A method for reconstructing zero-dimensional indium halide crystal structures based on the same precursor system and the scintillator prepared therefrom.

By controlling the crystal growth environment and using a combination of cooling crystallization and seeding methods, the controllable reconstruction of zero-dimensional indium halide crystal structures and the preparation of high-quality large-size crystals were achieved. This solved the problems of difficult crystal structure reconstruction and large-size single crystal preparation in existing technologies, and yielded crystal materials with excellent luminescence and X-ray scintillation properties, which are suitable for high-energy ray detection and imaging.

CN123107675APending Publication Date: 2026-11-17TECHNICAL INST OF PHYSICS & CHEMISTRY - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611021598.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies make it difficult to achieve controllable reconstruction of zero-dimensional indium halide crystal structures and the preparation of high-quality, large-size single crystals in the same precursor system, which makes it difficult to meet the application requirements of high-performance X-ray detection and intelligent imaging.

Method used

By controlling the crystal growth environment, including the volume ratio of acid to organic solvent, ambient humidity, and temperature, inorganic coordination units are induced to recombine. Zero-dimensional indium halide crystals with different crystal structures are prepared by combining cooling crystallization with seed crystal method.

Benefits of technology

Controllable reconstruction of crystal structure was achieved under the same precursor system, resulting in high-quality, large-size zero-dimensional indium halide crystals with excellent luminescence and X-ray scintillation properties, suitable for high-energy ray detection and imaging, environmental response detection, and intelligent imaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107675A_ABST
    Figure CN123107675A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of organic-inorganic hybrid metal halide scintillators, and relates to a method for reconstructing the zero-dimensional indium halide crystal structure based on the same precursor system and the scintillator prepared therefrom. The method for reconstructing the zero-dimensional indium halide crystal structure of this invention uses organic molecular precursors, indium halide precursors, and optionally added or unadded doped metal halide precursors as raw materials. By controlling the crystallization environment to induce recombination of inorganic coordination units, the zero-dimensional indium halide crystal structure is controllably reconstructed within the same precursor system, thereby obtaining crystal materials with different luminescence and scintillation properties. The prepared zero-dimensional indium halide scintillator exhibits excellent luminescence performance, X-ray scintillation performance, high spatial resolution imaging capability, and environmental response characteristics, and can be applied in fields such as high-energy ray detection and imaging, environmental response detection, and intelligent imaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of organic-inorganic hybrid metal halide scintillator technology, and relates to crystal structure control and single crystal growth technology. More specifically, it relates to a method for reconstructing a zero-dimensional indium-based halide crystal structure based on the same precursor system and the scintillator prepared therefrom. Background Technology

[0002] Multifunctional and intelligent X-ray imaging technology is becoming an important development direction in fields such as medical diagnosis, security inspection, industrial non-destructive testing, and radiation detection. Currently, indirect X-ray imaging technology based on scintillators is one of the most widely used X-ray imaging techniques due to its advantages such as high detection sensitivity, large imaging area, low cost, and ease of integration. Therefore, developing novel scintillator materials with excellent luminescence and radiation response properties is of great significance.

[0003] In recent years, organic-inorganic hybrid metal halides (OIMHs) have attracted widespread attention due to their combination of the structural tunability of the organic component and the excellent photoelectric properties of the inorganic component. In particular, zero-dimensional OIMHs, with their discrete inorganic coordination units, are conducive to the formation of self-trapped excitons, enabling efficient broadband luminescence, and are therefore considered important candidate materials for next-generation X-ray scintillators.

[0004] In existing technologies, the optimization of the luminescence and scintillation properties of OIMHs mainly relies on compositional modulation strategies, such as changing organic cations, adjusting the composition of metal ions, and halogen substitution, to achieve regulation of coordination structure, band gap, and luminescence properties. Although the above methods improve material properties to some extent, changes in chemical composition are often accompanied by simultaneous changes in crystal structure, local coordination environment, and electronic structure. This leads to the coupling of multiple influencing factors, making it difficult to accurately reveal the intrinsic correlation mechanism between crystal structure and luminescence properties, thus limiting the rational design of materials based on structure-property relationships.

[0005] Furthermore, existing technologies for controlling crystal structure reconstruction while maintaining the precursor system largely unchanged are still relatively lacking. In particular, there are even fewer studies on inducing recombination of inorganic coordination units by controlling the crystal growth environment within the same precursor system to obtain different crystal structures and establish clear structure-luminescence relationships. Meanwhile, the preparation of high-quality, large-size single crystals remains challenging, hindering material structure analysis and its application in high-resolution X-ray imaging.

[0006] Therefore, there is an urgent need to develop a method for reconstructing zero-dimensional indium halide crystal structures based on the same precursor system. The goal is to achieve controllable recombination of inorganic coordination units by regulating the crystallization environment while maintaining the basic chemical composition, thereby obtaining crystal materials with different structures and luminescence properties. Furthermore, this will enable the preparation of high-quality, large-size single crystals to meet the application requirements of high-performance X-ray detection and intelligent imaging. Summary of the Invention

[0007] To address the aforementioned technical problems, the present invention aims to provide a method for reconstructing a zero-dimensional indium halide crystal structure based on the same precursor system and the scintillator prepared therefrom. By controlling the crystal growth environment to induce the recombination of inorganic coordination units, different crystal structures can be constructed in a controllable manner, thereby obtaining large-size crystal materials with excellent luminescence and X-ray scintillation properties.

