A novel method for smelting G115 steel and the resulting G115 steel and its applications.

By using recycled G115 steel shavings as raw material, combined with a multi-process collaborative method involving deep dephosphorization in an EAF furnace, batch addition of low-carbon lime and alloys in LF refining, VD vacuum treatment, and argon-filled protection in die casting, the difficulties in composition control and cost in the G115 steel smelting process have been solved, achieving efficient and low-cost G115 steel production.

CN123108403APending Publication Date: 2026-11-17BAOWU SPECIAL METALLURGICAL (MAANSHAN) GAOJIN TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611205108.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The smelting process of G115 steel is complex, the composition is difficult to control, the raw material cost is high, and existing technologies are difficult to achieve stable production, lacking mature technologies that are widely mastered.

Method used

Using recycled G115 steel shavings as raw material, a multi-process collaborative method is employed, including deep dephosphorization in an EAF furnace, batch addition of low-carbon lime and alloys in LF refining, VD vacuum treatment, and argon-filled mold casting protection, to control the precision and purity of the composition, reduce harmful impurities, and prevent secondary oxidation.

Benefits of technology

Significantly reduce raw material costs, broaden the process operation window, improve the finished product qualification rate, reduce ingot defects, and achieve the production of G115 steel with high purity and high yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108403A_ABST
    Figure CN123108403A_ABST
Patent Text Reader

Abstract

This invention discloses a novel method for smelting G115 steel and its application. The method includes: using recycled G115 steel shavings as raw material; deep dephosphorization by oxygen blowing and carbon injection in an EA furnace, controlling the final C ≤ 0.04% and P ≤ 0.003%, with a tapping temperature of 1660~1680℃ and oxygen activity < 800ppm; adding low-carbon lime during LF refining, deoxidizing the slag surface with SiFe powder, and adding metallic Cr or low-carbon ferrochrome, Co, Cu, and W at ≥1600℃; argon blowing throughout the VD vacuum treatment process, with pump inlet ≤ 8min, holding pressure at 66.7Pa ≥ 20min, and hydrogen concentration ≤ 2.0ppm; and in-mold casting using in-mold argon filling, MWD-1 protective slag, and holding at temperature ≥ 8h. The synergistic operation of each process in this invention achieves low cost, easy operation, high-precision alloying, and high purity control, significantly reducing ingot defects, improving yield and product stability. The resulting G115 steel is suitable for main steam pipelines.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metallurgical technology, specifically to a new method for smelting G115 steel and the resulting G115 steel and its applications. Background Technology

[0002] G115 is a martensitic heat-resistant steel (material grade: 08Cr9W3Co3VNbCuBN), mainly used in key components of ultra-supercritical thermal power units with steam parameters of 630℃ and above, such as main steam pipelines. This material exhibits significantly better oxidation resistance and creep strength than traditional P92 steel, allowing for a reduction of approximately one-third in pipe wall thickness and about half in weight, making it a crucial material for supporting high-end energy equipment. However, the smelting and preparation of G115 presents extremely high technical barriers. This steel employs a multi-element composite strengthening design with W, Co, Cu, N, and B, requiring precise control of the content of each alloying element during smelting. The composition windows for sensitive elements such as C, B, and N are particularly stringent, and the requirements for harmful elements (P, S) and gaseous substances (O, N, H) in the steel are far higher than those for conventional heat-resistant steels. Therefore, its production process is complex, typically requiring multiple steps including electric arc furnace (EAF) primary smelting, LF refining (using a large amount of white slag), VD vacuum deep degassing, and mold casting with protective coating. Each step has a narrow process window, making control extremely difficult. These technical challenges mean that the industrial-scale trial production of G115 requires over a decade of continuous research and development, with substantial R&D investment. Only a very few companies with strong technological accumulation, financial strength, and supply chain integration capabilities can achieve stable production. Currently, there is a lack of widely mastered, mature technology, necessitating the development of a new method for smelting G115 with stable quality. Summary of the Invention

[0003] This invention addresses the shortcomings of existing technologies by providing a novel method for smelting G115 steel using recycled materials. The method includes the following steps: Batching: Using 50-60 tons of recycled G115 steel shavings as raw material, which are reclaimed scraps generated during the machining of G115 steel. Existing G115 smelting techniques generally utilize large quantities of primary pig iron, purchased high-nickel scrap steel, and various alloy materials for batching, resulting in high raw material costs and significant difficulty in controlling the nickel content of the molten steel. This method uses 50-60 tons of recycled G115 steel shavings as raw material in the batching stage. This recycled scrap, generated during the machining of G115 steel, effectively reduces the raw material cost per ton of steel while ensuring the purity of the molten steel and that the chemical composition of the finished product meets the G115 standard requirements. This significantly reduces the overall smelting production cost and improves the economic benefits for enterprises.

[0004] Furthermore, the method also includes: EAF furnace smelting: the prepared furnace charge is heated to melt, and oxygen and carbon are blown and injected at 1200-1700℃ for deep dephosphorization, controlling the C ≤ 0.04% and P ≤ 0.003% at the electric furnace endpoint, controlling the tapping temperature at 1660-1680℃, and the oxygen activity before tapping is < 800ppm. The endpoint control adopts existing technology, generally by taking samples after melting and analyzing the composition.

