A eutectic solvent, its preparation method, and a method for recovering gold and platinum based on the eutectic solvent.

By utilizing the anion exchange mechanism of eutectic solvents, the problem of poor selectivity and low efficiency in the recovery of gold and platinum in existing technologies has been solved, achieving high selectivity and high efficiency in the recovery process. This method is suitable for the green and environmentally friendly recovery of gold and platinum from electronic waste, spent catalysts, and ores.

CN123108306APending Publication Date: 2026-11-17SHENZHEN SHINESKY BIOLOGICAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610978503.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-02
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing gold and platinum recovery technologies suffer from poor selectivity, low efficiency, poor stability, and low recycling rates. Furthermore, traditional methods are highly polluting and costly.

Method used

A eutectic solvent composed of hydrogen bond acceptors and hydrogen bond donors connected by hydrogen bonds is used. By adjusting the types and molar ratios of hydrogen bond acceptors and hydrogen bond donors, a stable liquid solvent is formed. Gold and platinum are selectively extracted using anion exchange mechanisms. Combined with pretreatment and back-extraction techniques, efficient recovery is achieved.

Benefits of technology

It achieves highly selective and efficient recovery of gold and platinum, with extraction rates greater than 99.99% and 99%, respectively. The extraction rate of interfering elements is less than 5%. The reaction conditions are mild and the solvent can be recycled, making it suitable for the recovery of large quantities of low-grade gold and platinum.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108306A_ABST
    Figure CN123108306A_ABST
Patent Text Reader

Abstract

This invention discloses a eutectic solvent, its preparation method, and a method for recovering gold and platinum based on the eutectic solvent. It relates to the field of metal and resource recovery technology, aiming to address the core technical shortcomings of existing precious metal recovery technologies, such as high toxicity and pollution, poor selectivity, inability to simultaneously and efficiently recover gold and platinum, and poor cycle stability. This invention uses a hydrophobic eutectic solvent prepared from one or more of tetramethylammonium chloride, hexadecyltrimethylammonium bromide, tetradecyldimethylbenzylammonium chloride, hexadecyltributylphosphine bromide, and dodecyltributylphosphine bromide as hydrogen bond acceptors, and one or more of hexanoic acid, menthol, thymol, octanoic acid, decanoic acid, and oleic acid as hydrogen bond donors. Through raw material pretreatment, selective extraction, and solvent regeneration and recycling processes, it achieves highly efficient and selective recovery of gold and platinum. This invention achieves a gold extraction rate ≥99.99%, a platinum extraction rate ≥99%, and a base metal extraction rate of less than 5%. The reaction conditions are mild, the solvent has excellent recyclability, and the entire process involves no highly toxic or corrosive reagents, making it environmentally friendly. It is suitable for various raw materials such as waste circuit boards, waste catalysts, and gold-bearing ores, and is easily applied on an industrial scale.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal recycling and resource recovery technology, specifically to a method for the efficient and selective recovery of gold and platinum from secondary resources based on a eutectic solvent system. Background Technology

[0002] Electronic waste has become one of the fastest-growing categories of solid waste globally. It mainly originates from industries such as consumer electronics, home appliances, semiconductors, electronic components, new energy, and batteries. Electronic waste contains important resources such as gold and platinum and has high recycling value.

[0003] Traditional technologies for secondary resource recovery of gold and platinum mainly include three categories: pyrometallurgical, hydrometallurgical, and biological recovery. Pyrometallurgical recovery is characterized by high pollution, high energy consumption, and high emissions; hydrometallurgical recovery often uses hazardous chemicals such as aqua regia and cyanide; biological recovery is characterized by long processing cycles, low efficiency, and high environmental requirements. Eutectic solvents, first reported in 2003, are liquids formed by mixing hydrogen bond donors and hydrogen bond acceptors in a specific ratio. Eutectic solvent extraction and separation technology, as an emerging precious metal recovery technology, has advantages such as low cost, low toxicity, and simple process. However, existing reports show problems such as poor selectivity, low recovery efficiency, poor stability, and low cycle count.

[0004] Therefore, there is a need to develop a green, environmentally friendly, highly selective, and low-cost recycling method for the extraction and recovery of gold and platinum. Summary of the Invention

[0005] In view of the shortcomings of the prior art, the purpose of this invention is to provide a eutectic solvent and its preparation method, as well as a method for recovering gold and platinum based on the eutectic solvent. This method can improve economic efficiency, avoid the use of hazardous chemicals, reduce pollution, energy consumption and emissions, and improve recovery efficiency, aiming to solve the problems of poor selectivity and low recovery efficiency of existing recovery methods.