[0008] To achieve the above objectives, the present invention adopts the following technical solution: A method for reconstructing the zero-dimensional indium halide crystal structure based on the same precursor system, the method comprising the following steps: (1) Mix the organic molecular precursor, indium halide precursor, optional doped metal halide precursor, acid, and optional organic solvent to form a saturated precursor solution or a supersaturated precursor solution; use the prepared saturated precursor solution or supersaturated precursor solution as the mother liquor, and obtain zero-dimensional indium halide seed crystals by cooling crystallization method, and then obtain zero-dimensional indium halide crystals by seed crystal method; (2) Adjust the crystallization environment parameters of the zero-dimensional indium halide crystal prepared in step (1) to induce the recombination of inorganic coordination units and prepare zero-dimensional indium halide crystals with different crystal structures to realize the reconstruction of the zero-dimensional indium halide crystal structure; the crystallization environment parameters include at least one of the volume ratio of acid to organic solvent, environmental humidity and environmental temperature.

[0009] According to an embodiment of the present invention, in step (1), the organic molecular precursor is a compound containing a morpholine group. Exemplarily, the compound containing the morpholine group has the structural formula shown in Formula 1 below: Formula 1 In Equation 1, R represents hydrogen and C represents hydrogen. 6-24 Aryl, 5-20 heteroaryl, 3-20 heterocyclic.

[0010] According to an embodiment of the present invention, in formula 1, R is hydrogen, C 6-14 Aryl, 5-14 membered heteroaryl, 3-14 membered heterocyclic.

[0011] According to an embodiment of the present invention, in formula 1, R is hydrogen, C6-12 Aryl, 5-12 heteroaryl, 3-12 heterocyclic.

[0012] According to an embodiment of the present invention, in formula 1, R is hydrogen, C 6-10 Aryl, 5-10 heteroaryl, 3-10 heterocyclic.

[0013] According to an embodiment of the present invention, in Formula 1, R is hydrogen, C6 aryl, 5-6 membered heteroaryl, or 5-6 membered heterocyclic group.

[0014] According to an embodiment of the present invention, the organic molecular precursor is selected from at least one of morpholine, 4-morpholinepyridine, 2-morpholinepyridine, 2-(3-pyridine)morpholine, 4-morpholinepiperidine, 4-phenylmorpholine and 2-phenylmorpholine.

[0015] The term "3-20 membered heterocyclic group" refers to a saturated or unsaturated monovalent monocyclic or bicyclic hydrocarbon ring containing 1-5 heteroatoms independently selected from N, O, and S, preferably a "3-10 membered heterocyclic group". The term "3-10 membered heterocyclic group" also refers to a saturated monovalent monocyclic or bicyclic hydrocarbon ring containing 1-5, preferably 1-3, heteroatoms selected from N, O, and S. The heterocyclic group can be connected to the rest of the molecule via any one of the carbon atoms or a nitrogen atom (if present). Specifically, the heterocyclic group can include, but is not limited to: 4-membered rings, such as azirrobutyl or oxobutyl; 5-membered rings, such as tetrahydrofuranyl, dioxacyclopentenyl, pyrrolyl, imidazoalkyl, pyrazolyl, or pyrrololinyl; or 6-membered rings, such as tetrahydropyranyl, piperidinyl, morpholinyl, dithiaalkyl, thiomorpholinyl, piperazinyl, or trithiaalkyl; or 7-membered rings, such as diazacycloheptyl. Optionally, the heterocyclic group may be benzo-fused. The heterocyclic group may be bicyclic, for example, but not limited to, a 5,5-membered ring, such as a hexahydrocyclopentano[c]pyrrole-2(1H)-yl ring, or a 5,6-membered bicyclic ring, such as a hexahydropyrrolo[1,2-a]pyrazin-2(1H)-yl ring. The nitrogen-containing ring may be partially unsaturated, i.e., it may contain one or more double bonds, for example, but not limited to, 2,5-dihydro-1H-pyrrole, 4H-[1,3,4]thiadiazinyl, 4,5-dihydrooxazolyl, or 4H-[1,4]thiazinyl, or it may be benzo-fused, for example, but not limited to, dihydroisoquinolinyl. According to the invention, the heterocyclic group is non-aromatic.