[0005] Furthermore, the method also includes: LF refining: heating the slag obtained after electric furnace smelting to 1400-1700℃, adding 100-300kg / batch of lime with a carbon content of less than 0.2% in 1-3 batches, using 75-85kg of SiFe powder for slag surface deoxidation, controlling the argon pressure to ensure that the molten steel does not overflow the slag surface, ensuring that the alloy is fully melted and the slag color turns white, adding metallic Cr or ferrochrome, metallic Co, copper plates and ferrotungsten with a carbon content of less than 0.04% in 1-3 batches, 0.6-1.0 tons per batch, when adding metals in batches, the temperature is ≥1600℃. Low-carbon lime is added in batches. During the early refining stage, the lime is heated and slag is formed. The batch size is determined based on the slag thickness and desulfurization capacity. If the slag thickness is insufficient or the desulfurization efficiency is low, low-carbon lime is added in 3 batches. If the slag thickness is moderate and the desulfurization effect is good, it can be added in 1-2 batches. The amount of low-carbon lime added in each batch is controlled between 100-300 kg. By continuously increasing the slag basicity through multiple slag-forming processes, deep desulfurization is stably achieved, ensuring that the finished product S ≤ 0.006%. The batch addition of metals such as Cr is determined based on the amount of each element in the molten steel and the state of the slag system. According to current technology, the content of each element in the molten steel is generally detected by spectroscopy. If the slag surface is severely yellowed and cannot quickly turn white after adding deoxidizer, it indicates that the deoxidation capacity of the molten steel is insufficient. Continuing to add more will aggravate alloy burn-off, and it must be forcibly stopped. Generally, adding less than 3 batches is sufficient.

[0006] Furthermore, the method also includes: VD vacuum treatment: during VD vacuum treatment, the tank is evacuated, and argon gas is continuously blown into the molten steel as a stirring gas. The entire VD vacuum treatment is argon blowing operation, and the argon gas flow rate is 120-170 NL / min.

[0007] Furthermore, the method also includes: during VD vacuum treatment, the pump inlet time is ≤8min; the holding time at 66.7Pa is ≥20min; the hydrogen concentration is ≤2.0ppm; and the ladle temperature is 1555~1565℃.

[0008] Furthermore, the method also includes in-mold casting: argon is filled into the mold at a flow rate of 80-120 NL / min for 30 min, and MWD-1 protective slag is used. The MWD-1 protective slag is composed of the following components: CaO, Al2O3, SiO2, MgO, CaF2, and FeO in a mass ratio of 45-55:15-25:3-13:13-23:0.5-1.5. After casting, the mold is lifted and hot-sent or annealed after ≥8 hours.

[0009] The G115 material obtained using the above method has the following composition: C 0.065-0.095%, Si≤0.5%, Mn 0.30-0.70%, P≤0.015%, S≤0.006%, Ni≤0.10%, Cr 8.50-9.50%, Cu 0.50-1.10%, W 2.40-3.10%, Co 2.85-3.20%, and N 0.005-0.010%. It meets the hardness requirements of G115 steel: HBW 195~250 or HV 195~265; it meets the requirements for non-metallic inclusions of G115 steel: according to the GB / T 10561-2005 Grade A evaluation method, the sum of the fine series grades of various inclusions shall not exceed 5.5, and the sum of the coarse series grades shall not exceed 4.5; it meets the grain size requirements of G115 steel: when the outer diameter of the steel pipe is not greater than 250mm, the actual grain size should reach Grade 4 or finer; when the outer diameter is greater than 250mm, the average austenite grain size should reach Grade 0 or finer, or the martensite grain size should reach Grade 3 or finer.

[0010] The smelting method of this invention produces G115 steel material, which can therefore be used to manufacture main steam pipes.

[0011] The beneficial effects achieved by this invention using the above technical solution are as follows: First, it significantly reduces raw material costs and greatly improves economic efficiency. Existing G115 smelting technologies generally use large amounts of virgin pig iron, high-nickel purchased scrap steel, and various alloy materials for steel blending, resulting in high raw material costs. This invention uses 50-60 tons of G115 steel shavings as the main raw material in the batching stage. This recycled material is the scrap generated from machining G115 steel. By replacing purchased virgin material with recycled material of the same steel grade, high-value alloying elements such as Cr, Co, and W in the steel can be effectively recovered, significantly reducing the raw material cost per ton of steel and significantly reducing the overall smelting production cost. Simultaneously, since the recycled material and the target steel grade share the same composition, the problem of difficult-to-control residual elements such as Ni in purchased scrap steel is avoided, reducing the difficulty of composition control from the source.

[0012] II. Expanding the process operation window and reducing the difficulty of controlling each process step: G115 steel has a complex composition and strict standards. Existing technologies have narrow process windows for each process step, resulting in extremely high control difficulty. This invention effectively expands the process window through the following measures:

[0013] EAF furnace stage: Deep dephosphorization is achieved through oxygen blowing and carbon injection at 1200-1700℃, with the endpoint C ≤ 0.04% and P ≤ 0.003%, and the oxygen activity before tapping < 800ppm. In existing technologies, dephosphorization and decarburization are contradictory; high oxygen supply makes it difficult to form high-basicity, high-oxidizing slag in the later stages, which is detrimental to dephosphorization operations. This invention provides operators with clear process boundaries by explicitly defining the temperature range and endpoint control indicators for oxygen blowing and carbon injection, reducing the risk of excessive component levels due to blind operation.

[0014] In the LF refining process: carbon powder deoxidation is explicitly prohibited (to avoid carbon gain), and the alloy addition temperature is limited to ≥1600℃, with a single batch feed rate of 0.6~1.0 tons. Existing technologies rely heavily on manual experience for alloy addition, which cannot optimize the feeding scheme and hinders narrow composition control. This invention quantifies the lower temperature limit and single batch feed rate, making operations more data-driven. Simultaneously, real-time spectral detection provides feedback on composition and slag condition, dynamically determining whether to continue adding, forming a closed-loop control of "detection-judgment-execution," significantly reducing the uncertainty caused by reliance on manual experience.

[0015] The vacuum stage of VD (Vacuum Dehydrogenation) is clearly defined with a pump inlet time ≤ 8 min, a holding time of 66.7 Pa ≥ 20 min, and a hydrogen concentration of ≤ 2.0 ppm. While existing technologies generally favor lower vacuum levels for dehydrogenation, they lack clear time-vacuum matching parameters. The quantitative parameters of this invention allow operators to precisely control the vacuum processing rhythm, avoiding incomplete dehydrogenation due to insufficient holding time or disruption to production schedules due to excessive holding time.