[0006] The technical solution of the present invention is as follows: In a first aspect, the present invention provides a eutectic solvent, wherein the eutectic solvent is composed of a hydrogen bond acceptor and a hydrogen bond donor through a hydrogen bond network; The hydrogen bond acceptor is one or more of tetramethylammonium chloride, hexadecyltrimethylammonium bromide, tetradecyldimethylbenzylammonium chloride, hexadecyltributylphosphine bromide, and dodecyltributylphosphine bromide; The hydrogen bond donor is one or more of the following: hexanoic acid, menthol, thymol, caprylic acid, decanoic acid, and oleic acid; The molar ratio of the hydrogen bond acceptor to the hydrogen bond donor is (1~10):(1~10).

[0007] Optionally, the hydrogen bond acceptor is dodecyltributylphosphine bromide or hexadecyltributylphosphine bromide, and the hydrogen bond donor is hexanoic acid.

[0008] Optionally, the hydrogen bond acceptor is hexadecyltributylphosphine bromide, and the hydrogen bond donor is thymol.

[0009] Optionally, the molar ratio of the hydrogen bond acceptor to the hydrogen bond donor is (1~3):(1~3).

[0010] A second aspect of the present invention provides a method for preparing the eutectic solvent of the present invention, comprising the steps of: mixing the hydrogen bond acceptor and the hydrogen bond donor in a molar ratio of (1~10):(1~10), and then heating and stirring to obtain the eutectic solvent.

[0011] Optionally, the heating temperature is 20~90℃; And / or, the stirring speed is 300~800 rpm.

[0012] A third aspect of the present invention provides a method for recovering gold and platinum based on a eutectic solvent, comprising the steps of: S1: Provide a eutectic solvent, wherein the eutectic solvent is the eutectic solvent described in this invention; S2: Provide the raw material to be extracted, which contains gold and / or platinum; pretreat the raw material to be extracted to obtain the extract solution; S3: The eutectic solvent and the extract to be extracted are mixed and stirred at room temperature to obtain a mixed solution. The mixed solution is then centrifuged to obtain a first upper layer solution and a first lower layer solution. S4: The first upper layer solution is back-extracted to obtain a regenerated eutectic solvent, thus completing the recovery of gold and / or platinum; the regenerated eutectic solvent can be returned to step S3 for recycling.

[0013] Optionally, the raw material to be extracted is one of the following: gold and / or platinum-containing electronic waste, gold and / or platinum-containing spent catalyst, gold and / or platinum-containing ore, gold and / or platinum-containing waste liquid, and gold and / or platinum-containing waste residue.

[0014] Optionally, the eutectic solvent and the extract to be extracted are mixed at a ratio of (1~10) g: (1~5000) mL, preferably (1~5) g: (1~5000) mL; The centrifugation speed is 3000~10000 rpm, and the centrifugation time is 5~30 min.

[0015] Optionally, step S4 specifically includes: Add a back-extraction agent to the first upper layer solution, then stir and centrifuge to obtain a second upper layer solution and a second lower layer solution; Add sodium borohydride solution to the second lower layer solution, then stir and centrifuge to complete the recovery of gold and / or platinum; The second upper layer solution is recovered, washed with water, and dried to obtain a regenerated eutectic solvent.

[0016] Compared with the prior art, the beneficial effects of the present invention include: The eutectic solvent provided by this invention has the characteristics of adjustable physical properties, low toxicity, and environmental friendliness when extracting gold and platinum. At the same time, it is simple to operate, has low requirements for equipment and other hardware conditions, and is easy to scale up for production.

[0017] The eutectic solvent provided by this invention is environmentally friendly in the extraction of gold and platinum, avoiding the use of hazardous chemicals such as cyanide and aqua regia in traditional methods.

[0018] The eutectic solvent provided by this invention exhibits high selectivity for gold and platinum during extraction, with an extraction rate of over 99.99% for gold and over 99% for platinum. However, the extraction rates for common interfering elements found in electronic waste, catalysts, and ores, such as copper, iron, nickel, tin, lead, arsenic, rhodium, and ruthenium, are all below 5%. The eutectic solvent provided by this invention has the ability to accurately and directionally extract gold and platinum.

[0019] The eutectic solvent provided by this invention requires a small amount of eutectic solvent when extracting gold and platinum. The maximum ratio of eutectic solvent to extractant can reach 1g:5000mL, making it suitable for large-scale extraction of low-grade gold and platinum.

[0020] The eutectic solvent provided by this invention provides mild reaction conditions and low energy consumption when extracting gold and platinum, and extraction can be performed at room temperature without additional heating.