[0016] Term "C" 6-20 "Aryl" should be understood as preferably representing a monocyclic, bicyclic, or tricyclic hydrocarbon ring having 6 to 20 carbon atoms and possessing monovalent aromaticity or partial aromaticity, preferably "C". 6-14 Aryl. The term "C" 6-14"Aryl" should be understood to preferably represent a monovalent aromatic or partially aromatic monocyclic, bicyclic, or tricyclic hydrocarbon ring ("C") having 6, 7, 8, 9, 10, 11, 12, 13, or 14 carbon atoms. 6-14 Aryl), particularly a ring with 6 carbon atoms (“C6 aryl”), such as phenyl; or biphenyl, or a ring with 9 carbon atoms (“C9 aryl”), such as indenyl or indenyl, or a ring with 10 carbon atoms (“C9 aryl”). 10 Aryl groups, such as tetrahydronaphthyl, dihydronaphthyl, or naphthyl, or rings with 13 carbon atoms (“C…”). 13 Aryl groups, such as fluorene groups, or rings with 14 carbon atoms (“C…”). 14 "Aryl", for example, anthracene.

[0017] The term "5-20-membered heteroaryl" should be understood to include monovalent monocyclic, bicyclic, or tricyclic aromatic ring systems having 5 to 20 ring atoms and containing 1 to 5 heteroatoms independently selected from N, O, and S, such as "5-14-membered heteroaryl". The term "5-14-membered heteroaryl" should also be understood to include monovalent monocyclic, bicyclic, or tricyclic aromatic ring systems having 5, 6, 7, 8, 9, 10, 11, 12, 13, or 14 ring atoms, particularly 5, 6, 9, or 10 carbon atoms, and containing 1 to 5, preferably 1 to 3, heteroatoms independently selected from N, O, and S, and in each case, may be benzofused. Specifically, the heteroaryl group is selected from thienyl, furanyl, pyrroleyl, oxazolyl, thiazolyl, imidazoleyl, pyrazolyl, isoxazolyl, isothiazolyl, oxadiazolyl, triazolyl, thiadiazolyl, thia-4H-pyrazolyl, and their benzo[derivatives], such as benzofuranyl, benzothienyl, benzooxazolyl, benzoisooxazolyl, benzoimidazolyl, benzotriazolyl, indazole, indolyl, isindolyl, etc.; or pyridyl, pyridazinyl, pyrimidinyl, pyrazinyl, triazinyl, and their benzo[derivatives], such as quinolinyl, quinazolinyl, isoquinolinyl, etc.; or acrylinyl, inazinyl, purinyl, and their benzo[derivatives]; or terpenolyl, phthalazinyl, quinazolinyl, quinoxolinyl, naphridinyl, pteridinyl, carbazolyl, acridineyl, phenazinyl, phenothiazinyl, phenothiazinyl, etc.

[0018] According to an embodiment of the present invention, in step (1), the indium halide precursor is selected from at least one of InCl3, InBr3 and InI3.

[0019] According to an embodiment of the present invention, in step (1), the acid is selected from at least one of HCl, HBr and HI.

[0020] According to an embodiment of the present invention, in step (1), the organic solvent is selected from organic solvents with a polarity value greater than 4; for example, the organic solvent is selected from at least one of methanol, ethanol, isopropanol, n-butanol, n-pentanol, glycerol, acetone, acetonitrile and ethyl acetate.

[0021] According to an embodiment of the present invention, in step (1), the doped metal halide precursor is a doped ns 2 Metal halide precursors with electronic configuration, the ns 2 The electronic configuration of the metal is selected from Sb 3+ Bi 3+ Sn 2+ and Te 4+ At least one of them.

[0022] According to an embodiment of the present invention, in step (1), the volume ratio of the acid to the organic solvent is 1:0-5, and the volume of the organic solvent is 0, which means that no organic solvent is added; for example, the volume ratio of the acid to the organic solvent is 1:0, 1:0.1, 1:0.2, 1:0.5, 1:0.8, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5 or 1:5.

[0023] According to an embodiment of the present invention, in step (1), the molar ratio of the organic molecular precursor to the halide is 1-4:1, for example, 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1 or 4:1; the halide includes indium halide precursor and doped metal halide precursor.

[0024] According to an embodiment of the present invention, in step (1), the molar ratio of the indium halide precursor to the doped metal halide precursor is 0.8-1:0-0.2, for example, 0.8:0.2, 0.85:0.15, 0.9:0.1 or 0.95:0.05; the doped metal halide precursor being 0 means that no doped metal halide precursor is added.

[0025] According to an embodiment of the present invention, in step (1), the saturated precursor solution or supersaturated precursor solution refers to the scintillator material formed by the reaction of halides (including indium halide precursors and doped metal halide precursors) with organic molecular precursors being saturated or supersaturated in a mixed system formed by organic solvents and acids.

[0026] According to an embodiment of the present invention, step (1) specifically includes the following steps: (a) Mix an organic molecular precursor, an indium halide precursor, an optional doped metal halide precursor, an acid, and an optional organic solvent, and stir to dissolve under heating conditions to obtain a saturated precursor solution or a supersaturated precursor solution. (b) Divide the saturated or supersaturated precursor solution prepared in step (a) into two portions. Cool one portion to room temperature at a rate of 0.01-5℃ / h to obtain a zero-dimensional indium halide single crystal. Place the obtained zero-dimensional indium halide single crystal as a seed crystal in the other portion of saturated or supersaturated precursor solution. After holding it at a certain temperature for a certain time, cool it to room temperature at a rate of 0.01-5℃ / h and grow the crystal under a certain humidity to achieve the preparation of zero-dimensional indium halide crystal.