[0016] III. Precise Control of Alloy Elements to Ensure Narrow Composition Qualification Rate: In LF refining, this invention involves adding low-carbon lime (100-300 kg / batch) in 1-3 batches to continuously increase slag basicity through phased slag formation, achieving stable deep desulfurization and ensuring that the finished product S≤0.006%; SiFe powder is used for slag surface deoxidation, and carbon powder is prohibited to effectively prevent carbon increase during refining; ferrochrome (Cr or C≤0.04%), Co, copper plates, and ferrotungsten (0.6-1.0 tons per batch) are added in batches, with the composition monitored in real time by spectral detection after each batch. Addition is stopped once the lower limit requirement of internal control is reached. This "small amount, multiple times, real-time detection, and dynamic termination" alloy addition strategy effectively solves the core problem of narrow composition control in G115 steel, enabling precise control of the content of sensitive elements such as C, Cr, Co, W, and Cu.

[0017] IV. Effectively Reduces Harmful Impurities in Steel and Improves Steel Purity: This invention controls harmful impurities through multi-stage synergistic control: Deep dephosphorization: The EAF furnace controls the final phosphorus content to ≤0.003% through oxygen blowing and carbon injection, reducing the harmful effects of phosphorus at the source; Deep desulfurization: LF refining ensures finished product sulfur content ≤0.006% by adding low-carbon lime in batches and maintaining white slag operation; Forced dehydrogenation: VD vacuum treatment limits the holding time to ≥20 min at 66.7 Pa, forcibly reducing hydrogen hydrogen content to ≤2.0 ppm, effectively preventing hydrogen-induced cracking and white spot defects; Prevention of secondary oxidation: The in-mold argon purging protection (80-120 NL / min, argon purging for 30 min) in the casting stage, combined with a special MWD-1 protective slag, effectively reduces secondary oxidation and slag entrapment during the casting process. Through the above multi-stage synergistic control, this invention systematically ensures the purity of molten steel.

[0018] V. Reducing ingot defects and improving yield and product stability; In existing mold casting processes, the lack of anti-splashing measures for the upper ingot, poor performance of the protective slag, or unclean molds can easily lead to defects such as inclusions, bubbles, and heavy scale on the surface or under the ingot. This invention adopts the following measures in the mold casting process: In-mold argon purging protection: argon flow rate 80-120 NL / min, purging time 30min, effectively isolating air and preventing secondary oxidation of molten steel; Special MWD-1 protective slag: composed of CaO, Al2O3, SiO2, MgO, CaF2, and FeO in a mass ratio of 45-55:15-25:3-13:13-23:0.5-1.5, which has good adsorption of inclusions and lubrication functions; Long-term heat preservation after casting: hoisting and hot delivery or annealing treatment ≥8 hours after casting, effectively reducing internal stress and crack tendency of the ingot.

[0019] In summary, this invention forms an organic whole through the close connection and synergistic effect of multiple processes, including deep dephosphorization in the EAF furnace, precise alloying in LF refining, forced dehydrogenation in VD vacuum, and full-process protection in ingot casting. Each process cooperates and supports the others: the EAF furnace provides high-quality primary steel with low phosphorus and low oxygen activity for LF refining, laying the foundation for purity; LF refining achieves precise control of narrow composition through batch lime slag formation, prohibition of carbon powder deoxidation, and limiting alloy addition temperature and batch feed amount, while providing steel with qualified composition and suitable temperature for VD vacuum treatment; VD vacuum treatment effectively eliminates hydrogen-induced defects through forced dehydrogenation and precise temperature control, providing high-purity qualified steel for ingot casting; argon purging protection, special protective slag, and post-casting insulation measures in the ingot casting process effectively prevent secondary oxidation of the steel and ingot cracking. This complete process chain is interconnected, fully leveraging the advantages of each process to create a synergistic effect of "1+1>2". The preparation method of this invention has synergistic steps, which can significantly reduce surface and internal defects of ingots, improve yield and product stability, and ultimately form a complete G115 steel smelting technology solution with low cost, easy operation, high precision, high purity and high yield. It has important practical application value for promoting the stable industrial production of G115 steel. Attached Figure Description

[0020] Figure 1 The image shows the finished G115 steel material obtained in Example 1.

[0021] Detailed Description of Embodiments: To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments are described clearly and completely below. The following embodiments are used to illustrate the present invention, but are not intended to limit the scope of the present invention. Unless otherwise described, the present invention uses existing technology. Embodiment 1: The present invention provides a new method for smelting G115 using new materials, comprising the following steps: (I) Batching: using G115 steel shavings recycled material as raw material, wherein the G115 steel shavings recycled material is 50t, and the G115 steel shavings recycled material is recycled scrap material generated from machining G115 steel.

[0022] (ii) Electric arc furnace (EAF) smelting:

[0023] The prepared furnace charge is loaded into the charging basket in two batches and then added into the electric furnace. Power is supplied to raise the temperature, and the charge is gradually melted using an electric arc. When the temperature of the molten steel reaches approximately 1500°C, oxygen is blown into the furnace and carbon powder is injected to remove phosphorus (P) from the molten steel through an oxidation reaction.

[0024] During the smelting process, steel composition is sampled and analyzed periodically. Oxygen blowing is stopped when the carbon (C) content in the molten steel drops to ≤0.04% and the phosphorus (P) content drops to ≤0.003%, meeting the electric furnace endpoint control requirements. Before tapping, the dissolved oxygen activity in the molten steel is measured using a constant oxygen probe, and the oxygen activity is controlled to be <800ppm. The tapping temperature of the electric furnace is 1660–1680℃. Eccentric bottom tapping (EBT) is used during tapping, with slag retention to ensure that most of the oxide slag remains in the electric furnace. Only the primary molten steel (with a small amount of floating slag) is poured into the ladle, which is then transported to the LF refining station by crane.

[0025] In this embodiment, the actual steel composition measured during tapping from the electric furnace was: C 0.03%, P 0.002%, oxygen activity 750ppm, and tapping temperature 1670℃.

[0026] (III) LF Refining

[0027] The ladle is positioned behind the LF refining station. The electrodes are lowered to supply power for heating, and the LF refining operation begins.

