyl glycol di(ethylhexanoate), 0.55 parts by weight of 4,4'-dioctyl diphenylamine, 0.40 parts by weight of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate isooctyl ester, 0.12 parts by weight of N,N-di(2-ethylhexyl)-1H-methylbenzotriazole-1-methylamine, 0.35 parts by weight of polymethacrylate, and 0.08 parts by weight of polyether-modified polydimethylsiloxane.

[0068] A5 was prepared using the same method as A1 in Example 1, except that: based on 100.00 parts by mass of polymethylhydrosiloxane, 42.87 parts by mass of 1-octene and 22.96 parts by mass of 1-decene were added, making the ratio of the total molar amount of carbon-carbon double bonds in 1-octene and 1-decene to the molar amount of Si-H 1.10:1, and the molar ratio of 1-octene to 1-decene was 70:30; the remaining catalyst dosage, reaction temperature, reaction time, activated carbon treatment, filtration, and de-boiling conditions were the same as in Example 1. The resulting A5 is a co-modified silicone oil in which octyl and decyl side chains are introduced in the same reaction system.

[0069] A5, PAO-6, and neopentyl glycol di(ethylhexanoate) ester were vacuum dehydrated for 2 hours at 70°C and a gauge pressure of -0.095 MPa. 3.00 parts by weight of PAO-6 were reserved from 18.00 parts by weight of PAO-6 for preparing the antioxidant mother liquor; 1.00 parts by weight of neopentyl glycol di(ethylhexanoate) ester was reserved from 14.50 parts by weight of neopentyl glycol di(ethylhexanoate) ester for preparing the passivation mother liquor. The preparation methods of the antioxidant and passivation mother liquors were the same as in Example 1, except that the amounts of antioxidant and metal passivating agent added were the same as those in the corresponding formulation of this example.

[0070] 66.00 parts by weight of A5, the remaining 15.00 parts by weight of PAO-6 and the remaining 13.50 parts by weight of neopentyl glycol di(ethylhexanoate) ester were added to a mixing vessel and stirred at 50°C for 60 min. Antioxidant mother liquor and passivation mother liquor were added and stirring was continued for 90 min. Then 0.35 parts by weight of polymethacrylate were added and stirred for 45 min. After cooling to 40°C, 0.08 parts by weight of polyether-modified polydimethylsiloxane were added and stirred for 30 min. Subsequently, vacuum degassing was carried out at 60°C and gauge pressure of -0.095 MPa for 60 min. The mixture was then filtered through 5 μm and 1 μm filter elements to obtain a low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling.

[0071] Comparative Example 1 Comparative Example 1 is based on Example 3, except that 60.00 parts by weight of A3 is replaced with a physical mixture of 30.00 parts by weight of octyl modified silicone oil B1 and 30.00 parts by weight of decyl modified silicone oil B2. Other components and their amounts, mother liquor preparation methods, blending methods, vacuum degassing and filtration conditions are the same as in Example 3.

[0072] Octyl-modified silicone oil B1 was prepared according to the preparation method of A1 in Example 1, except that: based on 100.00 parts by mass of polymethylhydrosiloxane, only 61.23 parts by mass of 1-octene were added, so that the molar ratio of carbon-carbon double bond to Si-H molar amount in 1-octene was 1.10:1; 1-decene was not added.

[0073] Decyl modified silicone oil B2 was prepared according to the preparation method of A1 in Example 1, except that: based on 100.00 parts by mass of polymethylhydrosiloxane, only 76.53 parts by mass of 1-decene were added, so that the molar ratio of carbon-carbon double bond to Si-H molar amount in 1-decene was 1.10:1; 1-octene was not added.

[0074] The overall molar ratio of C8 / C10, the amount of base oil and additives were the same in Comparative Example 1 and Example 3. The difference was that Example 3 used double-side-chain modified silicone oil A3 prepared in the same reaction system, while Comparative Example 1 used a physical mixture of octyl modified silicone oil B1 and decyl modified silicone oil B2.