[0021] The eutectic solvent provided by this invention has high extraction efficiency when extracting gold and platinum. After adding the eutectic solvent of this invention, a 99% extraction rate of gold and platinum can be achieved within 5 minutes.

[0022] The eutectic solvent provided by this invention has excellent recycling performance when extracting gold and platinum. It can be directly recycled, and after 10 cycles, the extraction rate of gold and platinum remains above 98%.

[0023] The eutectic solvent provided by this invention is formed by mixing the aforementioned hydrogen bond acceptors and hydrogen bond donors in a specific molar ratio. The hydrogen bond acceptors include quaternary ammonium salts and quaternary phosphine salts, while the hydrogen bond donors include carboxylic acids and phenolic compounds. The halogen anions in the hydrogen bond acceptors form strong hydrogen bond interactions with the polar functional groups such as carboxyl and hydroxyl groups of the hydrogen bond donor molecules, constructing a continuous three-dimensional hydrogen bond network. This results in a melting point of the mixed solvent lower than that of the individual components, thus creating a stable liquid state at room temperature. By adjusting the types and molar ratio of hydrogen bond acceptors and hydrogen bond donors, the hydrophobicity, viscosity, and anion exchange capacity of the eutectic solvent can be precisely controlled to adapt to different scenarios. Through anion exchange mechanisms, the eutectic solvent interacts with chloroaurate ions (AuCl4) in electronic waste, spent catalysts, and ore leachates (i.e., solutions formed after pretreatment). - ) and chloroplatinate ions (PtCl6²) - A hydrophobic ionic complex is formed. During this process, the halide anions originally present in the eutectic solvent are converted by AuCl4. - or PtCl6² - In this process, the latter, after entering the eutectic solvent phase, combines with quaternary ammonium salt cations or quaternary phosphine salt cations through electrostatic interactions to form stable ion pairs, thereby achieving the selective transfer of gold and platinum from the aqueous phase to the eutectic solvent phase. This technology not only provides a green, efficient, low-volatility, and non-toxic recovery pathway, but also enables the precise capture of gold and platinum from leachates of complex electronic waste, spent catalysts, or ores by designing eutectic solvents with specific compositions, achieving high-purity separation and recovery. Attached Figure Description

[0024] Figure 1 This is a schematic flowchart of a method for recovering gold and platinum based on a eutectic solvent, provided as an embodiment of the present invention. Detailed Implementation

[0025] This invention provides a eutectic solvent, its preparation method, and a method for recovering gold and platinum based on the eutectic solvent. To make the objectives, technical solutions, and effects of this invention clearer and more explicit, the invention is further described in detail below. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0026] This invention provides a eutectic solvent, wherein the eutectic solvent is composed of hydrogen bond acceptors and hydrogen bond donors through a hydrogen bond network; The hydrogen bond acceptor is one or more of tetramethylammonium chloride, hexadecyltrimethylammonium bromide, tetradecyldimethylbenzylammonium chloride, hexadecyltributylphosphine bromide, and dodecyltributylphosphine bromide; The hydrogen bond donor is one or more of the following: hexanoic acid, menthol, thymol, caprylic acid, decanoic acid, and oleic acid; The molar ratio of the hydrogen bond acceptor to the hydrogen bond donor is (1~10):(1~10).

[0027] In a preferred embodiment, the hydrogen bond acceptor is dodecyltributylphosphine bromide or hexadecyltributylphosphine bromide, and the hydrogen bond donor is hexanoic acid.

[0028] The eutectic solvent prepared by combining the hydrogen bond acceptor and hydrogen bond donor exhibits a stronger affinity for gold and platinum, which can effectively improve the subsequent recovery efficiency.

[0029] In a preferred embodiment, the hydrogen bond acceptor is hexadecyltributylphosphine bromide, and the hydrogen bond donor is thymol.

[0030] The eutectic solvent prepared by combining the hydrogen bond acceptor and hydrogen bond donor exhibits a stronger affinity for gold and platinum, which can effectively improve the subsequent recovery efficiency.

[0031] In a preferred embodiment, the molar ratio of the hydrogen bond acceptor to the hydrogen bond donor is (1~3):(1~3), such as 1:1, 1:2, 1:3, 2:1, 2:3, 3:1, 3:2, etc. Other specific values ​​within the above range can be selected, and will not be elaborated here.

[0032] In a preferred embodiment, the hydrogen bond acceptor is two of tetramethylammonium chloride, hexadecyltrimethylammonium bromide, tetradecyldimethylbenzylammonium chloride, hexadecyltributylphosphine bromide, and dodecyltributylphosphine bromide. The hydrogen bond donor is one of hexanoic acid, menthol, thymol, caprylic acid, decanoic acid, and oleic acid; The molar ratio of the hydrogen bond acceptor to the hydrogen bond donor is (1~5):(1~5).