[0028] 1. Slag Heating and Formation: Using an electric arc, the slag-forming material pre-added to the ladle is melted, forming a reactive refining slag layer on the surface of the molten steel. Depending on the slag's fluidity and condition, low-carbon lime is added to the slag surface in 1-3 batches, with each batch containing 100-300 kg. After adding lime, heating continues to maintain the slag layer's good fluidity and chemical reactivity. The lime used is low-carbon lime with a carbon content below 0.2%.

[0029] 2. Slag Surface Deoxidation: Slag surface deoxidation is carried out using ferrosilicon powder (SiFe powder), and the use of carbon powder (C powder) is strictly prohibited. During the deoxidation process, argon gas is continuously introduced into the bottom of the ladle for bottom stirring. The argon gas pressure is adjusted and controlled to prevent the molten steel from overflowing the slag surface, thus preventing the exposed molten steel from absorbing gas. As the deoxidation reaction proceeds, the slag color gradually changes from black to white (i.e., "slag color turning white"), indicating that the refined slag has changed from oxidizing to reducing properties, possessing good desulfurization and inclusion adsorption capabilities.

[0030] 3. Temperature measurement and sampling: After ensuring that all alloys have melted, perform temperature measurement and sampling, analyze the composition of the molten steel, and calculate the amount of each alloy to be added based on the analysis results.

[0031] 4. Alloying: After the slag turns white, add metallic chromium (ferrochrome with a carbon content below 0.04%), metallic cobalt, copper plates, and ferrotungsten in batches, with each batch consisting of 0.6 to 1.0 tons. The molten steel temperature must be ≥1600℃ when adding each batch of alloys to ensure rapid melting and uniform diffusion, avoiding segregation of alloying elements. The preferred order of addition is: first add metallic chromium or low-carbon ferrochrome, then add metallic cobalt and copper plates, and finally add ferrotungsten. After each batch of alloys is added, adjust the argon stirring intensity appropriately, and add the next batch only after the alloys are fully melted, until the content of each alloying element reaches the target requirements.

[0032] In this embodiment, the slag obtained after electric furnace smelting is heated to 1400℃. Lime is added in two batches during the LF refining process: 100kg of lime is added in the first batch, and 250kg of lime is added in the second batch. 80kg of SiFe powder is used for slag surface deoxidation. When the molten steel temperature reaches 1620℃, alloys are added in three batches: the first batch adds 1.0 ton of metallic chromium (with 0.6 ton of ferrochrome with a carbon content of less than 0.04%), the second batch adds 0.9 ton of metallic cobalt and 0.6 ton of copper plate, and the third batch adds 0.7 ton of ferrotungsten. Each batch ensures that the molten steel temperature is ≥1600℃. After alloying, samples are taken and analyzed to ensure that the molten steel composition meets all target ranges. The molten steel temperature is adjusted to 1690℃ (meeting the VD inlet temperature requirements), and the ladle is hoisted to the VD vacuum treatment station.

[0033] (iv) VD vacuum treatment

[0034] The ladle is placed into the VD vacuum tank, the tank lid is closed, and the vacuum pump is started to evacuate the molten steel. At the same time, high-purity argon (Ar) gas is continuously blown into the molten steel through the permeable bricks at the bottom of the ladle as a stirring gas. Argon gas is used throughout the entire process from the start of vacuuming until the pump stops (pump withdrawal), and switching to nitrogen gas is strictly prohibited.

[0035] During vacuum pumping, the pump inlet time (the time from starting the vacuum pump to the pressure inside the tank dropping to the working vacuum level) must be ≤8 minutes. Once the vacuum level inside the tank reaches 66.7 Pa, this vacuum level should be maintained for at least 20 minutes. Under these vacuum conditions, gases such as hydrogen (H), nitrogen (N), and oxygen (O) in the molten steel continuously escape from the molten steel under low partial pressure. These gases are carried to the slag surface by argon bubbles and then pumped away by the vacuum pump, achieving deep degassing. Simultaneously, the stirring effect of bottom-blown argon promotes the homogenization of the molten steel's temperature and composition and facilitates the flotation and removal of non-metallic inclusions.

[0036] After the required pressure holding time is reached, stop evacuation and venting (pump withdrawal). Immediately after venting, take samples for analysis to confirm the nitrogen (N) content in the molten steel, ensuring that the nitrogen content of the finished product is within the target range of 0.005~0.010%. Use a hydrogen analyzer to determine the hydrogen content in the molten steel, ensuring H≤2.0ppm. Simultaneously, measure the temperature of the molten steel. When the temperature drops to the ladle temperature range of 1555~1565℃, hoist the ladle to the casting station.

[0037] In this embodiment, the entire VD vacuum treatment process involved argon blowing, with an argon flow rate of 150 NL / min, a pump inlet time of 7 minutes, and a pressure holding time of 66.7 Pa for 22 minutes. The hydrogen content was determined to be 1.2 ppm, the nitrogen content analysis result was 0.008%, and the actual measured temperature of the molten steel was 1560℃.

[0038] (v) Ingot casting

[0039] After the VD pump is deactivated, the steel casting station is notified to prepare for casting. Before casting, argon (Ar) gas is introduced into the ingot mold for gas protection, and the air inside the mold is purged to prevent secondary oxidation of the molten steel during casting. The ladle is hoisted onto the casting car, aligned with the center of the ingot mold, and cast at a rate of 13.5t / ingot. During the casting process, a special MWD-1 type protective slag is used to cover the surface of the molten steel to keep it warm, prevent oxidation, and adsorb inclusions.

[0040] After casting, the steel ingot cools and solidifies naturally in the mold. It can only be lifted and removed from the mold ≥8 hours after casting, and then hot-sent (to the forging or rolling process) or annealed to eliminate the internal stress generated during the cooling process.

[0041] In this embodiment, the argon flow rate is 100 NL / min, the argon charging time is 30 min, and the MWD-1 protective slag is composed of CaO, Al2O3, SiO2, MgO, CaF2, and FeO in a mass ratio of 50:20:10:18:1. After casting, it is cooled for 10 hours, lifted and demolded. The steel ingot has good surface quality, without cracks, scale, or other defects, and is then sent to an annealing furnace for annealing treatment.