[0075] Comparative Example 2 Comparative Example 2 is based on Example 3, except that 60.00 parts by weight of A3 is replaced with 60.00 parts by weight of octyl modified silicone oil B1, and the other components and their amounts, mother liquor preparation method, blending method, vacuum degassing and filtration conditions are the same as in Example 3.

[0076] The preparation method of octyl-modified silicone oil B1 is the same as that of Comparative Example 1.

[0077] The difference between Comparative Example 2 and Example 3 is that Comparative Example 2 uses a single octyl modified silicone oil B1 instead of the double-side-chain modified silicone oil A3 prepared in the same reaction system.

[0078] Comparative Example 3 Comparative Example 3 is based on Example 3, except that 60.00 parts by weight of A3 is replaced with 60.00 parts by weight of decyl modified silicone oil B2. Other components and their amounts, mother liquor preparation methods, blending methods, vacuum degassing and filtration conditions are the same as in Example 3.

[0079] The preparation method of decyl modified silicone oil B2 is the same as that of Comparative Example 1.

[0080] The difference between Comparative Example 3 and Example 3 is that Comparative Example 3 uses a single decyl modified silicone oil B2 instead of the double-side-chain modified silicone oil A3 prepared in the same reaction system.

[0081] Comparative Example 4 Comparative Example 4 is based on Example 3, except that 23.50 parts by mass of PAO-6 is replaced with 23.50 parts by mass of A3, that is, the total amount of A3 is adjusted to 83.50 parts by mass. Other components and their amounts, mother liquor preparation methods, blending methods, vacuum degassing and filtration conditions are the same as in Example 3.

[0082] Specifically, based on 100 parts by weight of the finished oil, the following components are included: 83.50 parts by weight of A3, 15.40 parts by weight of trimethylolpropane tri(ethylhexanoate), 0.42 parts by weight of 4,4'-dioctyl diphenylamine, 0.28 parts by weight of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate isooctyl ester, 0.08 parts by weight of N,N-di(2-ethylhexyl)-1H-methylbenzotriazole-1-methylamine, 0.28 parts by weight of polymethyl methacrylate, and 0.04 parts by weight of polyether-modified polydimethylsiloxane.

[0083] In Comparative Example 4, since PAO-6 was not present, the antioxidant mother liquor was prepared using A3 reserved from 83.50 parts by mass of A3 as a solvent, and the passivation mother liquor was prepared using ester reserved from 15.40 parts by mass of trimethylolpropane tri(ethylhexanoic acid) ester as a solvent. All reserved components were included in the total amount of the corresponding components.

[0084] The difference between Comparative Example 4 and Example 3 is that Comparative Example 4 does not contain PAO-6, and the amount of PAO-6 applied is replaced by A3.

[0085] Comparative Example 5 Comparative Example 5 was based on Example 3, except that 15.40 parts by weight of trimethylolpropane tri(ethylhexanoate) ester was replaced with 15.40 parts by weight of PAO-6, that is, the total amount of PAO-6 was adjusted to 38.90 parts by weight. Other components and their amounts, mixing methods, vacuum degassing and filtration conditions were the same as in Example 3.

[0086] Specifically, based on 100 parts by weight of the finished oil, the following components are included: 60.00 parts by weight of A3, 38.90 parts by weight of PAO-6, 0.42 parts by weight of 4,4'-dioctyl diphenylamine, 0.28 parts by weight of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate isooctyl ester, 0.08 parts by weight of N,N-di(2-ethylhexyl)-1H-methylbenzotriazole-1-methylamine, 0.28 parts by weight of polymethyl methacrylate, and 0.04 parts by weight of polyether-modified polydimethylsiloxane.

[0087] In Comparative Example 5, both the antioxidant mother liquor and the passivation mother liquor were prepared using reserved PAO-6 as a solvent, wherein N,N-di(2-ethylhexyl)-1H-methylbenzotriazole-1-methylamine was dissolved in reserved PAO-6.