[0033] In a preferred embodiment, the hydrogen bond acceptor is one of tetramethylammonium chloride, hexadecyltrimethylammonium bromide, tetradecyldimethylbenzylammonium chloride, hexadecyltributylphosphine bromide, and dodecyltributylphosphine bromide; The hydrogen bond donor is two of the following: hexanoic acid, menthol, thymol, caprylic acid, decanoic acid, and oleic acid. The molar ratio of the hydrogen bond acceptor to the hydrogen bond donor is (1~5):(1~5).

[0034] In a preferred embodiment, the hydrogen bond acceptor is hexadecyltributylphosphine bromide, and the hydrogen bond donor is a mixed carboxylic acid composed of hexanoic acid and octanoic acid; wherein the molar ratio of hexadecyltributylphosphine bromide to the mixed carboxylic acid (hexanoic acid and octanoic acid) is 1:2, and the molar ratio of hexanoic acid to octanoic acid is 1:1.

[0035] The eutectic solvent prepared within this ratio range exhibits higher stability, maintaining a homogeneous and stable liquid state at room temperature. It also demonstrates optimal selective adsorption of gold and platinum, while achieving higher raw material utilization and avoiding waste due to component imbalances, making it more suitable for the needs of large-scale industrial production.

[0036] This invention provides a method for preparing the eutectic solvent as described above, comprising the steps of: mixing the hydrogen bond acceptor and the hydrogen bond donor in a molar ratio of (1~10):(1~10), followed by heating and stirring to obtain the eutectic solvent.

[0037] In one embodiment, the heating temperature is 20~90℃, such as 20℃, 30℃, 50℃, 70℃, 90℃, etc. Other specific values ​​within the above range can be selected, and will not be described in detail here.

[0038] Heating within this temperature range can promote the full interaction between hydrogen bond acceptors and hydrogen bond donors to form a uniform and stable eutectic system, without damaging the molecular structure of the components due to excessively high temperatures. It can also reduce energy consumption in the preparation process and control production costs.

[0039] In one embodiment, the stirring speed is 300~800 rpm, such as 300 rpm, 400 rpm, 500 rpm, 600 rpm, 700 rpm, 800 rpm, etc. Other specific values ​​within the above range can be selected, and will not be described in detail here.

[0040] Stirring within this speed range allows for more uniform mixing of the hydrogen bond acceptor and hydrogen bond donor, promoting full contact between them, while avoiding unnecessary energy consumption due to excessively high speeds. After stirring, a clear and homogeneous liquid product is obtained, which is the desired eutectic solvent.

[0041] Combination Figure 1 As shown, this embodiment of the invention provides a method for recovering gold and platinum based on a eutectic solvent, comprising the following steps: S1: Provide a eutectic solvent, wherein the eutectic solvent is the eutectic solvent described in this invention; S2: Provide the raw material to be extracted, which contains gold and / or platinum; pretreat the raw material to be extracted to obtain the extract solution; S3: The eutectic solvent and the extract to be extracted are mixed and stirred at room temperature to obtain a mixed solution. The mixed solution is then centrifuged to obtain a first upper layer solution and a first lower layer solution. S4: The first upper layer solution is back-extracted to obtain a regenerated eutectic solvent, thus completing the recovery of gold and / or platinum; the regenerated eutectic solvent can be returned to step S3 for recycling.

[0042] Compared with the prior art, the technical advantages of this embodiment include: The eutectic solvent provided in this embodiment has the characteristics of adjustable physical properties, low toxicity, and environmental friendliness when extracting gold and platinum. At the same time, it is simple to operate, has low requirements for equipment and other hardware conditions, and is easy to scale up for production.

[0043] The eutectic solvent provided in this embodiment is environmentally friendly in its raw material source when extracting gold and platinum, avoiding the use of hazardous chemicals such as cyanide and aqua regia in traditional methods.

[0044] The eutectic solvent provided in this embodiment exhibits high selectivity for gold and platinum during extraction, with an extraction rate greater than 99.99% for gold and greater than 99% for platinum. However, the extraction rates for common interfering elements found in electronic waste, catalysts, and ores, such as copper, iron, nickel, tin, lead, arsenic, rhodium, and ruthenium, are all less than 5%. The eutectic solvent provided by this invention has the ability to accurately and directionally extract gold and platinum.

[0045] The eutectic solvent provided in this embodiment requires a small amount of solvent when extracting gold and platinum. The maximum ratio of eutectic solvent to extractant can be 1g:5000mL, making it suitable for large-scale extraction of low-grade gold and platinum.