[0027] According to an embodiment of the present invention, in step (a), the heating temperature is 80℃-140℃, for example, 80℃, 90℃, 100℃, 110℃, 120℃, 130℃ or 140℃; the heating time is not particularly limited, as long as it ensures that a saturated precursor solution or a supersaturated precursor solution can be prepared under stirring conditions.

[0028] According to an embodiment of the present invention, in step (b), the temperature is reduced to room temperature at a rate of 0.01℃ / h, 0.02℃ / h, 0.05℃ / h, 0.08℃ / h, 0.1℃ / h, 0.2℃ / h, 0.5℃ / h, 0.8℃ / h, 1℃ / h, 1.5℃ / h, 2℃ / h, 2.5℃ / h, 3℃ / h, 3.5℃ / h, 4℃ / h, 4.5℃ / h, or 5℃ / h.

[0029] According to an embodiment of the present invention, in step (b), the certain temperature is 80℃-140℃, for example, 80℃, 90℃, 100℃, 110℃, 120℃, 130℃ or 140℃; the certain time is 5-20 minutes, for example, 5 minutes, 10 minutes, 15 minutes or 20 minutes; the certain humidity is relative humidity 25%-90%, for example, relative humidity 25%, relative humidity 30%, relative humidity 35%, relative humidity 40%, relative humidity 45%, relative humidity 50%, relative humidity 55%, relative humidity 60%, relative humidity 65%, relative humidity 70%, relative humidity 75%, relative humidity 80%, relative humidity 85% or relative humidity 90%.

[0030] According to an embodiment of the present invention, in step (b), the growth time of the crystal is 1-10 days, for example, 1 day, 2 days, 3 days, 4 days, 5 days, 6 days, 7 days, 8 days, 9 days or 10 days.

[0031] According to an embodiment of the present invention, in step (b), the size of the zero-dimensional indium halide crystal prepared is ≥5 mm; preferably, the size of the zero-dimensional indium halide crystal prepared is ≥10 mm.

[0032] According to an embodiment of the present invention, in step (1), by adjusting the ambient humidity and the volume ratio of acid to organic solvent during the preparation process of the zero-dimensional indium halide crystal, zero-dimensional indium halide crystals with different crystal structures can be obtained.

[0033] For example, using 4-morpholinopyridine as an organic molecular precursor, by adjusting the volume ratio of acid to organic solvent during the preparation of the zero-dimensional indium halide crystal, zero-dimensional indium halides with different crystal structures can be obtained, such as (C9H) 13 N2O)4In2Cl 10 :Sb 3+ Crystal and (C9H) 13 N2O)2(H5O2)InCl6:Sb 3+ Crystal.

[0034] According to the embodiment of the present invention, in step (2), the zero-dimensional indium halide crystal prepared in step (1) is placed under specific ambient humidity and ambient temperature to induce the inorganic coordination units to recombine, thereby preparing zero-dimensional indium halide crystals with different crystal structures and realizing the reconstruction of the zero-dimensional indium halide crystal structure.

[0035] According to an embodiment of the present invention, in step (2), the range of environmental humidity control is 25% to 90% relative humidity, for example, 25% relative humidity, 30% relative humidity, 35% relative humidity, 40% relative humidity, 45% relative humidity, 50% relative humidity, 55% relative humidity, 60% relative humidity, 65% relative humidity, 70% relative humidity, 75% relative humidity, 80% relative humidity, 85% relative humidity, or 90% relative humidity.

[0036] According to an embodiment of the present invention, in step (2), the range of ambient temperature control is 20℃-100℃, for example, 20℃, 25℃, 30℃, 35℃, 40℃, 45℃, 50℃, 55℃, 60℃, 65℃, 70℃, 75℃, 80℃, 85℃, 90℃, 95℃ or 100℃.

[0037] According to an embodiment of the present invention, in step (2), the zero-dimensional indium halide crystal prepared in step (1) is placed in a recombination solution or vapor formed by the recombination solution to induce recombination of inorganic coordination units, thereby preparing zero-dimensional indium halide crystals with different crystal structures and realizing the reconstruction of the zero-dimensional indium halide crystal structure; the recombination solution includes acid and / or organic solvent.

[0038] According to an embodiment of the present invention, the acid is selected from at least one of HCl, HBr and HI.

[0039] According to an embodiment of the present invention, the organic solvent is selected from organic solvents with a polarity value greater than 4; exemplaryly, the organic solvent is selected from at least one of methanol, ethanol, isopropanol, n-butanol, n-pentanol, glycerol, acetone, acetonitrile, and ethyl acetate.

[0040] According to an embodiment of the present invention, the volume ratio of the acid to the organic solvent is 1:0-5, and the volume of the organic solvent is 0, which means that no organic solvent is added; exemplaryly, the volume ratio of the acid to the organic solvent is 1:0, 1:0.1, 1:0.2, 1:0.5, 1:0.8, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5 or 1:5.