[0042] The chemical composition analysis of the G115 steel ingot obtained through the above process is as follows: C 0.078%, Si 0.32%, Mn 0.52%, P 0.008%, S 0.003%, Ni 0.06%, Cr 9.12%, Cu 0.82%, W 2.76%, Co 3.05%, N 0.008%, all meeting the G115 steel standard requirements. After subsequent forging and heat treatment, the finished steel was tested using existing technical methods, and the hardness HBW was 195-250. According to the GB / T 10561-2005 Grade A rating method, the total fine inclusions were no greater than grade 5.5, and the total coarse inclusions were no greater than grade 4.5; the average austenite grain size reached grade 0, meeting the G115 steel material standard and suitable for use as a material for steam main pipelines. The obtained G115 steel... Figure 1 As shown.

[0043] Example 2: The present invention provides a new method for smelting G115 using new materials, comprising the following steps: (i) Batching: using G115 steel shavings recycled material as raw material, wherein the G115 steel shavings recycled material is 60t, and the G115 steel shavings recycled material is recycled scrap material generated from machining G115 steel.

[0044] (ii) Electric arc furnace (EAF) smelting:

[0045] The prepared furnace charge is loaded into the charging basket in two batches and then added into the electric furnace. Power is supplied to raise the temperature, and the charge is gradually melted using an electric arc. When the temperature of the molten steel reaches approximately 1200°C, oxygen is blown into the furnace and carbon powder is injected to remove phosphorus (P) from the molten steel through an oxidation reaction.

[0046] During the smelting process, steel composition is sampled and analyzed periodically. Oxygen blowing is stopped when the carbon (C) content in the molten steel drops to ≤0.04% and the phosphorus (P) content drops to ≤0.003%, meeting the electric furnace endpoint control requirements. Before tapping, the dissolved oxygen activity in the molten steel is measured using a constant oxygen probe, and the oxygen activity is controlled to be <800ppm. The tapping temperature of the electric furnace is 1660–1680℃. Eccentric bottom tapping (EBT) is used during tapping, with slag retention to ensure that most of the oxide slag remains in the electric furnace. Only the primary molten steel (with a small amount of floating slag) is poured into the ladle, which is then transported to the LF refining station by crane.

[0047] In this embodiment, the actual steel composition measured during tapping from the electric furnace was: C 0.01%, P 0.001%, oxygen activity 700ppm, and tapping temperature 1660℃.

[0048] (III) LF Refining

[0049] The ladle is positioned behind the LF refining station. The electrodes are lowered to supply power for heating, and the LF refining operation begins.

[0050] 1. Slag Heating and Formation: Using an electric arc, the slag-forming material pre-added to the ladle is melted, forming a reactive refining slag layer on the surface of the molten steel. Depending on the slag's fluidity and condition, low-carbon lime is added to the slag surface in 1-3 batches, with each batch containing 100-300 kg. After adding lime, heating continues to maintain the slag layer's good fluidity and chemical reactivity. The lime used in this invention is low-carbon lime with a carbon content below 0.2%.

[0051] 2. Slag Surface Deoxidation: Slag surface deoxidation is carried out using ferrosilicon powder (SiFe powder), and the use of carbon powder (C powder) is strictly prohibited. During the deoxidation process, argon gas is continuously introduced into the bottom of the ladle for bottom stirring. The argon gas pressure is adjusted and controlled to prevent the molten steel from overflowing the slag surface, thus preventing the exposed molten steel from absorbing gas. As the deoxidation reaction proceeds, the slag color gradually changes from black to white (i.e., "slag color turning white"), indicating that the refined slag has changed from oxidizing to reducing properties, possessing good desulfurization and inclusion adsorption capabilities.

[0052] 3. Temperature measurement and sampling: After ensuring that all alloys have melted, perform temperature measurement and sampling, analyze the composition of the molten steel, and calculate the amount of each alloy to be added based on the analysis results.

[0053] 4. Alloying: After the slag turns white, add metallic chromium (ferrochrome with a carbon content below 0.04%), metallic cobalt, copper plates, and ferrotungsten in batches, with each batch consisting of 0.6 to 1.0 tons. The molten steel temperature must be ≥1600℃ when adding each batch of alloys to ensure rapid melting and uniform diffusion, avoiding segregation of alloying elements. The preferred order of addition is: first add metallic chromium or low-carbon ferrochrome, then add metallic cobalt and copper plates, and finally add ferrotungsten. After each batch of alloys is added, adjust the argon stirring intensity appropriately, and add the next batch only after the alloys are fully melted, until the content of each alloying element reaches the target requirements.

[0054] In this embodiment, the slag obtained after electric arc furnace smelting is heated to 1700℃, and a batch of low-carbon lime (300 kg of lime) is added during the LF refining process. 85 kg of SiFe powder is used for slag surface deoxidation. When the molten steel temperature reaches 1610℃, alloys are added in three batches: the first batch adds 0.6 tons of metallic chromium (with 1 ton of micro-carbon ferrochrome added simultaneously), the second batch adds 0.6 tons of metallic cobalt and 1 ton of copper plate, and the third batch adds 1 ton of ferrotungsten. Each batch ensures the molten steel temperature is ≥1600℃. After alloying, samples are taken for analysis, and all steel composition meets the target range. The molten steel temperature is adjusted to 1680℃ (meeting the VD inlet temperature requirements), and the ladle is hoisted to the VD vacuum treatment station.

[0055] (iv) VD vacuum treatment

[0056] The ladle is placed into the VD vacuum tank, the tank lid is closed, and the vacuum pump is started to evacuate the molten steel. At the same time, high-purity argon (Ar) gas is continuously blown into the molten steel through the permeable bricks at the bottom of the ladle as a stirring gas. Argon gas is used throughout the entire process from the start of vacuuming until the pump stops (pump withdrawal), and switching to nitrogen gas is strictly prohibited.