[0046] The eutectic solvent provided in this embodiment provides mild reaction conditions and low energy consumption when extracting gold and platinum. Extraction can be performed at room temperature without additional heating.

[0047] The eutectic solvent provided in this embodiment has high extraction efficiency when extracting gold and platinum. After adding the eutectic solvent of this invention, a 99% extraction rate of gold and platinum can be achieved within 5 minutes.

[0048] The eutectic solvent provided in this embodiment has excellent recycling performance when extracting gold and platinum. It can be directly recycled, and after 10 cycles, the extraction rate of gold and platinum remains above 98%.

[0049] The eutectic solvent provided by this invention is composed of hydrogen bond acceptors and hydrogen bond donors mixed in a specific molar ratio. The hydrogen bond acceptors include quaternary ammonium salts and quaternary phosphine salts, and the hydrogen bond donors include carboxylic acids and phenolic compounds. The halogen anions in the hydrogen bond acceptors form strong hydrogen bond interactions with the carboxyl and hydroxyl groups of the hydrogen bond donor molecules, constructing a continuous three-dimensional hydrogen bond network. This results in a melting point of the mixed solvent lower than that of a single component, thus creating a stable liquid state at room temperature. By adjusting the types and molar ratio of hydrogen bond acceptors and hydrogen bond donors, the hydrophobicity, viscosity, and anion exchange capacity of the eutectic solvent can be precisely controlled to adapt to different scenarios. The eutectic solvent, through anion exchange mechanisms, interacts with chloroaurate ions (AuCl4) in electronic waste, spent catalysts, and ore leachates.- ) and chloroplatinate ions (PtCl6²) - A hydrophobic ionic complex is formed. During this process, the halide anions originally present in the eutectic solvent are converted by AuCl4. - or PtCl6² - In this process, the latter, after entering the eutectic solvent phase, combines with quaternary ammonium salt cations or quaternary phosphine salt cations through electrostatic interactions to form stable ion pairs, thereby achieving the selective transfer of gold and platinum from the aqueous phase to the eutectic solvent phase. This technology not only provides a green, efficient, low-volatility, and non-toxic recovery pathway, but also enables the precise capture of gold and platinum from the leachates of complex electronic waste, spent catalysts, or ores by designing eutectic solvents with specific compositions, achieving high-purity separation and recovery. In one embodiment, the raw material to be extracted is one of the following: gold and / or platinum-containing electronic waste, gold and / or platinum-containing spent catalysts, gold and / or platinum-containing ores, gold and / or platinum-containing waste liquid, or gold and / or platinum-containing waste residue.

[0050] In one embodiment, the step of pretreating the raw material to be extracted to obtain the extract solution specifically includes: filtering the waste liquid containing gold and / or platinum to obtain the extract solution.

[0051] In one embodiment, the step of pretreating the raw material to be extracted to obtain the extract solution specifically includes: leaching the gold and / or platinum-containing waste catalyst in an acid solution to obtain the extract solution.

[0052] In one embodiment, the step of pretreating the raw material to be extracted to obtain the extract liquid specifically includes: mechanically crushing the gold and / or platinum-containing electronic waste to obtain powder, leaching the powder in a mixed solution of HCl-H2O2, and separating the solid and liquid to obtain the pretreated liquid.

[0053] In one embodiment, the eutectic solvent and the extract to be extracted are mixed at a volume ratio of (1~10) g:(1~5000) mL, preferably (1~5) g:(1~5000) mL, such as 1 g:1000 mL, 1 g:2000 mL, 1 g:3000 mL, 1 g:4000 mL, 1 g:5000 mL, etc. Other specific values ​​within the above range can be selected, and will not be described in detail here.

[0054] The eutectic solvent provided in this embodiment requires a small amount of solvent when extracting gold and platinum. The maximum ratio of eutectic solvent to extractant can be 1g:5000mL, making it suitable for large-scale extraction of low-grade gold and platinum.

[0055] In one embodiment, the centrifugation speed is 3000~10000 rpm, such as 3000 rpm, 4000 rpm, 5000 rpm, 6000 rpm, 7000 rpm, 8000 rpm, 9000 rpm, 10000 rpm, etc. Other specific values ​​within the above range can be selected, and will not be described in detail here.

[0056] In one embodiment, the centrifugation time is 5 to 30 minutes, such as 5 minutes, 8 minutes, 10 minutes, 15 minutes, 20 minutes, 22 minutes, 25 minutes, 30 minutes, etc. Other specific values ​​within the above range can be selected, and will not be described in detail here.