[0041] According to an embodiment of the present invention, in step (2), the reconstruction process is reversible reconstruction. The reconstruction refers to the transformation between different crystal structures of the zero-dimensional indium halide crystal prepared in step (1) under the action of external stimuli. The external stimuli include at least one of acid stimulation, humidity stimulation, heat stimulation and organic solvent stimulation. That is, the zero-dimensional indium halide crystal prepared in step (1) can achieve reversible transformation between different crystal structures under the action of acid stimulation, humidity stimulation, heat stimulation and organic solvent stimulation.

[0042] According to an embodiment of the present invention, in step (2), the zero-dimensional indium halide crystals with different crystal structures all originate from the same precursor system, and the zero-dimensional indium halide crystals with different crystal structures have different luminescence properties and scintillation performance.

[0043] According to an embodiment of the present invention, in step (2), the structure of the zero-dimensional indium halide crystal includes at least one of a dimer coordination structure, an isolated octahedral coordination structure, and a mixed coordination structure containing coordinated water molecules.

[0044] The present invention also provides a zero-dimensional indium halide scintillator prepared by the above method.

[0045] According to an embodiment of the present invention, the crystal structure of the zero-dimensional indium halide scintillator includes at least one of a dimer coordination structure, an isolated octahedral coordination structure, and a mixed coordination structure containing coordinated water molecules.

[0046] According to an embodiment of the present invention, the zero-dimensional indium halide scintillator has the structural formulas (C4H8ON-RH)2(H5O2)InCl6, (C4H8ON-RH)4(InCl6)[InCl4(H2O)2], and (C4H8ON-RH)4In2Cl 10 (C4H8ON-RH)2(H5O2)InCl6:X, (C4H8ON-RH)4(InCl6)[InCl4(H2O)2]:X, or (C4H8ON-RH)4In2Cl 10 :X; where C4H8ON-R is the chemical formula of the organic molecular precursor, and R is defined as described above; X is the ns dopant in the scintillator. 2 Metal ions with electronic configurations, the ns 2 The electronic configuration of the metal ion is selected from Sb. 3+ Bi 3+ Sn 2+ and Te 4+ One or more of them.

[0047] According to an embodiment of the present invention, the crystal size of the zero-dimensional indium halide scintillator is ≥5 mm; preferably, the crystal size of the zero-dimensional indium halide scintillator is ≥10 mm.

[0048] According to an embodiment of the present invention, the scintillator is doped with ns 2 Metal ions with electronic configurations, the ns 2 The electronic configuration of the metal ion is selected from Sb. 3+ Bi 3+ Sn 2+ and Te 4+ One or more of them.

[0049] According to an embodiment of the present invention, the ns 2 The doping concentration of the metal ions in the electronic configuration is 0-20 mol, preferably 5-10 mol, for example 1 mol%, 2 mol%, 3 mol%, 4 mol%, 5 mol%, 6 mol%, 7 mol%, 8 mol%, 9 mol%, 10 mol%, 12 mol%, 14 mol%, 15 mol%, 16 mol%, 18 mol%, or 20 mol%.

[0050] According to an embodiment of the present invention, the scintillator has broadband light emission, self-trapped exciton light emission, and excellent X-ray scintillation performance.

[0051] The present invention also provides the application of the above-mentioned zero-dimensional indium halide scintillators in high-energy ray detection and imaging, environmental response detection and intelligent imaging.

[0052] According to an embodiment of the present invention, the zero-dimensional indium halide scintillator, after being cut and polished, can be used as a scintillator screen for high-resolution X-ray imaging.

[0053] The beneficial effects of this invention are: 1. This invention achieves for the first time the controllable reconstruction of zero-dimensional indium halide crystal structures under the same precursor system. By adjusting the volume ratio of acid to organic solvent and crystallization environment parameters such as ambient humidity and ambient temperature, different crystal structures such as dimer structures, isolated octahedral structures and mixed coordination structures can be obtained, avoiding the problem of simultaneous changes in multiple structural factors caused by changes in chemical composition in traditional composition engineering.

[0054] 2. This invention establishes the correlation between crystal structure and luminescence performance under the same chemical composition conditions, providing an effective platform for studying the structure-property relationship between inorganic coordination structure, local coordination environment and luminescence behavior in organic-inorganic hybrid metal halides, which is beneficial for realizing the rational design of scintillators.

[0055] 3. This invention employs a strategy combining cooling crystallization and seed crystal method to achieve controllable preparation of high-quality, large-size zero-dimensional indium halide crystals, which is beneficial for meeting the requirements of high-resolution X-ray imaging for scintillator size and crystal quality.

[0056] 4. The zero-dimensional indium halide crystal obtained by this invention has excellent X-ray scintillation performance and reversible environmental response characteristics. It can achieve dynamic control of structure and luminescence properties under various external stimuli and can be applied to fields such as high-energy ray detection and imaging, environmental response detection and intelligent imaging.