[0057] During vacuum pumping, the pump inlet time (the time from starting the vacuum pump to the pressure inside the tank dropping to the working vacuum level) must be ≤8 minutes. Once the vacuum level inside the tank reaches 66.7 Pa, this vacuum level should be maintained for at least 20 minutes. Under these vacuum conditions, gases such as hydrogen (H), nitrogen (N), and oxygen (O) in the molten steel continuously escape from the molten steel under low partial pressure. These gases are carried to the slag surface by argon bubbles and then pumped away by the vacuum pump, achieving deep degassing. Simultaneously, the stirring effect of bottom-blown argon promotes the homogenization of the molten steel's temperature and composition and facilitates the flotation and removal of non-metallic inclusions.

[0058] After the required pressure holding time is reached, stop evacuation and venting (pump withdrawal). Immediately after venting, take samples for analysis to confirm the nitrogen (N) content in the molten steel, ensuring that the nitrogen content of the finished product is within the target range of 0.005~0.010%. Use a hydrogen analyzer to determine the hydrogen content in the molten steel, ensuring H≤2.0ppm. Simultaneously, measure the temperature of the molten steel. When the temperature drops to the ladle temperature range of 1555~1565℃, hoist the ladle to the casting station.

[0059] In this embodiment, the entire VD vacuum treatment process involved argon blowing, with an argon flow rate of 120 NL / min, a pump inlet time of 6 minutes, and a pressure holding time of 66.7 Pa for 25 minutes. The hydrogen content was determined to be 1.5 ppm, the nitrogen content analysis result was 0.005%, and the actual measured temperature of the molten steel was 1555℃.

[0060] (v) Ingot casting

[0061] After the VD pump is deactivated, the steel casting station is notified to prepare for casting. Before casting, argon (Ar) gas is introduced into the ingot mold for gas protection, and the air inside the mold is purged to prevent secondary oxidation of the molten steel during casting. The ladle is hoisted onto the casting car, aligned with the center of the ingot mold, and cast at a rate of 13.5t / ingot. During the casting process, a special MWD-1 type protective slag is used to cover the surface of the molten steel to keep it warm, prevent oxidation, and adsorb inclusions.

[0062] After casting, the steel ingot cools and solidifies naturally in the mold. It can only be lifted and removed from the mold ≥8 hours after casting, and then hot-sent (to the forging or rolling process) or annealed to eliminate the internal stress generated during the cooling process.

[0063] In this embodiment, the argon flow rate is 80 NL / min, the argon charging time is 15 min, and the MWD-1 protective slag is composed of CaO, Al2O3, SiO2, MgO, CaF2, and FeO in a mass ratio of 45:15:3:13:0.5. After casting, it is cooled for 12 hours, lifted and demolded. The steel ingot has good surface quality, without cracks, scale, or other defects, and is then sent to an annealing furnace for annealing treatment.

[0064] The chemical composition analysis results of the G115 steel ingot obtained by the above-mentioned smelting process are as follows: C 0.065%, Si 0.28%, Mn 0.30%, P 0.005%, S 0.004%, Ni 0.05%, Cr 8.50%, Cu 0.50%, W 2.40%, Co 2.85%, N 0.005%, all of which meet the requirements of the G115 steel standard. After subsequent forging and heat treatment, the hardness of the finished steel is tested using existing technical methods to HV195~265. According to the GB / T 10561-2005 Grade A rating method, the sum of the fine series of inclusions is not greater than 5.5, and the sum of the coarse series is not greater than 4.5; the martensite grain size should reach a finer grain size of grade 3 or below, which meets the standard of G115 steel material and can be used as a material for steam main pipelines. Example 3: The present invention provides a new method for smelting G115 using new materials, comprising the following steps: (i) Batching: using G115 steel shavings recycled material as raw material, wherein the G115 steel shavings recycled material is 55t, and the G115 steel shavings recycled material is recycled scrap material generated from machining G115 steel.

[0065] (ii) Electric arc furnace (EAF) smelting:

[0066] The prepared furnace charge is loaded into the charging basket in two batches and then added into the electric furnace. Power is supplied to raise the temperature, and the charge is gradually melted using an electric arc. When the molten steel temperature reaches approximately 1700°C, oxygen is blown into the furnace and carbon powder is injected to remove phosphorus (P) from the molten steel through an oxidation reaction.

[0067] During the smelting process, steel composition is sampled and analyzed periodically. Oxygen blowing is stopped when the carbon (C) content in the molten steel drops to ≤0.04% and the phosphorus (P) content drops to ≤0.003%, meeting the electric furnace endpoint control requirements. Before tapping, the dissolved oxygen activity in the molten steel is measured using a constant oxygen probe, and the oxygen activity is controlled to be <800ppm. The tapping temperature of the electric furnace is 1660–1680℃. Eccentric bottom tapping (EBT) is used during tapping, with slag retention to ensure that most of the oxide slag remains in the electric furnace. Only the primary molten steel (with a small amount of floating slag) is poured into the ladle, which is then transported to the LF refining station by crane.

[0068] In this embodiment, the actual steel composition measured during tapping from the electric furnace was: C 0.04%, P 0.003%, oxygen activity 800ppm, and tapping temperature 1680℃.

[0069] (III) LF Refining

[0070] The ladle is positioned behind the LF refining station. The electrodes are lowered to supply power for heating, and the LF refining operation begins.

[0071] 1. Slag Heating and Formation: Using an electric arc, the slag-forming material pre-added to the ladle is melted, forming a reactive refining slag layer on the surface of the molten steel. Depending on the slag's fluidity and condition, low-carbon lime is added to the slag surface in 1-3 batches, with each batch containing 100-300 kg. After adding lime, heating continues to maintain the slag layer's good fluidity and chemical reactivity. The lime used in this invention has a carbon content of less than 0.2%.