[0057] In one implementation, step S4 specifically includes: Add a back-extraction agent to the first upper layer solution, then stir and centrifuge to obtain a second upper layer solution and a second lower layer solution; Add sodium borohydride solution (sodium borohydride acts as a reducing agent to reduce gold / platinum) to the second lower layer solution, then stir and centrifuge to complete the recovery of gold and / or platinum; The second upper layer solution is recovered, washed with water, and dried to obtain a regenerated eutectic solvent, which can be recycled in step S3.

[0058] It should be noted that this embodiment is not limited to the back-extraction method; separation and recovery can also be achieved through heating, electrodeposition, displacement precipitation, co-precipitation, and other methods.

[0059] The present invention will be further described below through several specific embodiments.

[0060] In the following embodiments of the present invention, all reagents used were purchased from Shanghai Titan Technology Co., Ltd., with an AR purity. They were used directly upon receipt without further purification or processing. The elemental content data in the embodiments were detected using an inductively coupled plasma optical emission spectrometer (ICP-OES), specifically an Agilent ICP-OES 720ES.

[0061] Example 1 S1: Weigh 2g of dodecyltributylphosphine bromide and 2g of hexanoic acid, mix them, and stir at 300rpm for 20min at 80℃ to obtain the hydrophobic eutectic solvent DES1.

[0062] S2: The gold-containing waste liquid was filtered to obtain the extract. The concentration of gold in the extract was measured to be 50 ppm by ICP. S3: Take 1g of the eutectic solvent DES1 and 2L of the extract to be extracted, and stir at 300rpm for 5min at room temperature to obtain a mixed solution. Centrifuge the mixed solution at 10000rpm for 10min to obtain a first upper layer and a first lower layer, which is the aqueous phase. Sample and test the gold concentration in the lower aqueous phase. ICP results show that the gold concentration in the lower aqueous phase is 0.003ppm, and the gold extraction rate is >99%.

[0063] S4: The first upper layer solution is back-extracted using 0.5 mol / L hydrochloric acid solution as the back-extractant. The back-extractant is added to the first upper layer solution at a volume ratio of 4:1. After stirring at 150 rpm for 1 hour at room temperature, the mixture is centrifuged at 10,000 rpm for 10 minutes. The second upper layer solution obtained after centrifugation is washed with water and dried to obtain the regenerated hydrophobic eutectic solvent DES1. 0.1 g / mL sodium borohydride solution is added to the separated second lower layer solution to reduce gold. The volume ratio of the second lower layer solution to sodium borohydride solution is 10:1. The mixture is then stirred at 150 rpm for 10 minutes at room temperature, followed by centrifugation at 10,000 rpm for 30 minutes to complete the gold recovery. The regenerated hydrophobic eutectic solvent DES1 is returned to step S3 as a eutectic solvent and recycled under the same process conditions. The number of cycles and the corresponding gold extraction rate are shown in Table 1. After ten cycles, the gold extraction rate is 98%.

[0064] Table 1. Number of cycles of the eutectic solvent and the corresponding gold extraction rate in Example 1

[0065] Example 2 S1: Weigh 2g of hexadecyltributylphosphine bromide and 1g of hexanoic acid, mix them, and stir at 300rpm for 20min at 80℃ to obtain the hydrophobic eutectic solvent DES2.

[0066] S2: The commercial platinum-carbon catalyst was leached in hydrochloric acid solution for 5 hours to obtain the extract. The concentration of platinum in the extract was measured to be 100 ppm by ICP.

[0067] S3: Take 1g of the eutectic solvent DES2 and 2L of the extract to be obtained, and stir at 300rpm for 20min at room temperature to obtain a mixed solution. Centrifuge the mixed solution at 10000rpm for 10min to obtain a first upper layer and a first lower layer, which is the aqueous phase. The platinum concentration in the lower aqueous phase was measured by sampling. The ICP results showed that the platinum concentration in the lower aqueous phase was 0.99ppm, and the platinum extraction rate was >99%.

[0068] S4: The first upper layer solution is back-extracted using 0.5 mol / L hydrochloric acid solution as the back-extractant. The back-extractant is added to the first upper layer solution at a volume ratio of 4:1. After stirring at 150 rpm for 1 hour at room temperature, the mixture is centrifuged at 10,000 rpm for 10 minutes. The second upper layer solution obtained after centrifugation is washed with water and dried to obtain the regenerated hydrophobic eutectic solvent DES2. 0.1 g / mL sodium borohydride solution is added to the separated second lower layer solution to reduce platinum. The volume ratio of the second lower layer solution to sodium borohydride solution is 10:1. The mixture is then stirred at 150 rpm for 10 minutes at room temperature, followed by centrifugation at 10,000 rpm for 30 minutes to complete the recovery of platinum. The regenerated hydrophobic eutectic solvent DES2 is returned to step S3 as a eutectic solvent and recycled under the same process conditions. The number of cycles and the corresponding platinum extraction rate are shown in Table 2. After ten cycles, the platinum extraction rate is 98%.