[0057] In summary, the method for reconstructing the zero-dimensional indium halide crystal structure of this invention uses organic molecular precursors, indium halide precursors, and optionally added or unadded doped metal halide precursors as raw materials. By controlling the crystallization environment to induce recombination of inorganic coordination units, the zero-dimensional indium halide crystal structure is controllably reconstructed within the same precursor system, thereby obtaining crystal materials with different luminescence and scintillation properties. Furthermore, high-quality, large-size crystals are prepared through cooling crystallization and seed crystal methods, and the reversible transformation of the zero-dimensional indium halide crystal structure is achieved under the stimulation of acid, humidity, heat, and organic solvents. The prepared zero-dimensional indium halide scintillator exhibits excellent luminescence performance, X-ray scintillation performance, high spatial resolution imaging capability, and environmental response characteristics, and can be applied in fields such as high-energy ray detection and imaging, environmental response detection, and intelligent imaging. Attached Figure Description

[0058] Figure 1 The example shown in Example 1 (C9H) 13 N2O)4In2Cl 10 :Sb3+ Crystal structure and schematic diagram of single crystal of the material; Figure 2 The example shown in Example 1 (C9H) 13 N2O)4In2Cl 10 :Sb 3+ Powder XRD and single-crystal XRD of the material, and ultraviolet and X-ray emission spectra; Figure 3 Example 2 shows (C9H) 13 N2O)2(H5O2)InCl6:Sb 3+ Crystal structure and schematic diagram of single crystal of the material; Figure 4 Example 2 shows (C9H) 13 N2O)2(H5O2)InCl6:Sb 3+ Powder XRD and single-crystal XRD of the material, and ultraviolet and X-ray emission spectra; Figure 5 Example 3 shows (C9H) 13 N2O)4(InCl6)[InCl4(H2O)2]:Sb 3+ Crystal structure and schematic diagram of single crystal of the material; Figure 6 Example 3 shows (C9H) 13 N2O)4(InCl6)[InCl4(H2O)2]:Sb 3+ Powder XRD and single-crystal XRD of the material, and ultraviolet and X-ray emission spectra; Figure 7 The example shown in Example 1 (C9H) 13 N2O)4In2Cl 10 :Sb 3+ An image of an object formed by a material under X-ray; Figure 8 The diagram shows the reversible luminescence of the three crystals in Example 4 under ultraviolet light after structural reconstruction. Detailed Implementation

[0059] The technical solution of the present invention will be further described in detail below with reference to specific embodiments. It should be understood that the following embodiments are merely illustrative and explanatory of the present invention, and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are covered within the scope of protection intended by the present invention.

[0060] Unless otherwise specified, the experimental methods used in the following examples are conventional methods; unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0061] Example 1 (C9H 13 N2O)4In2Cl 10 :Sb 3+ Crystal preparation: (a) Weigh out 2 mmol of 4-morpholinopyridine, 1 mmol of SbCl3 and InCl3, of which Sb 3+ A concentration of 0.05 mmol was added to a mixed solvent of 5 mL hydrochloric acid and 20 mL ethanol, and heated and stirred at 120 °C until completely dissolved to form a clear and transparent saturated precursor solution.

[0062] (b) The saturated precursor solution prepared in step (a) was divided into two portions. One portion was cooled at a rate of 5 °C / h to obtain a zero-dimensional indium halide single crystal. The prepared zero-dimensional indium halide single crystal was placed as a seed crystal in the other portion of the saturated precursor solution and held at 120 °C for 5 min. Then, it was cooled to room temperature at a rate of 1 °C / h. Single crystal growth was carried out in an environment with a relative humidity of 25%. After about 7 days of growth, a large-sized transparent crystal was obtained. Luminescence testing showed that it emitted green light under ultraviolet and X-ray conditions.

[0063] Example 2 (C9H 13 N2O)2(H5O2)InCl6:Sb 3+ Crystal preparation: (a) Weigh out 2 mmol of 4-morpholinopyridine, 1 mmol of SbCl3 and InCl3, of which Sb 3+ A 0.05 mmol solution was added to 5 mL of hydrochloric acid and heated and stirred at 120 °C until completely dissolved, forming a clear and transparent saturated precursor solution.

[0064] (b) The saturated precursor solution prepared in step (a) was divided into two portions. One portion was cooled at a rate of 5 °C / h to obtain a zero-dimensional indium halide single crystal. The prepared zero-dimensional indium halide single crystal was placed as a seed crystal in the other portion of the saturated precursor solution and held at 120 °C for 5 min. Then, it was cooled to room temperature at a rate of 1 °C / h. Single crystal growth was carried out in an environment with a relative humidity of 25%. After about 2 days of growth, a large-sized transparent crystal was obtained. Luminescence testing showed that it emitted yellow light under ultraviolet light and X-rays.

[0065] Example 3 (C9H 13 N2O)4(InCl6)[InCl4(H2O)2]:Sb 3+ Crystal preparation: The (C9H) prepared in Example 2 13 N2O)2(H5O2)InCl6:Sb3+ The crystal was stored at 25°C and 80% relative humidity for 24 hours to obtain a new crystal phase (C9H). 13 N2O)4(InCl6)[InCl4(H2O)2]:Sb 3+ Luminescence tests were conducted, and the results showed that it emitted red light under ultraviolet and X-ray conditions.