[0072] 2. Slag Surface Deoxidation: Slag surface deoxidation is carried out using ferrosilicon powder (SiFe powder), and the use of carbon powder (C powder) is strictly prohibited. During the deoxidation process, argon gas is continuously introduced into the bottom of the ladle for bottom stirring. The argon gas pressure is adjusted and controlled to prevent the molten steel from overflowing the slag surface, thus preventing the exposed molten steel from absorbing gas. As the deoxidation reaction proceeds, the slag color gradually changes from black to white (i.e., "slag color turning white"), indicating that the refined slag has changed from oxidizing to reducing properties, possessing good desulfurization and inclusion adsorption capabilities.

[0073] 3. Temperature measurement and sampling: After ensuring that all alloys have melted, perform temperature measurement and sampling, analyze the composition of the molten steel, and calculate the amount of each alloy to be added based on the analysis results.

[0074] 4. Alloying: After the slag turns white, add metallic chromium (or ferrochrome with a carbon content below 0.04%), metallic cobalt, copper plates, and ferrotungsten in batches, with each batch consisting of 0.6 to 1.0 tons. The molten steel temperature must be ≥1600℃ when adding each batch of alloys to ensure rapid melting and uniform diffusion, avoiding segregation of alloying elements. The preferred order of addition is: first add metallic chromium or low-carbon ferrochrome, then add metallic cobalt and copper plates, and finally add ferrotungsten. After each batch of alloys is added, adjust the argon stirring intensity appropriately, and add the next batch only after the alloys are fully melted, until the content of each alloying element reaches the target requirements.

[0075] In this embodiment, the slag obtained after electric arc furnace smelting is heated to 1500℃. During the LF refining process, three batches of low-carbon lime are added: 100kg in the first batch, 150kg in the second, and 100kg in the third. 75kg of SiFe powder is used for slag surface deoxidation. When the molten steel temperature reaches 1600℃, alloys are added in three batches: the first batch adds 1 ton of metallic chromium (with 0.6 tons of micro-carbon ferrochrome added simultaneously); the second batch adds 1 ton of metallic cobalt and 0.6 tons of copper plate; and the third batch adds 0.6 tons of ferrotungsten. Each batch ensures the molten steel temperature is ≥1600℃. After alloying, samples are taken and analyzed to ensure the molten steel composition meets all target ranges. The molten steel temperature is adjusted to 1600℃ (meeting the VD inlet temperature requirements), and the ladle is hoisted to the VD vacuum treatment station.

[0076] (iv) VD vacuum treatment

[0077] The ladle is placed into the VD vacuum tank, the tank lid is closed, and the vacuum pump is started to evacuate the molten steel. At the same time, high-purity argon (Ar) gas is continuously blown into the molten steel through the permeable bricks at the bottom of the ladle as a stirring gas. Argon gas is used throughout the entire process from the start of vacuuming until the pump stops (pump withdrawal), and switching to nitrogen gas is strictly prohibited.

[0078] During vacuum pumping, the pump inlet time (the time from starting the vacuum pump to the pressure inside the tank dropping to the working vacuum level) must be ≤8 minutes. Once the vacuum level inside the tank reaches 66.7 Pa, this vacuum level should be maintained for at least 20 minutes. Under these vacuum conditions, gases such as hydrogen (H), nitrogen (N), and oxygen (O) in the molten steel continuously escape from the molten steel under low partial pressure. These gases are carried to the slag surface by argon bubbles and then pumped away by the vacuum pump, achieving deep degassing. Simultaneously, the stirring effect of bottom-blown argon promotes the homogenization of the molten steel's temperature and composition and facilitates the flotation and removal of non-metallic inclusions.

[0079] After the required pressure holding time is reached, stop evacuation and venting (pump withdrawal). Immediately after venting, take samples for analysis to confirm the nitrogen (N) content in the molten steel, ensuring that the nitrogen content of the finished product is within the target range of 0.005~0.010%. Use a hydrogen analyzer to determine the hydrogen content in the molten steel, ensuring H≤2.0ppm. Simultaneously, measure the temperature of the molten steel. When the temperature drops to the ladle temperature range of 1555~1565℃, hoist the ladle to the casting station.

[0080] In this embodiment, the entire VD vacuum treatment process involved argon blowing, with an argon flow rate of 90 NL / min, a pump inlet time of 8 minutes, and a pressure holding time of 66.7 Pa for 20 minutes. The hydrogen content was determined to be 2.0 ppm, the nitrogen content analysis result was 0.010%, and the actual measured temperature of the molten steel was 1565℃.

[0081] (v) Ingot casting

[0082] After the VD pump is deactivated, the steel casting station is notified to prepare for casting. Before casting, argon (Ar) gas is introduced into the ingot mold for gas protection, and the air inside the mold is purged to prevent secondary oxidation of the molten steel during casting. The ladle is hoisted onto the casting car, aligned with the center of the ingot mold, and cast at a rate of 13.5t / ingot. During the casting process, a special MWD-1 type protective slag is used to cover the surface of the molten steel to keep it warm, prevent oxidation, and adsorb inclusions.

[0083] After casting, the steel ingot cools and solidifies naturally in the mold. It can only be lifted and removed from the mold ≥8 hours after casting, and then hot-sent (to the forging or rolling process) or annealed to eliminate the internal stress generated during the cooling process.

[0084] In this embodiment, the argon flow rate is 120 NL / min, the argon charging time is 45 min, and the MWD-1 protective slag is composed of CaO, Al2O3, SiO2, MgO, CaF2, and FeO in a mass ratio of 55:25:13:23:1.5. After casting, it is cooled for 8 hours, lifted and demolded. The steel ingot has good surface quality, without cracks, scale, or other defects, and is then sent to an annealing furnace for annealing treatment.

[0085] The chemical composition analysis results of the G115 steel ingot obtained by the above-mentioned smelting process are as follows: C 0.095%, Si 0.5%, Mn 0.70%, P 0.015%, S 0.006%, Ni 0.10%, Cr 9.50%, Cu 1.10%, W 3.10%, Co 3.20%, N 0.010%. After subsequent forging and heat treatment, the hardness of the finished steel is tested using existing technical methods, and the hardness is HBW 195~250. According to the GB / T 10561-2005 Grade A rating method, the total fine inclusions are no greater than grade 5.5, and the total coarse inclusions are no greater than grade 4.5. The average austenite grain size reaches grade 0, which meets the standard of G115 steel material and can be used as a material for steam main pipelines.