[0069] Table 2. Number of cycles of the eutectic solvent and the corresponding platinum extraction rate in Example 2.

[0070] Example 3 S1: Weigh 2g of hexadecyltributylphosphine bromide and 2.96g of thymol, mix them, and stir at 300rpm for 20min at 80℃ to obtain the hydrophobic eutectic solvent DES3.

[0071] S2: The waste circuit boards were mechanically crushed to obtain powder. The powder was then leached in a mixed solution of HCl and H2O2 at 80°C for 3 hours. Solid-liquid separation was performed to obtain a pretreatment solution. The metal concentrations in the pretreatment solution were measured by ICP: Au 40ppm, Pt 2ppm, Cu 8500ppm, Ni 450ppm, Fe 600ppm, and Pb 220ppm.

[0072] S3: Take 2g of eutectic solvent DES3 and 2L of pretreatment solution, and stir at 300rpm for 2h at room temperature to obtain a mixed solution. Centrifuge the mixed solution at 10000rpm for 10min to obtain a first upper layer solution and a first lower layer solution, which is the aqueous phase. Samples were taken to detect the metal concentration in the lower aqueous phase, and the extraction rate is shown in Table 3.

[0073] S4: The first upper layer solution is subjected to stepwise back-extraction. Specifically, 0.5 mol / L thiourea solution is used as the back-extraction agent to back-extract gold. The back-extraction agent is added to the first upper layer solution at a volume ratio of 4:1. After stirring at 150 rpm for 1 hour at room temperature, the solution is centrifuged at 10,000 rpm for 10 minutes. The resulting second upper layer solution is the second back-extraction solution. 0.1 g / mL sodium borohydride solution is added to the resulting second lower layer solution to reduce gold. The volume ratio of the second lower layer solution to sodium borohydride solution is 10:1. The solution is then stirred at 150 rpm for 10 minutes at room temperature and centrifuged at 10,000 rpm for 30 minutes to complete the recovery of gold. Platinum was then back-extracted using 0.5 mol / L hydrochloric acid solution as the stripping agent. The stripping agent to the second stripping solution was added to the solution to be back-extracted, with a volume ratio of 4:1. The mixture was stirred at 150 rpm for 1 hour at room temperature, then centrifuged at 10,000 rpm for 10 minutes. The resulting upper third layer was washed with water and dried to obtain the regenerated hydrophobic eutectic solvent DES3. Platinum was then reduced by adding 0.1 g / mL sodium borohydride solution to the lower third layer, with a volume ratio of 10:1. The mixture was then stirred at 150 rpm for 10 minutes at room temperature, followed by centrifugation at 10,000 rpm for 30 minutes, completing the recovery of platinum. The regenerated hydrophobic eutectic solvent DES3 can be returned to step S3 as a eutectic solvent for recycling under the same process conditions.

[0074] Table 3. Extraction rates of each element by the eutectic solvent in Example 3.

[0075] Comparative Example 1 The only difference from Example 1 is that the eutectic solvent DES1 is replaced with dodecyltributylphosphine bromide or hexanoic acid.

[0076] Results: When using dodecyltributylphosphine bromide alone, the gold extraction rate was only 55%. When using hexanoic acid alone, the gold extraction rate was less than 10%.

[0077] Comparative Example 2 The only difference from Example 2 is that tetrabutylammonium chloride is used instead of hexadecyltributylphosphine bromide, and DES is prepared by mixing it with hexanoic acid at a molar ratio of 1:2.

[0078] Results: Under the same conditions, the extraction rate of platinum using the tetrabutylammonium chloride-hexanoic acid DES system was only 80%.

[0079] Comparative Example 3 The only difference from Example 3 is that commercially available tributyl phosphate (TBP) is used instead of the eutectic solvent DES3 in Example 3.

[0080] Results: TBP achieved extraction rates of 96% for Au and 88% for Pt, but exhibited poor selectivity with co-extraction rates of 30%-60% for impurity elements such as Cu, Ni, Fe, and Pb.