[0066] Example 4 Take the (C9H) prepared in Example 1 13 N2O)4In2Cl 10 :Sb 3+ Crystalline powder was used as the initial sample. The sample was added to hydrochloric acid solution and thoroughly dispersed, then allowed to stand at room temperature, followed by filtration and natural drying to obtain a new crystalline phase (C9H). 13 N2O)2(H5O2)InCl6:Sb 3+ This indicates that the crystal structure has transformed from a dimer structure to an isolated octahedral structure.

[0067] Furthermore, the obtained (C9H) 13 N2O)2(H5O2)InCl6:Sb 3+ The crystal was stored at 25°C and 80% relative humidity for 24 hours to obtain a new crystal phase (C9H). 13 N2O)4(InCl6)[InCl4(H2O)2]:Sb 3+ This indicates that the crystal further transforms into a mixed coordination structure.

[0068] Subsequently, the obtained (C9H) 13 N2O)4(InCl6)[InCl4(H2O)2]:Sb 3+ When the crystals are stored in an ethanol solution for 24 hours, the resulting crystals revert to the crystalline phase (C9H). 13 N2O)4In2Cl 10 :Sb 3+ This indicates that the crystal has recovered to its initial structure.

[0069] Alternatively, the obtained (C9H) 13 N2O)4(InCl6)[InCl4(H2O)2]:Sb 3+ Heating the crystal at 100℃ for 10 minutes resulted in the crystal reverting to the crystalline phase (C9H). 13 N2O)4In2Cl 10 :Sb 3+ This indicates that the crystal has recovered to its initial structure.

[0070] Meanwhile, under 365nm ultraviolet light irradiation, the crystals with different structures obtained above exhibited different emission colors, and the structural transformations were reversible, indicating that the material can achieve synergistic regulation of structure, luminescence and scintillation performance.

[0071] The above results show that the zero-dimensional indium halide crystal provided by the present invention can achieve reversible structural reconstruction under acid stimulation, humidity stimulation, heat stimulation and organic solvent stimulation, and has good cycle stability. It can be applied to environmental response detection, information encryption and intelligent X-ray imaging and other fields.

[0072] The embodiments of the present invention have been described above. However, the present invention is not limited to the above embodiments. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for reconstructing a zero-dimensional indium halide crystal structure based on the same precursor system, the reconstruction method comprising the following steps: (1) Mix the organic molecular precursor, indium halide precursor, optional doped metal halide precursor, acid, and optional organic solvent to form a saturated precursor solution or a supersaturated precursor solution; use the prepared saturated precursor solution or supersaturated precursor solution as the mother liquor, and obtain zero-dimensional indium halide seed crystals by cooling crystallization method, and then obtain zero-dimensional indium halide crystals by seed crystal method; (2) Adjust the crystallization environment parameters of the zero-dimensional indium halide crystal prepared in step (1) to induce the recombination of inorganic coordination units and prepare zero-dimensional indium halide crystals with different crystal structures to realize the reconstruction of the zero-dimensional indium halide crystal structure; the crystallization environment parameters include at least one of the volume ratio of acid to organic solvent, environmental humidity and environmental temperature.

2. The reconstruction method according to claim 1, wherein, In step (1), the organic molecular precursor is a compound containing a morpholine group. Preferably, the compound containing the morpholine group has the structural formula shown in Formula 1: Formula 1 In Equation 1, R represents hydrogen and C represents hydrogen. 6-24 Aryl, 5-20 heteroaryl, 3-20 heterocyclic. Preferably, in Formula 1, R is hydrogen, C ... 6-14 Aryl, 5-14 membered heteroaryl, 3-14 membered heterocyclic. Preferably, in Formula 1, R is hydrogen, C ... 6-12 Aryl, 5-12 heteroaryl, 3-12 heterocyclic. Preferably, in Formula 1, R is hydrogen, C ... 6-10 Aryl, 5-10 heteroaryl, 3-10 heterocyclic. Preferably, in Formula 1, R is hydrogen, C6 aryl, 5-6 membered heteroaryl, or 5-6 membered heterocyclic group. Preferably, the organic molecular precursor is selected from at least one of morpholine, 4-morpholinepyridine, 2-morpholinepyridine, 2-(3-pyridine)morpholine, 4-morpholinepiperidine, 4-phenylmorpholine and 2-phenylmorpholine. Preferably, in step (1), the indium halide precursor is selected from at least one of InCl3, InBr3 and InI3; And / or, in step (1), the acid is selected from at least one of HCl, HBr and HI; And / or, in step (1), the organic solvent is selected from organic solvents with a polarity value greater than 4; for example, the organic solvent is selected from at least one of methanol, ethanol, isopropanol, n-butanol, n-pentanol, glycerol, acetone, acetonitrile and ethyl acetate; And / or, in step (1), the doped metal halide precursor is a doped ns 2 Metal halide precursors with electronic configuration, the ns 2 The electronic configuration of the metal is selected from Sb 3+ Bi 3+ Sn 2+ and Te 4+ At least one of them; And / or, in step (1), the volume ratio of the acid to the organic solvent is 1:0-5, and the volume of the organic solvent is 0, which means that no organic solvent is added; And / or, in step (1), the molar ratio of the organic molecular precursor to the halide is 1. 4:1; the halide includes indium halide precursors and doped metal halide precursors; And / or, in step (1), the molar ratio of the indium halide precursor to the doped metal halide precursor is 0.8-1:0-0.2; the doped metal halide precursor being 0 means that no doped metal halide precursor is added.