[0086] The following is a comparison between the methods of smelting G115 steel according to the present invention and the prior art, in order to illustrate the beneficial effects obtained by the present invention.

[0087] Process Comparison Dimensions Existing technology This invention Beneficial effects achieved Ingredients Source of raw materials Steel is produced using a large amount of raw pig iron, purchased high-nickel scrap steel, and various alloy materials. Using G115 steel shavings as raw material Replacing virgin materials of the same steel grade with recycled materials of the same grade reduces costs from the source and avoids the problem of difficult control of residual elements such as Ni. EAF furnace smelting Endpoint control Endpoint control parameters not specified Oxygen blowing and carbon injection at 1200-1700℃, with a clear endpoint of C≤0.04% and P≤0.003%, tapping temperature 1660~1680℃, and oxygen activity <800ppm. Quantifying endpoint indicators and temperature control ranges reduces the burden on LF furnace refining. LF furnace refining Deoxidation treatment Deoxidation using toner SiFe powder To prevent carbon buildup, precisely control the lower limit of carbon content in the finished product. VD vacuum treatment Vacuum control Without using argon, there is a lack of clear quantitative indicators for time-vacuum matching. Pump inlet time ≤ 8 min; 66.7 Pa holding time ≥ 20 min; hydrogen concentration H ≤ 2.0 ppm; jug temperature 1555~1565℃ Quantify pumping speed, holding time, and ladle temperature to accurately remove hydrogen and nitrogen while ensuring the pouring temperature window. Ingot casting Antioxidation / Defect Prevention If anti-splashing measures are not taken for the ingot casting, the protective slag performance is poor, or the mold is not clean, it is easy to produce surface / subcutaneous inclusions, bubbles, and heavy scale on the ingot surface. Argon purging in the mold (80-120 NL / min, 15-45 min); special MWD-1 protective slag (with clearly defined composition); heat preservation for ≥8 hours after casting, followed by hot delivery / annealing. The entire process combines physical and chemical protection, significantly reducing surface and internal defects in the ingot.

[0088] In summary, this invention achieves a complete G115 steel smelting technology solution that is low-cost, easy to operate, high-precision, high-purity, and high-yield by closely linking the processes of deep dephosphorization in EAF furnace, precise alloying in LF refining, forced dehydrogenation in VD vacuum, and full protection in die casting. Each step is a prerequisite for and a guarantee for the others, giving full play to the synergistic effect. This solution has important practical application value for promoting the stable industrial production of G115 steel.

[0089] It should be noted that the above-described technical content of this invention is merely an explanation and clarification to enable those skilled in the art to understand the technical essence of this invention, and therefore is not intended to limit the scope of protection of this invention. The scope of protection of this invention should be determined by the claims. Those skilled in the art should understand that any modifications, equivalent substitutions, and improvements made based on the essential spirit of this invention should be within the scope of protection of this invention.

Claims

1. A novel method for smelting G115 using new materials, characterized in that, The process includes the following steps: Ingredient preparation: using G115 steel shavings recycled material as raw material, wherein the G115 steel shavings recycled material is 50-60t, and the G115 steel shavings recycled material is the recycled scrap material generated from the machining of G115 steel.

2. The method according to claim 1, characterized in that, The method also includes: EAF furnace smelting: the prepared furnace charge is heated to melt, oxygen and carbon are blown and injected at 1200-1700℃ for deep dephosphorization, the C at the end point of the electric furnace is controlled to be ≤0.04% and P ≤0.003%, the tapping temperature is controlled to be 1660~1680℃, and the oxygen activity before tapping is <800ppm.

3. The method according to claim 1, characterized in that, The method further includes: LF refining: heating the slag obtained after electric furnace smelting to 1400-1700℃, adding 100-300kg / batch of lime with a carbon content of less than 0.2% in 1-3 batches, using 75kg-85kg of SiFe powder for slag surface deoxidation, controlling the argon pressure to ensure that the molten steel does not overflow the slag surface, ensuring that the alloy is fully melted and the slag color turns white, adding 0.6-1.0 tons of metallic Cr or ferrochrome, metallic Co, copper plates and ferrotungsten with a carbon content of less than 0.04% in 1-3 batches, with the temperature ≥1600℃ when adding the metals in batches.

4. The method according to claim 1, characterized in that, The method also includes: VD vacuum treatment: During VD vacuum treatment, the tank is evacuated, and argon gas is continuously blown into the molten steel as a stirring gas. The entire VD vacuum treatment is argon blowing operation, and the argon gas flow rate is 120-170 NL / min.

5. The method according to claim 4, characterized in that, The method further includes: during VD vacuum treatment, the pump inlet time is ≤8min; the holding time at 66.7Pa is ≥20min; the hydrogen concentration is ≤2.0ppm; and the ladle temperature is 1555~1565℃.

6. The method according to claim 1, characterized in that, The method also includes in-mold casting: argon is filled into the mold at a flow rate of 80-120 NL / min for 15-45 min. MWD-1 protective slag is used, which is composed of CaO, Al2O3, SiO2, MgO, CaF2, and FeO in a mass ratio of 45-55:15-25:3-13:13-23:0.5-1.

5. After casting, the mold is lifted and hot-sent or annealed after ≥8 hours.

7. A G115 steel material, characterized in that, The composition is: C 0.065-0.095%, Si≤0.5%, Mn 0.30-0.70%, P≤0.015%, S≤0.006%, Ni≤0.10%, Cr 8.50-9.50%, Cu 0.50-1.10%, W 2.40-3.10%, Co 2.85-3.20%, N 0.005-0.010%, prepared by the method described in any one of claims 1-6.

8. The application of G115 steel material obtained by the new material smelting method as described in any one of claims 1 to 6 in the main steam pipeline.