[0081] In summary, this invention provides a eutectic solvent, its preparation method, and a method for recovering gold and platinum based on the eutectic solvent. It relates to the field of metal and resource recovery technology, aiming to address the core technical shortcomings of existing precious metal recovery technologies, such as high toxicity and pollution, poor selectivity, inability to simultaneously and efficiently recover gold and platinum, and poor cycle stability. This invention uses a hydrophobic eutectic solvent prepared from one or more of tetramethylammonium chloride, hexadecyltrimethylammonium bromide, tetradecyldimethylbenzylammonium chloride, hexadecyltributylphosphine bromide, and dodecyltributylphosphine bromide as hydrogen bond acceptors, and one or more of hexanoic acid, menthol, thymol, octanoic acid, decanoic acid, and oleic acid as hydrogen bond donors. Through raw material pretreatment, selective extraction, and solvent regeneration and recycling processes, it achieves highly efficient and selective recovery of gold and platinum. This invention achieves a gold extraction rate of ≥99.99%, a platinum extraction rate of ≥99%, and a base metal extraction rate of less than 5%. The reaction conditions are mild, the solvent has excellent recyclability, and there are no highly toxic or corrosive reagents throughout the process. It is environmentally friendly and suitable for various raw materials such as waste circuit boards, waste catalysts, and gold-bearing ores, making it easy to apply on a large industrial scale.

[0082] It should be understood that the application of the present invention is not limited to the examples above. Those skilled in the art can make improvements or modifications based on the above description, and all such improvements and modifications should fall within the protection scope of the appended claims.

Claims

1. A deep eutectic solvent characterized in that, The eutectic solvent is composed of hydrogen bond acceptors and hydrogen bond donors through a hydrogen bond network; The hydrogen bond acceptor is one or more of tetramethylammonium chloride, hexadecyltrimethylammonium bromide, tetradecyldimethylbenzylammonium chloride, hexadecyltributylphosphine bromide, and dodecyltributylphosphine bromide; The hydrogen bond donor is one or more of the following: hexanoic acid, menthol, thymol, caprylic acid, decanoic acid, and oleic acid; The molar ratio of the hydrogen bond acceptor to the hydrogen bond donor is (1~10):(1~10). 2.The deep eutectic solvent of claim 1, wherein, The hydrogen bond acceptor is dodecyltributylphosphine bromide or hexadecyltributylphosphine bromide, and the hydrogen bond donor is hexanoic acid.

3. The deep eutectic solvent of claim 1, wherein, The hydrogen bond acceptor is hexadecyltributylphosphine bromide, and the hydrogen bond donor is thymol.

4. The deep eutectic solvent of claim 1, wherein, The molar ratio of the hydrogen bond acceptor to the hydrogen bond donor is (1~3):(1~3).

5. A method of producing the eutectic solvent according to any one of claims 1 to 4, characterized by, The process includes the following steps: mixing the hydrogen bond acceptor and the hydrogen bond donor in a molar ratio of (1~10):(1~10), followed by heating and stirring to obtain the eutectic solvent.

6. The method of producing a deep eutectic solvent according to claim 5, wherein The heating temperature is 20~90℃; And / or, the stirring speed is 300~800 rpm.

7. A method for recovering gold and platinum based on a deep eutectic solvent, characterized by, Including the following steps: S1: Provide a eutectic solvent, wherein the eutectic solvent is the eutectic solvent according to any one of claims 1 to 4; S2: Provide the raw material to be extracted, which contains gold and / or platinum; pretreat the raw material to be extracted to obtain the extract solution; S3: The eutectic solvent and the extract to be extracted are mixed and stirred at room temperature to obtain a mixed solution. The mixed solution is then centrifuged to obtain a first upper layer solution and a first lower layer solution. S4: The first upper layer solution is back-extracted to obtain a regenerated eutectic solvent, thus completing the recovery of gold and / or platinum; the regenerated eutectic solvent can be returned to step S3 for recycling.

8. The method for recovering gold and platinum based on a deep eutectic solvent according to claim 7, characterized in that, The raw material to be extracted is one of the following: gold and / or platinum-containing electronic waste, gold and / or platinum-containing spent catalyst, gold and / or platinum-containing ore, gold and / or platinum-containing waste liquid, and gold and / or platinum-containing waste residue.

9. The method for recovering gold and platinum based on a deep eutectic solvent according to claim 7, characterized in that, Mix the eutectic solvent with the extract at a ratio of (1~10) g: (1~5000) mL; The centrifugation speed is 3000~10000 rpm, and the centrifugation time is 5~30 min.

10. The method for recovering gold and platinum based on a deep eutectic solvent according to claim 7, characterized in that, Step S4 specifically includes: Add a back-extraction agent to the first upper layer solution, then stir and centrifuge to obtain a second upper layer solution and a second lower layer solution; Add sodium borohydride solution to the second lower layer solution, and then recover gold and / or platinum by stirring and centrifugation; The second upper layer solution is recovered, washed with water, and dried to obtain a regenerated eutectic solvent.