3. The reconstruction method according to claim 1 or 2, wherein, Step (1) specifically includes the following steps: (a) Mix an organic molecular precursor, an indium halide precursor, an optional doped metal halide precursor, an acid, and an optional organic solvent, and stir to dissolve under heating conditions to obtain a saturated precursor solution or a supersaturated precursor solution. (b) Divide the saturated or supersaturated precursor solution prepared in step (a) into two portions. Cool one portion to room temperature at a rate of 0.01-5℃ / h to obtain a zero-dimensional indium halide single crystal. Place the obtained zero-dimensional indium halide single crystal as a seed crystal in the other portion of saturated or supersaturated precursor solution. After holding it at a certain temperature for a certain time, cool it to room temperature at a rate of 0.01-5℃ / h and grow the crystal under a certain humidity to achieve the preparation of zero-dimensional indium halide crystal.

4. The reconstruction method according to claim 3, wherein, In step (a), the heating temperature is 80℃-140℃; And / or, in step (b), the specified temperature is 80℃-140℃; the specified time is 5-20 minutes; and the specified humidity is 25%-90% relative humidity. And / or, in step (b), the crystal growth time is 1-10 days.

5. The reconstruction method according to any one of claims 1-4, wherein, In step (2), the zero-dimensional indium halide crystal prepared in step (1) is placed under specific ambient humidity and temperature to induce the recombination of inorganic coordination units, thereby preparing zero-dimensional indium halide crystals with different crystal structures and realizing the reconstruction of the zero-dimensional indium halide crystal structure. Preferably, in step (2), the range of ambient humidity control is 25% to 90% relative humidity; And / or, in step (2), the range of ambient temperature regulation is 20-100℃.

6. The reconstruction method according to any one of claims 1-5, wherein, In step (2), the zero-dimensional indium halide crystal prepared in step (1) is placed in a recombination solution or vapor formed by the recombination solution to induce recombination of inorganic coordination units, thereby preparing zero-dimensional indium halide crystals with different crystal structures and realizing the reconstruction of the zero-dimensional indium halide crystal structure; the recombination solution includes acid and / or organic solvent. Preferably, the acid is selected from at least one of HCl, HBr, and HI; And / or, the organic solvent is selected from organic solvents with a polarity value greater than 4; for example, the organic solvent is selected from at least one of methanol, ethanol, isopropanol, n-butanol, n-pentanol, glycerol, acetone, acetonitrile, and ethyl acetate; And / or, the volume ratio of the acid to the organic solvent is 1:0-5, and the volume of the organic solvent is 0, which means that no organic solvent is added.

7. The reconstruction method according to any one of claims 1-6, wherein, In step (2), the reconstruction process is reversible reconstruction. The reconstruction means that the zero-dimensional indium halide crystal prepared in step (1) can achieve the transformation between different crystal structures under the action of external stimuli. The external stimuli include at least one of acid stimulation, humidity stimulation, heat stimulation and organic solvent stimulation. Preferably, in step (2), the zero-dimensional indium halide crystals with different crystal structures all originate from the same precursor system, and the zero-dimensional indium halide crystals with different crystal structures have different luminescence properties and scintillation performance.

8. The zero-dimensional indium halide scintillator prepared by the reconstruction method according to any one of claims 1-7.

9. The zero-dimensional indium halide scintillator according to claim 8, wherein the crystal structure of the zero-dimensional indium halide scintillator includes at least one of a dimer coordination structure, an isolated octahedral coordination structure, and a mixed coordination structure containing coordinated water molecules. Preferably, the zero-dimensional indium halide scintillator has the structural formula (C4H8ON-RH)2(H5O2)InCl6, (C4H8ON-RH)4(InCl6)[InCl4(H2O)2], or (C4H8ON-RH)4In2Cl 10 (C4H8ON-RH)2(H5O2)InCl6:X, (C4H8ON-RH)4(InCl6)[InCl4(H2O)2]:X, or (C4H8ON-RH)4In2Cl 10 :X; where, C4H8ON-R is the chemical formula of the organic molecular precursor, and R is defined as described above; X is the ns dopant in the scintillator. 2 Metal ions with electronic configurations, the ns 2 The electronic configuration of the metal ion is selected from Sb. 3+ Bi 3+ Sn 2+ and Te 4+ One or more of them. Preferably, the crystal size of the zero-dimensional indium halide scintillator is ≥5 mm. Preferably, the scintillator is doped with ns 2 Metal ions with electronic configurations, the ns 2 The electronic configuration of the metal ion is selected from Sb. 3+ Bi 3+ Sn 2+ and Te 4+ One or more of them. Preferably, the ns 2 The doping concentration of the electronically configured metal ions is 0-20 mol.