[0088] The difference between Comparative Example 5 and Example 3 is that Comparative Example 5 does not contain branched saturated polyol esters, and the application amount of branched saturated polyol esters is replaced by PAO-6.

[0089] Performance testing methods The samples obtained in each embodiment and comparative example were subjected to performance tests according to the following methods: kinematic viscosity was tested according to GB / T 265; flash point was tested according to the open cup method of GB / T 3536; pour point was tested according to GB / T 3535; moisture content was tested using a coulometric Karl Fischer moisture analyzer; breakdown voltage was tested according to GB / T 507; dielectric constant and dielectric loss factor were tested according to GB / T 5654; ​​copper strip corrosion was tested according to GB / T 5096; and foaming property was tested according to GB / T 12579. Evaporation loss was evaluated using mass loss at 150℃ for 24 hours. Thermo-oxidative aging was performed using air aging conditions at 120℃ for 168 hours. Thermal cycling consisted of 10 cycles of holding at -40℃ for 4 hours followed by raising to 80℃ and holding for 4 hours. Thermal storage stability was evaluated using a static condition at 80℃ for 7 days. Material compatibility was assessed by immersing EPDM, silicone rubber, aluminum sheet, and tin solder at 120°C for 168 hours and observing changes in quality, dimensions, and appearance.

[0090] Table 1 Basic physical properties ; As shown in Table 1, Examples 1-5 maintained a high flash point even with low kinematic viscosity at 40°C, and remained clear and flowable after standing at -50°C for 24 hours. This indicates that the compositions of the present invention can balance low viscosity, high flash point, low volatility, and low-temperature transparency. Compared with Example 3, Comparative Example 1 showed slight opalescence and increased evaporation loss; Comparative Example 2 had a lower flash point and higher evaporation loss; Comparative Examples 3 and 4 showed increased viscosity and worsened low-temperature appearance; and Comparative Example 5 showed increased evaporation loss. This indicates a synergistic relationship between the dual-side-chain modified silicone oil, PAO-6, and the branched saturated polyol ester.

[0091] Table 2 Dielectric properties and initial stability ; Table 2 shows that Examples 1-5 exhibit higher breakdown voltage, higher volume resistivity, and lower dielectric loss under low moisture conditions. Compared to Example 3, Comparative Example 5, without branched saturated polyol esters and with PAO-6 as the main pre-dispersion medium for passivation, showed worse dielectric loss, breakdown voltage, and copper strip corrosion results. This indicates that the ternary base oil system involving branched saturated polyol esters is beneficial for improving the dispersion stability of trace additives and the metal protection effect.

[0092] Table 3 Aging stability and thermal cycling ; As shown in Table 3, Examples 1-5 maintained good appearance and dielectric stability after thermal aging, thermal storage, and thermal cycling. Compared with Comparative Example 1, Example 3, under the same C8 / C10 ratio and the same amount of base oil and additives, used a double-side-chain modified silicone oil formed in the same reaction system, which is beneficial to improving the appearance after thermal cycling and the dielectric loss after aging.

[0093] Table 4 Material Compatibility ; As shown in Table 4, Examples 1-5 all exhibited good material compatibility with EPDM, silicone rubber, aluminum sheet, and solder. Compared with Example 3, the rubber mass change rate and dimensional change rate of Comparative Examples 1, 2, and 5 increased. In Comparative Example 5, slight dark spots appeared on the aluminum sheet and solder, indicating that the formulation system of the present invention is beneficial to improving the long-term contact stability of sealing materials and metal materials.

[0094] like Figures 2-6 As shown, Example 3, compared with Comparative Examples 1 to 5, exhibits a better overall balance in terms of kinematic viscosity at 40°C, flash point, evaporation loss, dielectric loss factor, and the rate of change in the mass of the rubber material.

[0095] As demonstrated in Examples 1-5 and Comparative Examples 1-5, the present invention utilizes a double-side-chain modified silicone oil prepared within the same reaction system, and blends it with PAO-6, branched saturated polyol ester, antioxidant mother liquor, passivation mother liquor, polymethyl methacrylate, and polyether-modified polydimethylsiloxane. This achieves a good overall balance between low viscosity, high flash point, low volatility, dielectric stability, low-temperature transparency, and material compatibility. Comparative results show that physical mixtures of octyl-modified and decyl-modified silicone oils, single octyl-modified silicone oil, single decyl-modified silicone oil, and systems lacking PAO-6 or branched saturated polyol esters all struggle to simultaneously achieve the aforementioned comprehensive properties. Therefore, the ternary base oil system and mother liquor addition method of the present invention are not arbitrarily blended, but rather a specific combination formed around the comprehensive performance requirements of immersion liquid-cooled dielectric cooling oil.

[0096] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. All equivalent substitutions, modifications, or improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing a low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling, characterized in that, Includes the following steps: Step (1) Under dry nitrogen protection, polymethylhydrosiloxane, 1-octene and 1-decene are subjected to hydrosilylation reaction in the same reaction system. After treatment with activated carbon, filtration and de-boiling point removal, double-side chain modified silicone oil is obtained. Step (2) Vacuum dehydrate the double-side-chain modified silicone oil, PAO-6, and branched saturated polyol ester respectively; Step (3) Reserve a portion of PAO-6 from the total amount of PAO-6 to prepare antioxidant mother liquor, and reserve a portion of branched saturated polyol ester from the total amount of branched saturated polyol ester to prepare passivation mother liquor; after mixing the double-side-chain modified silicone oil, PAO-6 and branched saturated polyol ester, add the antioxidant mother liquor and passivation mother liquor. Step (4) Add polymethyl methacrylate and polyether-modified polydimethylsiloxane, and then degas and filter under vacuum to obtain the liquid cooling low viscosity high flash point dielectric cooling oil composition.

2. The method for preparing the low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling according to claim 1, characterized in that, In step (1), the ratio of the total molar amount of carbon-carbon double bonds in 1-octene and 1-decene to the molar amount of Si-H in polymethylhydrosiloxane is 1.08~1.15:

1. The hydrosilylation reaction uses Karstedt catalyst, and the amount of catalyst is 5~20 ppm based on platinum. The amount of catalyst is calculated based on the total mass of polymethylhydrosiloxane, 1-octene and 1-decene. The reaction temperature is 75~95℃ and the reaction time is 3~6h. The conditions for removing low-boiling points are: temperature 120~150℃, gauge pressure -0.098MPa~-0.095MPa, and time 2~5h.

3. The method for preparing the low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling according to claim 1, characterized in that, In step (1), the molar ratio of 1-octene to 1-decene is 30:70 to 70:30; after the preparation of the double-side chain modified silicone oil, the residual Si-H content is not higher than 10 ppm, the total content of residual 1-octene and 1-decene is not higher than 0.5 wt%, and the moisture content is not higher than 100 ppm.

4. The method for preparing the low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling according to claim 1, characterized in that, The preparation method of the antioxidant mother liquor and the passivation mother liquor includes the following steps: Based on 100 parts by weight of the finished oil, 0.30~0.55 parts by weight of 4,4'-dioctyl diphenylamine and 0.18~0.40 parts by weight of isooctyl ester of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate are dissolved in the reserved PAO-6 to obtain an antioxidant mother liquor; Based on 100 parts by weight of the finished oil, 0.05 to 0.12 parts by weight of N,N-di(2-ethylhexyl)-1H-methylbenzotriazole-1-methylamine are dissolved in the reserved branched saturated polyol ester to obtain the passivation mother liquor. The reserved PAO-6 is included in the total amount of PAO-6 used, and the reserved branched saturated polyol ester is included in the total amount of branched saturated polyol ester used.

5. The method for preparing the low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling according to claim 4, characterized in that, Based on a total of 100 parts by weight of the finished oil, the following components are used: 55-66 parts by weight of the double-side-chain modified silicone oil, 18-28 parts by weight of PAO-6, 8-16 parts by weight of the branched saturated polyol ester, 0.30-0.55 parts by weight of 4,4'-dioctyl diphenylamine, 0.18-0.40 parts by weight of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate isooctyl ester, 0.05-0.12 parts by weight of N,N-di(2-ethylhexyl)-1H-methylbenzotriazole-1-methylamine, 0.10-0.35 parts by weight of polymethacrylate, and 0.01-0.08 parts by weight of polyether-modified polydimethylsiloxane. The amounts of each component are selected within the above ranges, and the total amount of the finished oil is 100 parts by weight.

6. The method for preparing the low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling according to claim 1, characterized in that, In step (2), the vacuum dehydration conditions are: temperature of 60~80℃, gauge pressure of -0.095MPa~-0.08MPa, and time of 1~3h.

7. The method for preparing the low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling according to claim 1, characterized in that, The branched saturated polyol ester is selected from one or more of trimethylolpropane tri(ethylhexanoate), pentaerythritol tetra(2-ethylhexanoate), and neopentyl glycol di(ethylhexanoate).

8. The method for preparing the low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling according to claim 1, characterized in that, In step (4), the polymethacrylate is a methacrylate copolymer containing C8~C18 alkyl ester side groups, with a weight-average molecular weight of 30,000~200,000; the polyether-modified polydimethylsiloxane is a polydimethylsiloxane with methyl-terminated polyether side-linked branches, with an effective content of not less than 90 wt%.

9. A low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling, characterized in that, Based on 100 parts by weight of the total composition, it comprises 55-66 parts by weight of bi-side-chain modified silicone oil, 18-28 parts by weight of PAO-6, 8-16 parts by weight of branched saturated polyol ester, 0.30-0.55 parts by weight of 4,4'-dioctyl diphenylamine, 0.18-0.40 parts by weight of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate isooctyl ester, 0.05-0.12 parts by weight of N,N-di(2-ethylhexyl)-1H-methylbenzotriazole-1-methylamine, 0.10-0.35 parts by weight of polymethacrylate, and 0.01-0.08 parts by weight of polyether-modified polydimethylsiloxane; wherein, the bi-side-chain... The modified silicone oil is prepared by hydrosilylation reaction of polymethylhydrosiloxane, 1-octene, and 1-decene in the same reaction system. The molar ratio of 1-octene to 1-decene is 30:70 to 70:

30. Before being mixed with other components, the residual Si-H content of the dual-side-chain modified silicone oil is not higher than 10 ppm, the total residual content of 1-octene and 1-decene is not higher than 0.5 wt%, and the moisture content is not higher than 100 ppm. Based on the feeding ratio and reaction conversion results, the dual-side-chain modified silicone oil contains an average of methyloctylsiloxane units and methyldecylsiloxane units. The amount of each component is selected within the above range, and the total amount of the composition is 100 parts by mass.

10. The low-viscosity, high-flash-point dielectric cooling oil composition for liquid cooling according to claim 9, characterized in that, Based on 100 parts by weight of the total composition, the double-side-chain modified silicone oil comprises 58-62 parts by weight, PAO-6 comprises 22-25 parts by weight, branched saturated polyol ester comprises 14-16 parts by weight, 4,4'-dioctyl diphenylamine comprises 0.38-0.46 parts by weight, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate isooctyl ester comprises 0.24-0.32 parts by weight, N,N-di(2-ethylhexyl)-1H-methylbenzotriazole-1-methylamine comprises 0.06-0.10 parts by weight, polymethacrylate comprises 0.20-0.32 parts by weight, and polyether-modified polydimethylsiloxane comprises 0.02-0.06 parts by weight.